A method for preparing layered oxide positive electrode material for sodium ion battery

By weighing the reaction molten salt precursor and the metal salt in a stoichiometric ratio, high-temperature heat treatment to generate molten salt and metal oxide, and mixing it with the sodium source to form a layered oxide positive electrode material, the high raw material cost in the prior art is solved and The complex process problem has achieved improved material performance and reduced cost.

CN118684282BActive Publication Date: 2024-11-26SICHUAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411156182.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-26
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

In the existing synthesis methods of sodium ion battery positive electrode materials, the solid phase method has high cost and poor material performance, the co-precipitation method has high purity requirements and complex process, and the additional molten salt method adds molten salt to increase cost and affects the material structure.

Method used

The reaction molten salt precursor and metal salt are weighed in stoichiometric ratio, and the high-temperature heat treatment is used to generate molten salt and metal oxide, and then mixed with sodium source and then heat treatment is carried out to form a layered oxide positive electrode material, using cheap raw materials and simplifying the process to avoid The effect of the salt washing step on the structure.

Benefits of technology

It realizes controllable material particle size, uniform element distribution, good cycle stability and rate performance, reduces raw material cost and process complexity, and is suitable for raw materials that are deteriorated or impurities-containing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118684282B_ABST
    Figure CN118684282B_ABST
Patent Text Reader

Abstract

The invention provides a method for preparing a sodium ion battery layered oxide positive electrode material, which relates to the field of sodium ion battery positive electrode materials, and specifically comprises the following steps: step 1: after component detection, a reaction molten salt precursor and a metal salt are weighed according to a stoichiometric ratio; step 2: after the above salts are mixed, a molten salt is generated by reaction during a high-temperature heat treatment process; step 3: after the heat treatment, the sample is washed and dried to obtain a metal oxide; step 4: the metal oxide is mixed with a sodium source, and the mixture is heat-treated to obtain a layered oxide positive electrode material; the chemical composition of the metal oxide is Na x MO y , where #imgabs0#; the chemical composition of the layered oxide cathode material is Na x MO 2 The material synthesized by the present invention has controllable particle size, uniform element distribution, high capacity, energy density, good cycle stability and rate performance, simple synthesis method, and can use deteriorated or impurity-containing raw materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of sodium ion battery positive electrode materials, and in particular to a method for preparing a sodium ion battery layered oxide positive electrode material. Background Art

[0002] Sodium ion battery is a clean, efficient and renewable secondary ion battery. The abundant sodium resources in the earth's crust make it a cheap energy storage device to solve today's energy crisis and environmental pollution. The positive electrode material is one of the most important components of sodium ion batteries, which determines the stability and charge and discharge performance of the battery. Layered oxide is the most common material in the positive electrode material of sodium ion batteries. Compared with polyanion and Prussian blue materials, its synthesis cost and industrialization difficulty are lower.

[0003] At present, the more mature synthesis methods for layered positive electrode materials are solid phase method and coprecipitation method. The solid phase method has a simple synthesis process, which is usually made by mixing metal oxides and sodium salts evenly and then subjecting them to high temperature heat treatment. The metal oxides used in the solid phase method usually come from metal sulfates or other metal salts, so its raw material cost is relatively high. In addition, since metal oxides generally have a high hardness, it is difficult to grind them evenly using the general mixing method, resulting in large differences in the size and shape of the obtained material particles, and there will also be uneven distribution of elements. Therefore, the advantages of the solid phase method are simple process and good batch quality, and the disadvantages are high raw material costs and poor product electrochemical performance.

[0004] The coprecipitation method usually dissolves metal sulfate in water, adds sodium hydroxide and ammonia complexing agent for precipitation in a warm water bath and under the protection of an inert atmosphere, obtains metal hydroxide after aging, filtering, washing, drying and other processes, and mixes the metal hydroxide and sodium salt evenly and then heat treats at high temperature. The raw materials of the coprecipitation method are cheap, and the synthesized materials generally have uniform particles, uniform element distribution, and good electrochemical properties. However, due to the complex influencing factors of the coprecipitation reaction, the raw materials for coprecipitation have high purity requirements. If the raw materials are oxidized or contain other ionic impurities, it will directly affect the coprecipitation process and cause the material performance to decline.

