A kind of water-soluble phenolic resin and preparation method thereof

By adjusting the substance ratio and temperature control of formaldehyde to phenol, a water-soluble phenolic resin with high content of hydroxymethyl group was prepared, which solved the problems of insufficient water solubility and poor compatibility of water-based phenolic resin, and improved the strength stability of rock wool boards and Hydrophobic nature.

CN118684845BActive Publication Date: 2024-11-01滁州都铂新材料科技有限公司 +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411166974.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-01
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

The existing water-based phenolic resins are insufficient in water solubility and poor compatibility with hydrophobic agents, resulting in unstable strength and deviation of hydrophobicity of rock wool boards.

Method used

By adjusting the substance ratio of formaldehyde to phenol and the formaldehyde addition process, the formation of hydroxymethyl groups is controlled, and the condensation reaction is slowed down through temperature regulation, a water-soluble phenolic resin with high content of hydroxymethyl groups is prepared to ensure its good proportion with the hydrophobic agent. Capacity.

Benefits of technology

The infinite water solubility of the aqueous phenolic resin and good compatibility with the hydrophobic agent are achieved, and the strength stability of the rock wool board is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118684845B_ABST
    Figure CN118684845B_ABST
Patent Text Reader

Abstract

The invention discloses a water-soluble phenolic resin and a preparation method thereof in the technical field of phenolic resins. The preparation method of the water-soluble phenolic resin comprises the following steps: weighing phenol and a 37% formaldehyde aqueous solution, weighing a catalyst, first adding the phenol and the catalyst, heating to 65-67°C, beginning to add a 37% formaldehyde aqueous solution to a reaction bottle, dripping it for 2.5 hours, then cooling to 60°C, dripping the remaining 20.3% of the 37% formaldehyde aqueous solution into the reaction bottle, and continuing to react for 2.5 hours. The invention adjusts the amount of hydroxymethyl groups generated by formaldehyde and phenol in the addition stage and determining the water solubility of the phenolic resin by controlling the molar ratio of formaldehyde to phenol and the process of adding formaldehyde, and then slowing down the condensation reaction between the generated hydroxymethyl groups by adjusting the temperature, so as to achieve the purpose of unlimited water solubility and good compatibility and stability with a hydrophobic agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of phenolic resins, in particular to a water-soluble phenolic resin and a preparation method thereof. Background Art

[0002] Phenolic resin has a history of 100 years since its industrialization. With its excellent mechanical properties, dimensional stability, heat resistance and flame retardancy, it is widely used in all walks of life today. As we all know, rock wool board is an inorganic fiber board made of basalt as the main raw material and processed by high-temperature melting. It has the excellent characteristics of light weight, low thermal conductivity, heat absorption and sound absorption, non-flammability, and stable chemical properties. It is also an environmentally friendly material. In recent years, with the rapid development of the construction industry, rock wool boards have been widely used. Water-based phenolic resin plays an indispensable role in the manufacture and use of rock wool boards. Water-based phenolic resin directly determines the tolerable strength of rock wool boards.

[0003] The existing water-based phenolic resin has a low water solubility and is prone to poor compatibility with water repellents, which results in unstable strength of the rock wool board and deviation or instability in water repellency. Summary of the invention

[0004] The purpose of this section is to summarize some aspects of the embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.

[0005] Therefore, the object of the present invention is to provide a water-soluble phenolic resin and a preparation method thereof, which can well solve the problems of insufficient water solubility of the phenolic resin and poor compatibility with a hydrophobic agent.

[0006] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:

[0007] A method for preparing a water-soluble phenolic resin comprises the following steps:

[0008] S1. Weigh phenol and 37% formaldehyde aqueous solution at a mass ratio of 1:2.76, and weigh a catalyst in an amount of 6.4%-8.84% of the mass of phenol. Add phenol and catalyst first, raise the temperature to 65-67°C, and start adding 79.7% of the weighed 37% formaldehyde aqueous solution to the reaction bottle, and drip it in 2.5 hours;

[0009] S2, then cool to 60°C, and then add the remaining 20.3% of the 37% formaldehyde aqueous solution dropwise into the reaction bottle, and continue the reaction for 2.5h;

[0010] S3. After the reaction is completed, the mixture obtained by the reaction is kept warm for 2 hours, then cooled to 40°C, urea in an amount of 3.02 times the mass of phenol and water in an amount of 2.476 times the mass of phenol are added, and the mixture is stirred for 30 minutes before discharging.