[0005] The molten salt method is a new method for synthesizing sodium-ion layered oxides. The Institute of Chemistry of the Chinese Academy of Sciences disclosed a sodium-based layered oxide single crystal particle with exposed active crystal faces and its preparation method and application (CN117497744A), Tianjin University of Technology disclosed a small-sized single crystal layered sodium-ion positive electrode material and its preparation method and application (CN116666621A), Sun Yat-sen University disclosed a doped nickel-manganese-based sodium-ion battery single crystal positive electrode material and its application (CN118099411A), Zhejiang DeChuang Sodium Electric New Energy Co., Ltd. disclosed a high-performance sodium-ion battery positive electrode material and its preparation method (CN116470039A).

[0006] The common point of the above methods is that metal oxide or metal hydroxide is mixed with sodium source and molten salt and then calcined to obtain a layered oxide and molten salt mixture, and the mixture is washed, dried and calcined again to obtain a layered oxide material. The material synthesized by the molten salt method has uniform particle size and element distribution and generally has stable electrochemical properties, but the additional addition of molten salt will increase the cost, and the salt washing step will also have an irreversible effect on the structure of the layered oxide, resulting in capacity loss. Summary of the invention

[0007] The object of the present invention is to provide a method for preparing a layered oxide positive electrode material for a sodium ion battery. The material synthesized by the present invention has controllable particle size, uniform element distribution, high capacity, energy density, good cycle stability and rate performance, a simple synthesis method, and can use deteriorated or impurity-containing raw materials.

[0008] In order to solve the above technical problems, the technical solution adopted by the present invention is:

[0009] A method for preparing a layered oxide positive electrode material for a sodium ion battery comprises the following steps:

[0010] Step 1: After component testing, the reaction molten salt precursor and the metal salt are weighed according to the stoichiometric ratio;

[0011] Step 2: After mixing the above salts, react during high temperature heat treatment to generate molten salt;

[0012] Step 3: After the heat treatment, the sample is washed and dried to obtain the metal oxide;

[0013] Step 4: mixing the metal oxide with the sodium source, and heat treating the mixture to obtain a layered oxide positive electrode material;

[0014] Among them, the chemical composition of metal oxides is Na x MO y ,in ;

[0015] The chemical composition of the layered oxide cathode material is Na x MO 2 ,in , M is one or more of magnesium, aluminum, calcium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, copper, zinc, zirconium, and tin, and the phase composition is an O3 structure or a P2 structure or a mixed structure of O3 and P2.

[0016] The reaction molten salt precursor includes one or more of carbonates, nitrates, oxalates, sulfates, chlorides and hydroxides of lithium, sodium and potassium.

[0017] Furthermore, the metal salt includes one or more of sulfates and chlorides of magnesium, aluminum, calcium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, copper, zinc, zirconium and tin.

[0018] Preferably, the metal salt is derived from a chemical reagent of chemical purity, analytical purity or higher purity, or from a salt deteriorated by oxidation and moisture absorption, or from an industrial salt containing one or more of the above ions as impurities, or from ferrous sulfate, a by-product of titanium dioxide production.

[0019] Furthermore, the material mixing method is grinding mixing, ball milling mixing or sand milling mixing.

[0020] The heat treatment conditions are as follows: in a dry air or oxygen atmosphere, the heating rate is To 400 ℃ -1000 ℃, keep warm for 2-24 hours, and cool naturally after sintering.

[0021] Furthermore, the sodium source comes from one or more of sodium carbonate, sodium hydroxide, sodium nitrate, and sodium oxalate.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The addition of the reaction molten salt precursor of the present invention, on the one hand, converts metal sulfates or chlorides with good thermal stability into other easily decomposable salts, which are easy to generate metal oxides during the heat treatment process; on the other hand, the cations of the reaction molten salt precursor react with the anions of the metal salt to generate a molten salt which simultaneously plays a role in regulating the morphology and element uniformity during the heat treatment process.

[0024] Compared with the solid phase method, the raw material source of this method is relatively cheap, the particle size of the synthesized material is adjustable, and the element distribution is uniform; compared with the coprecipitation method, the process of this method is simple, and raw materials that have been deteriorated or contain other ionic impurities can be used; compared with the traditional molten salt method, since the first heat treatment product of this method is a mixture of molten salt and metal oxides, salt washing will not affect the structure of the material. The traditional molten salt method uses metal oxides or hydroxides as raw materials, and this method directly uses cheaper raw materials to react to generate molten salt, which is lower in cost and simpler in process. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0026] Figure 1 The present invention is a flow chart of the preparation method.

[0027] Figure 2 This is a SEM image of the nickel-iron-manganese oxide obtained by the first sintering in Example 1.

[0028] Figure 3 The second sintering in Example 1 SEM image of the positive electrode material.

[0029] Figure 4 The nickel-iron-manganese oxide in Example 1 and XRD spectrum of the positive electrode material.

[0030] Figure 5 In Example 1 Charge and discharge curves of positive electrode materials at different rates.

[0031] Figure 6 In Example 1 The positive electrode material The cyclic stability curve.

[0032] Figure 7 This is a SEM image of the nickel-iron-manganese oxide obtained by the first sintering in Example 2.

[0033] Figure 8 The second sintering in Example 2 SEM image of the positive electrode material.

[0034] Fig. 9 The nickel-iron-manganese oxide and XRD spectrum of the positive electrode material.

[0035] Fig.10 In Example 2 Charge and discharge curves of positive electrode materials at different rates.

[0036] Fig.11 In Example 2 The positive electrode material The cyclic stability curve.

[0037] Fig.12 This is a SEM image of the metal oxide obtained by the first sintering in Example 3.

[0038] Fig.13 This is a SEM image of the layered positive electrode material obtained by the second sintering in Example 3.

[0039] Fig.14 It is the XRD spectrum of the metal oxide and layered positive electrode material in Example 3.

[0040] Fig.15 3 is the charge and discharge curve of the positive electrode material at different rates.

[0041] Fig.16 The positive electrode material in Example 3 is The cyclic stability curve.

[0042] Fig.17 The O3 structure is obtained by the second sintering in Example 4. SEM image of the positive electrode material.

[0043] Fig.18 In Example 4 XRD spectrum of .

[0044] Fig.19 4 is the charge and discharge curve of the positive electrode material at different rates.

[0045] Fig. 20 In Example 4 The positive electrode material The cyclic stability curve.

[0046] Fig.21 This is the SEM image of the positive electrode material sintered for the second time in Example 5.

[0047] Fig. 22 This is the XRD spectrum of the positive electrode material in Example 5.

[0048] Fig.23 1 is the charge and discharge curve of the positive electrode material in Example 5 at different rates.

[0049] Fig.24 The positive electrode material in Example 5 is The cyclic stability curve.

[0050] Fig.25 The P2 structure is obtained by the second sintering in Example 6. SEM image of the positive electrode material.

[0051] Fig.26 In Example 6 XRD spectrum of .

[0052] Fig. 27 In Example 6 Charge and discharge curves of positive electrode materials at different rates.

[0053] Fig.28 In Example 6 Cycling stability curve of the cathode material at 1C.

[0054] Fig.29 This is a SEM image of the layered positive electrode material obtained by the second sintering in Example 7.

[0055] Fig.30 This is the XRD spectrum of the layered positive electrode material in Example 7.

[0056] Fig.31 1 is the charge and discharge curve of the positive electrode material in Example 7 at different rates.

[0057] Fig.32 This is the cycle stability curve of the positive electrode material in Example 7 at 1C.

[0058] Fig.33 The O3 / P2 mixed structure obtained by the second sintering in Example 8 SEM image of the positive electrode material.

[0059] Fig.34 In Example 8 XRD spectrum of .

[0060] Fig.35 This is a SEM image of the metal oxide obtained by the first heat treatment in Example 9.

[0061] Fig.36 This is the XRD spectrum of the metal oxide obtained by the first heat treatment in Example 9.

[0062] Fig.37 This is a SEM image of the metal oxide obtained by the first sintering in Example 10.

[0063] Fig.38 This is the XRD spectrum of the metal oxide obtained by the first sintering in Example 10.

[0064] Fig.39 This is a SEM image of the metal oxide obtained by the first sintering in Example 11.

[0065] Fig.40 This is the XRD spectrum of the metal oxide obtained by the first sintering in Example 11.

[0066] Fig.41 In comparative example 1 SEM image of the positive electrode material.

[0067] Fig.42 In comparative example 1 XRD patterns of positive electrode materials.

[0068] Fig.43 In comparative example 1 Charge and discharge curves of positive electrode materials at different rates.

[0069] Fig.44 In comparative example 1 Cycling stability curve of the cathode material at 1C.

[0070] Fig.45 In comparative example 2 SEM image of the positive electrode material.