[0011] As a preferred embodiment of the method for preparing a water-soluble phenolic resin according to the present invention, the catalyst is one or two of sodium hydroxide, potassium hydroxide and triethylamine.

[0012] As a preferred embodiment of the method for preparing a water-soluble phenolic resin according to the present invention, in step S3, the insulation temperature is 40-60°C.

[0013] A water-soluble phenolic resin is prepared by a preparation method of the water-soluble phenolic resin.

[0014] Compared with the prior art, the present invention has the following beneficial effects: the present invention adjusts the amount of methylol groups that determine the water solubility of the phenolic resin generated by formaldehyde and phenol in the addition stage by controlling the molar ratio of formaldehyde to phenol and the process of adding formaldehyde, and then slows down the condensation reaction between the generated methylol groups by adjusting the temperature, thereby maximally ensuring that the content of methylol groups in the obtained water-based phenolic resin is at a high level, so that the purpose of unlimited water solubility and good compatibility and stability with the water repellent are finally achieved. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the present invention will be described in detail below in combination with the accompanying drawings and detailed embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:

[0016] Figure 1 The present invention is a flow chart of a method for preparing a water-soluble phenolic resin;

[0017] Figure 2 Schematic diagrams of test results of samples prepared in three embodiments and two comparative examples. DETAILED DESCRIPTION

[0018] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0019] The invention provides a water-soluble phenolic resin and a preparation method thereof, which solves the problems of insufficient water solubility of the phenolic resin and poor compatibility with a water-repellent agent.

[0020] In order to illustrate the above scheme, the following Examples 1-3 and Comparative Examples 1-2 are provided below for verification. Example 1

[0021] Add 50g of phenol, 0.4g of 32% sodium hydroxide, 2.8g of triethylamine and 110g of 37% formaldehyde aqueous solution into a reaction bottle, heat to 65°C, react for 2h, then cool to 60°C, add the remaining 28g of 37% formaldehyde aqueous solution, and continue to react for 2.5h. After the reaction is completed, keep the mixture warm for 2h, then cool to 40°C, add 151g of urea and 123.8g of water, stir for 30min and then discharge. Example 2

[0022] Add 50g of phenol, 0.4g of 32% sodium hydroxide and 2.8g of triethylamine into a reaction flask, heat it to 65°C, start to add 110g of 37% formaldehyde aqueous solution dropwise into the reaction flask, finish adding it after 2.5h, then cool it to 60°C, add the remaining 28g of 37% formaldehyde aqueous solution dropwise into the reaction flask over 15min, continue to react for 2.5h, after the reaction is completed, keep the mixture obtained by the reaction warm for 2h, then cool it to 40°C, add 151g of urea and 123.8g of water, stir for 30min and then discharge. Example 3

[0023] Add 50g of phenol and 4.42g of 32% sodium hydroxide into a reaction flask, raise the temperature to 67°C, begin to drop 110g of 37% formaldehyde aqueous solution into the reaction flask, finish dropping after 2.5h, then cool to 60°C, add the remaining 28g of 37% formaldehyde aqueous solution into the reaction flask over 15min, continue to react for 2.5h, after the reaction is completed, keep the mixture warm for 2h, then cool to 40°C, add 151g of urea and 123.8g of water, stir for 30min and discharge.

[0024] Comparative Example 1

[0025] 50g of phenol, 1.2g of 32% sodium hydroxide, 1.5g of triethylamine and 138g of 37% formaldehyde aqueous solution were added into the reaction bottle at one time, the temperature was raised to 75°C, the reaction was continued for 2h, the temperature was raised to 85°C, the reaction was continued for 2h, after the reaction was completed, the mixture was kept warm for 2h, then cooled to 40°C, 151g of urea and 123.8g of water were added, and the mixture was stirred for 30min before discharging.