[0071] Fig.46 In comparative example 2 XRD patterns of positive electrode materials.

[0072] Fig.47 In comparative example 2 Charge and discharge curves of positive electrode materials at different rates.

[0073] Fig.48 In comparative example 2 Cycling stability curve of the cathode material at 1C.

[0074] Fig.49 In comparative example 3 SEM image of the positive electrode material.

[0075] Fig.50 In comparative example 3 XRD patterns of positive electrode materials.

[0076] Fig.51 In comparative example 3 Charge and discharge curves of positive electrode materials at different rates.

[0077] Fig.52 In comparative example 3 Cycling stability curve of the cathode material at 1C. DETAILED DESCRIPTION

[0078] In the following, only some exemplary embodiments are briefly described. As those skilled in the art will appreciate, the described embodiments may be modified in various ways without departing from the spirit or scope of the embodiments of the present invention. Therefore, the drawings and descriptions are considered to be exemplary and non-restrictive in nature. Embodiments of the present invention are described in detail below in conjunction with the accompanying drawings.

[0079] Example 1

[0080] See also Figure 1 This embodiment discloses a method for preparing a layered oxide positive electrode material for a sodium ion battery, which specifically comprises the following steps:

[0081] Step 1: After component testing, the reaction molten salt precursor and the metal salt are weighed according to the stoichiometric ratio;

[0082] Step 2: After the above salts are mixed, they react during high temperature heat treatment to generate a mixture of molten salt and metal oxide;

[0083] Step 3: After the heat treatment, the sample is washed and dried to obtain the metal oxide;

[0084] Step 4: mixing the metal oxide with the sodium source, and heat treating the mixture to obtain a layered oxide positive electrode material;

[0085] The specific preparation case is as follows:

[0086] 60 mmol of sodium carbonate, 20 mmol of nickel sulfate hexahydrate, 20 mmol of ferrous sulfate heptahydrate, and 20 mmol of manganese sulfate monohydrate were weighed and placed in a ball mill. The mixture was ball milled at 400 rpm for 30 min in a planetary ball mill. The ball milled product was placed in a corundum boat and heated to 900°C at a rate of 5°C / min. The mixture was kept warm for 2 h and then naturally cooled to room temperature.

[0087] The sample was washed with water and then dried to obtain nickel-iron-manganese oxide. The oxide and sodium carbonate were placed in a ball mill according to the stoichiometric ratio and ball milled in a planetary ball mill at 400 rpm for 30 min. The ball milled product was placed in a corundum boat and heated at a rate of 5°C / min to 900°C. After keeping the temperature for 15 h, it was naturally cooled to room temperature to obtain an O3 structured Positive electrode material.

[0088] In this embodiment, the reaction molten salt precursor and the metal sulfate undergo the following reaction during mixing and heat treatment:

[0089]

[0090] The reaction process generates sodium sulfate molten salt, which plays a role in morphology regulation during the decomposition of metal carbonates.

[0091] Figure 2 This is a SEM image of the nickel-iron-manganese oxide obtained by the first sintering in Example 1.

[0092] Figure 3 The second sintering in Example 1 SEM image of the positive electrode material.

[0093] Figure 4 The nickel-iron-manganese oxide in Example 1 and XRD spectrum of the positive electrode material.

[0094] Figure 5 In Example 1 Charge and discharge curves of positive electrode materials at different rates.

[0095] Figure 6 In Example 1 The positive electrode material The cyclic stability curve.

[0096] See also Figure 2-Figure 6 The first sintering yields nickel-iron-manganese oxide with uniform particle size distribution and spinel structure. The second sintering yields The positive electrode material has regular particles and belongs to the O3 layered structure. The positive electrode material has good rate performance and cycle stability, which proves the feasibility of this method for preparing O3 layered positive electrode materials.

[0097] Example 2

[0098] Compared with Example 1, the only difference is that analytically pure ferrous sulfate heptahydrate is replaced with deteriorated analytically pure ferrous sulfate heptahydrate. Therefore, the steps after weighing are the same as those in Example 1. It is only necessary to determine the relative content of iron in the deteriorated reagent before weighing. The specific steps are as follows:

[0099] Weigh 20 g of metamorphic ferrous sulfate heptahydrate, place it in a corundum boat, raise the temperature to 900°C at a rate of 5°C / min, keep it for 2 hours, then naturally cool it to room temperature, weigh the mass of the product iron oxide to determine the iron content in the metamorphic ferrous sulfate heptahydrate.

[0100] Figure 7 This is a SEM image of the nickel-iron-manganese oxide obtained by the first sintering in Example 2;

[0101] Figure 8 The second sintering in Example 2 SEM images of cathode materials;

[0102] Fig. 9The nickel-iron-manganese oxide and XRD spectrum of positive electrode material;

[0103] Fig.10 In Example 2 The charge and discharge curves of the cathode material at different rates;

[0104] Fig.11 In Example 2 The positive electrode material The cyclic stability curve.

[0105] See also Figure 7-Figure 11 The first sintering yields nickel-iron-manganese oxide with uniform particle size distribution and spinel structure. The second sintering yields The positive electrode material particles are regular and belong to the O3 layered structure. The positive electrode material has good rate performance and cycle stability. The morphology and electrochemical performance of the positive electrode material are basically the same as those of Example 1, proving that this method can use deteriorated raw materials to synthesize O3 layered materials with excellent performance.

[0106] Example 3

[0107] Compared with Example 1, the only difference is that analytically pure ferrous sulfate heptahydrate is replaced by ferrous sulfate, a byproduct produced by titanium dioxide. This raw material not only contains impurity ions but also deteriorates. Therefore, the steps after weighing are the same as those in Example 1. It is only necessary to determine the relative content of various metal ions in the byproduct ferrous sulfate before weighing. The specific steps are as follows:

[0108] Weigh 100 mg of ferrous sulfate, a byproduct of titanium dioxide, and digest it in nitric acid. After diluting the digestion solution to a certain ratio, measure ICP to obtain the relative content of various metal ions.

[0109] Table 1 shows the relative molar content of ferrous sulfate metal ions as a byproduct of a batch of titanium dioxide:

[0110]

[0111] Only the analytically pure ferrous sulfate heptahydrate in Example 1 was replaced with an equal molar amount of ferrous sulfate produced as a byproduct of titanium dioxide.

[0112] Fig.12 This is a SEM image of the metal oxide obtained by the first sintering in Example 3.

[0113] Fig.13 This is a SEM image of the layered positive electrode material obtained by the second sintering in Example 3.

[0114] Fig.14 It is the XRD spectrum of the metal oxide and layered positive electrode material in Example 3.

[0115] Fig.15 3 is the charge and discharge curve of the positive electrode material at different rates.

[0116] Fig.16 The positive electrode material in Example 3 is The cyclic stability curve.

[0117] See also Figure 12-16 The first sintering yields a uniform particle size distribution of metal oxides, belonging to the spinel structure, and the second sintering yields regular particles of the positive electrode material, belonging to the O3 layered structure. The positive electrode material has good rate performance and cycle stability, and the morphology and electrochemical properties of the positive electrode material are basically the same as those of Example 1, proving that this method can use industrial raw materials rich in impurities to synthesize O3 layered materials with excellent performance.

[0118] See also Figure 2-16 , Combining Example 1, Example 2 and Example 3, it can be seen that changing the purity of the raw materials has little effect on the morphology, phase composition and electrochemical properties of the samples.

[0119] Example 4

[0120] Compared with Example 1, the only difference is that the formula is replaced with 60 mmol sodium carbonate, 13.2 mmol copper sulfate pentahydrate, 18 mmol ferrous sulfate heptahydrate, and 28.8 mmol manganese sulfate monohydrate.

[0121] Fig.17 The O3 structure is obtained by the second sintering in Example 4. SEM image of the positive electrode material. Fig.18 In Example 4 XRD spectrum of . Fig.19 4 is the charge and discharge curve of the positive electrode material at different rates. Fig. 20 In Example 4 The positive electrode material The cyclic stability curve.

[0122] See also Figure 17-Figure 20 , the second sintering yields The positive electrode material has regular particles and belongs to the O3 layered structure. The positive electrode material has good rate performance and cycle stability, proving that this method can also be used to prepare The feasibility of O3 layered cathode materials.

[0123] Example 5

[0124] Compared with Example 4, the only difference is that analytically pure ferrous sulfate heptahydrate is replaced by ferrous sulfate, a by-product produced by titanium dioxide.