[0026] Comparative Example 2

[0027] Add 50g of phenol, 0.4g of 32% sodium hydroxide, 2.8g of triethylamine and 110g of 37% formaldehyde aqueous solution into a reaction bottle, heat to 65°C, react for 2h, then add the remaining 28g of 37% formaldehyde aqueous solution, heat to 80°C, continue to react for 1h, after the reaction is completed, keep the mixture warm for 2h, then cool to 40°C, add 151g of urea and 123.8g of water, stir for 30min and then discharge.

[0028] The samples prepared in the three embodiments of the present invention and the two comparative examples were tested for water solubility and compatibility with the water repellent agent;

[0029] The water solubility test method is: take 10g of aqueous phenolic resin solution, gradually add water to the solution, and observe the change in the solution state at the same time.

[0030] The compatibility test method with the water repellent is: take 20g of aqueous phenolic resin solution, add 2g of water repellent emulsion, stir evenly and let stand at room temperature for 2h. If there is still no change, it means that the compatibility is good. If stratification or precipitation occurs, it means that the compatibility is poor.

[0031] The test results of the samples prepared in the three embodiments and two comparative examples are as follows Figure 2 As shown;

[0032] Depend on Figure 2 It can be clearly seen that, when other conditions remain unchanged, after the addition of formaldehyde in the latter stage, lowering the reaction temperature will lead to a significant improvement in water solubility. This is because the lower reaction temperature reduces the reaction probability between methylol groups to a certain extent, increases the content of methylol groups, and thus increases water solubility. When the formaldehyde is added in a dripping manner instead of a one-time addition, on the one hand, the temperature instability caused by the instantaneous heat release in the addition reaction stage can be slowed down. Secondly, the phenol in the system can be kept in a hungry state for a long time, avoiding the instantaneous increase in the concentration of methylol groups, and further reducing the reaction probability between methylol groups, thereby achieving a state of infinite miscibility with water. After the catalyst is changed to sodium hydroxide, both the water solubility and compatibility with the hydrophobic agent reach the best state.

[0033] Although the present invention has been described above with reference to the embodiments, various modifications may be made thereto and parts thereof may be replaced by equivalents without departing from the scope of the present invention. In particular, as long as there is no structural conflict, the various features in the embodiments disclosed in the present invention may be used in combination with each other in any manner, and the fact that these combinations are not exhaustively described in this specification is only for the sake of omitting space and saving resources. Therefore, the present invention is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.

Claims

1. A method for preparing a water-soluble phenolic resin, characterized in that: Here are the steps: S1. Weigh phenol and 37% formaldehyde aqueous solution at a mass ratio of 1:2.76, and weigh a catalyst in an amount of 6.4%-8.84% of the mass of phenol. Add phenol and catalyst first, raise the temperature to 65-67°C, and start adding 79.7% of the weighed 37% formaldehyde aqueous solution to the reaction bottle, and drip it in 2.5 hours; S2, then cool to 60°C, and then drop the remaining 20.3% of the 37% formaldehyde aqueous solution into the reaction bottle, and continue the reaction for 2.5h; S3. After the reaction is completed, the mixture obtained by the reaction is kept warm for 2 hours, then cooled to 40°C, urea in an amount of 3.02 times the mass of phenol and water in an amount of 2.476 times the mass of phenol are added, and the mixture is stirred for 30 minutes before discharging.

2. The method for preparing a water-soluble phenolic resin according to claim 1, wherein The catalyst is one or two of sodium hydroxide, potassium hydroxide and triethylamine.

3. A method for preparing a water-soluble phenolic resin according to claim 1, characterized in that: In step S3, the insulation temperature is 40-60°C.

4. A water-soluble phenolic resin, characterized in that The water-soluble phenolic resin is prepared by the preparation method of the water-soluble phenolic resin according to claim 1.