[0125] Fig.21 This is the SEM image of the positive electrode material sintered for the second time in Example 5. Fig. 22 This is the XRD spectrum of the positive electrode material in Example 5. Fig.23 1 is the charge and discharge curve of the positive electrode material in Example 5 at different rates. Fig.24 The positive electrode material in Example 5 is The cyclic stability curve.

[0126] See also Figure 21-24 The second sintering results in regular particles of positive electrode material, which belongs to the O3 layered structure. The positive electrode material has good rate performance and cycle stability. The morphology and electrochemical performance of the positive electrode material are basically the same as those of Example 4, proving that the method can use industrial raw materials rich in impurities to synthesize chemical composition O3 layered materials.

[0127] It can be shown in combination with Examples 1-5 that the method is applicable to a variety of O3 type sodium positive electrode materials, and the use of deteriorated or impure raw materials will not have a significant impact on the morphology, structure and electrochemical properties of the O3 type materials.

[0128] Example 6

[0129] Compared with Example 1, the only difference is that the formula is replaced with 60 mmol sodium carbonate, 18 mmol ferrous sulfate heptahydrate, 30 mmol manganese sulfate monohydrate, 6 mmol magnesium sulfate, and 6 mmol titanyl sulfate, and the second sintering temperature is changed to 950°C.

[0130] Fig.25 The P2 structure is obtained by the second sintering in Example 6. SEM image of the positive electrode material. Fig.26 In Example 6 XRD spectrum of . Fig. 27 In Example 6 Charge and discharge curves of positive electrode materials at different rates. Fig.28 In Example 6 Cycling stability curve of the cathode material at 1C.

[0131] See also Figure 25-28 , the second sintering yields The positive electrode material has regular particles and belongs to the P2 layered structure. The positive electrode material has good rate performance and cycle stability, proving that this method can also be used to synthesize P2 type sodium layered positive electrode materials.

[0132] Example 7

[0133] Compared with Example 6, the only difference is that analytically pure ferrous sulfate heptahydrate is replaced by ferrous sulfate, a by-product produced by titanium dioxide.

[0134] Fig.29 This is a SEM picture of the layered positive electrode material obtained by the second sintering in Example 7. Fig.30 This is the XRD spectrum of the layered positive electrode material in Example 7. Fig.31 1 is the charge and discharge curve of the positive electrode material in Example 7 at different rates. Fig.32 This is the cycle stability curve of the positive electrode material in Example 7 at 1C.

[0135] See also Figure 29-Figure 32 The second sintering results in regular positive electrode material particles, belonging to the P2 layered structure. The positive electrode material has good rate performance and cycle stability. The morphology and electrochemical performance of the positive electrode material are basically the same as those of Example 6. The use of deteriorated or impure raw materials will not have a significant impact on the morphology, structure and electrochemical performance of the P2 type material. This proves that the method can use industrial raw materials rich in impurities to synthesize chemical compositions. P2 layered material.

[0136] Example 8

[0137] Compared with Example 1, the only difference is that the formula is replaced with 60 mmol sodium carbonate, 6 mmol copper sulfate pentahydrate, 6 mmol cobalt sulfate heptahydrate, 15 mmol nickel sulfate hexahydrate, 24 mmol manganese sulfate monohydrate, and 9 mmol titanyl sulfate.

[0138] Fig.33 The O3 / P2 mixed structure obtained by the second sintering in Example 8 SEM image of the positive electrode material. Fig.34 In Example 8 XRD spectrum of .

[0139] See also Figure 33-Figure 34 The second sintering results in regular cathode material particles, with O3 and P2 structures appearing simultaneously in XRD, and the ratio of O3 to P2 phases is calculated to be 6:4. This example proves that the method can also be used to synthesize O3 / P2 type mixed sodium layered cathode materials.

[0140] Example 9

[0141] Compared with Example 1, the only difference is that no sodium carbonate is added. When no sodium carbonate is added, the following reaction occurs during the first heat treatment process:

[0142]

[0143] During the reaction, sulfate decomposes into metal oxides and and Gas, the emission of gas will cause environmental pollution.

[0144] Fig.35 This is a SEM image of the metal oxide obtained by the first heat treatment in Example 9. Fig.36 This is the XRD spectrum of the metal oxide obtained by the first heat treatment in Example 9.

[0145] See also Figure 35-Figure 36 , it can be seen that the absence of molten salt will make the morphology distribution of metal oxides more uneven, but the metal oxides still have a spinel structure.

[0146] Example 10

[0147] Compared with Example 1, the only difference is that the amount of sodium carbonate is increased to 75 mmol. The added sodium carbonate is used as a sodium source, which decomposes in the molten salt reaction to generate sodium oxide and reacts with the metal oxide to generate a layered metal oxide. The generation of the layered metal oxide can control the morphology of the material obtained by the first sintering, thereby controlling the morphology of the layered positive electrode obtained subsequently.

[0148] Fig.37 This is a SEM picture of the metal oxide obtained by the first sintering in Example 10. Fig.38 This is the XRD spectrum of the metal oxide obtained by the first sintering in Example 10.

[0149] See also Figure 37-Figure 38 , it can be seen that flaky grains appear after adding excess sodium carbonate, and the XRD spectrum shows that part of the spinel phase transforms into a layered structure.

[0150] Embodiment 11

[0151] Compared with Example 1, the only difference is that the amount of sodium carbonate is increased to 90 mmol. Fig.39 This is a SEM picture of the metal oxide obtained by the first sintering in Example 11. Fig.40 This is the XRD spectrum of the metal oxide obtained by the first sintering in Example 11.

[0152] See also Figure 39-40 It can be seen that more lamellar grains appear as sodium carbonate is added, and the XRD spectrum shows that the layered structure component accounts for the main component.

[0153] In combination with Example 10, it can be seen that the more sodium source is added in the molten salt reaction process, the more flaky grains there are and they tend to become larger, and the proportion of layered structures will also increase. In combination with Examples 9, 10, and 11, it can be seen that molten salt can play a role in morphology regulation, and adding a sodium source in the molten salt reaction can regulate the morphology.

[0154] Comparative Example 1

[0155] In this case, NaNi was synthesized by solid phase method.1 / 3 Fe 1 / 3 Mn 1 / 3 O 2 Positive electrode material. 30mmol sodium carbonate, 20mmol nickel oxide, 10mmol ferric oxide, and 10mmol manganese oxide were weighed and placed in a ball mill. The ball mill was milled at 400rpm for 2h in a planetary ball mill. The ball milled product was placed in a corundum boat and heated to 900℃ at a rate of 5℃ / min. After keeping the temperature for 15h, it was naturally cooled to room temperature to obtain NaNi with O3 structure. 1 / 3 Fe 1 / 3 Mn 1 / 3 O 2 Positive electrode material.

[0156] Fig.41 In comparative example 1 SEM image of the positive electrode material. Fig.42 In comparative example 1 XRD patterns of positive electrode materials. Fig.43 In comparative example 1 Charge and discharge curves of positive electrode materials at different rates. Fig.44 In comparative example 1 Cycling stability curve of cathode material at 1C.

[0157] See also Figure 41-44 , synthesized by solid phase method The positive electrode material particles are not uniform and belong to the O3 layered structure. The rate performance and cycle stability of the positive electrode material are poor. This comparative example successfully synthesized the Positive electrode material, but because the solid phase method is difficult to control the product shape and uniform element distribution, the electrochemical performance is poor.

[0158] Comparative Example 2

[0159] In this case, the coprecipitation method was used to synthesize Positive electrode material. Prepare 2M solution of nickel sulfate hexahydrate, ferrous sulfate heptahydrate and manganese sulfate monohydrate in equal stoichiometric amounts, and prepare ammonia water and sodium hydroxide solution with solubility of 3M and 7M respectively. In the coprecipitation reactor, the water bath temperature is controlled at 55°C. Under nitrogen protective gas and a rotation speed of 600rpm of polytetrafluoroethylene blades, the two solutions are pumped into the sulfate solution, and the pH of the solution is controlled to 11. After the reaction, the reactants are aged for 4 hours, filtered, washed with water, and dried to obtain metal hydroxide. The hydroxide and sodium carbonate are placed in a ball mill according to the stoichiometric ratio, and ball milled in a planetary ball mill at a speed of 400rpm for 30 minutes. The ball milled product is placed in a corundum boat and heated to 900°C at a rate of 5°C / min. After keeping warm for 15 hours, it is naturally cooled to room temperature to obtain an O3 structure. Positive electrode material.

[0160] Fig.45 In comparative example 2 SEM image of the positive electrode material. Fig.46 In comparative example 2 XRD patterns of positive electrode materials. Fig.47 In comparative example 2 Charge and discharge curves of positive electrode materials at different rates. Fig.48 In comparative example 2 Cycling stability curve of the cathode material at 1C.

[0161] See also Figure 45-Figure 48 , synthesized by coprecipitation method The positive electrode material particles are uniform and belong to the O3 layered structure. The positive electrode material has good rate performance and cycle stability. This comparative example successfully synthesized the Positive electrode material, but the liquid phase process is complicated.

[0162] Comparative Example 3

[0163] In this case, the coprecipitation method was used to synthesize Positive electrode material: The only difference from Comparative Example 2 is that analytically pure ferrous sulfate heptahydrate is replaced with ferrous sulfate, a byproduct of titanium dioxide.

[0164] Fig.49 In comparative example 3 SEM image of the positive electrode material. Fig.50 In comparative example 3 XRD patterns of positive electrode materials. Fig.51 In comparative example 3 Charge and discharge curves of positive electrode materials at different rates. Fig.52 In comparative example 3 Cycling stability curve of the cathode material at 1C.

[0165] See also Figure 49-Figure 52 , synthesized by coprecipitation of raw materials containing impurities The positive electrode material particles agglomerate and belong to the O3 layered structure. The rate performance and cycle stability of the positive electrode material are significantly reduced compared with the comparative example 2. This comparative example successfully synthesized the coprecipitation method of the impurity-containing raw material. Positive electrode material, but the liquid phase method has high requirements on the purity of raw materials, and the electrochemical performance will decrease.

[0166] Table 2 is a comparison of the electrochemical performance of Example 1, Example 2, Example 3 and Comparative Example 1, Comparative Example 2, Comparative Example 3 at 1C.

[0167]

[0168] As can be seen from Table 2, this method has higher capacity and better capacity retention rate than the solid phase method of Comparative Example 1. The capacity retention rate of this method is higher than that of the coprecipitation method of Comparative Example 2. By comparing Example 3 and Comparative Example 3, it can be seen that the raw materials containing impurities or that have deteriorated have little effect on the electrochemical performance of this method, but have a greater impact on the coprecipitation method. This is because the deteriorated raw materials affect the coprecipitation process, but will not cause a significant impact on this method.

[0169] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0170] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. It should be pointed out that any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a layered oxide positive electrode material for a sodium ion battery, characterized in that: The specific steps include: Step 1: After component testing, the reaction molten salt precursor and the metal salt are weighed according to the stoichiometric ratio; Step 2: After mixing the above salts, react during high temperature heat treatment to generate molten salt; Step 3: After the heat treatment, the sample is washed and dried to obtain the metal oxide; Step 4: mixing the metal oxide with the sodium source, and heat treating the mixture to obtain a layered oxide positive electrode material; Among them, the chemical composition of metal oxides is Na x MO y , where 0≤x≤1,1≤y≤2; The chemical composition of the layered oxide cathode material is Na x MO2, wherein 0.6≤x≤1, M is one or more of magnesium, aluminum, calcium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, copper, zinc, zirconium, and tin, and the phase composition is an O3 structure or a P2 structure or a mixed structure of O3 and P2; the reaction molten salt precursor includes one or more of carbonates, nitrates, oxalates, sulfates, halides, phosphates, and hydroxides of lithium, sodium, and potassium; the metal salt includes one or more of sulfates, halides, and phosphates of magnesium, aluminum, calcium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, copper, zinc, zirconium, and tin.

2. The method for preparing a sodium ion battery layered oxide positive electrode material according to claim 1, characterized in that: The metal salt comes from chemical reagents of chemical purity, analytical purity or higher purity, or from salts deteriorated due to oxidation and moisture absorption, or from industrial salts with one or more of the above ions as impurities, or from ferrous sulfate, a by-product of titanium dioxide production.

3. The method for preparing a sodium ion battery layered oxide positive electrode material according to claim 1, characterized in that: The material mixing method is grinding mixing, ball milling mixing or sand milling mixing.

4. The method for preparing a sodium ion battery layered oxide positive electrode material according to claim 1, characterized in that: The heat treatment conditions are: in dry air or oxygen atmosphere, the heating rate is 1-10 ℃ min -1 To 400 ℃ -1000 ℃, keep warm for 2-24 hours, and cool naturally after sintering.

5. The method for preparing a sodium ion battery layered oxide positive electrode material according to claim 1, characterized in that: The sodium source comes from one or more of sodium carbonate, sodium hydroxide, sodium nitrate and sodium oxalate.