A method for preparing highly conductive carbon nanotube conductive slurry
By catalyzing phenolic resin to generate carbon nanotubes and hydrothermally modified graphene, combined with fatty amine and ball milling technology, the problem of difficult dispersion and poor stability of carbon nanotubes in conductive slurry is solved, achieving high conductivity and durability, and improving improve the performance of conductive paste.
Patent Information
- Application Number
- CN202411164081.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-08-23
AI Technical Summary
Carbon nanotubes in existing conductive slurries are difficult to disperse and have poor stability, resulting in poor conductivity and rough surface. In addition, a large amount of acetylene black is added, which affects circuit performance.
Using phenolic resin as the carbon source and carrier, carbon nanotubes are catalytically generated through hydroxylation of spherical nanometal nickel powder, combined with hydrothermal modification of graphene, addition of fatty amines and ball milling modification to form hybrid fillers and improve the quality of carbon nanotubes. Adhesion and dispersion, enhance conductivity.
High conductivity and durability are achieved. Through the synergistic effect of carbon nanotubes and hybrid fillers, uniform dispersion and chemical bond bridging improve the stability and conductive effect of the conductive slurry.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of conductive materials, in particular to a method for preparing a highly conductive carbon nanotube conductive slurry. Background Art
[0002] Conductive paste, as a basic electronic material with specific functions, is widely used in electronic circuit fields such as printed circuit boards, solar cells, surface mount, RFID radio frequency antennas, touch screen circuits, and flexible printed circuits (FPC). Currently, the application field of metal conductive pastes is usually to use these metal conductive pastes to prepare metal conductive films, and the commonly used film-forming technologies include embossing, printing, coating, spraying, etc.
[0003] Conductive pastes in the prior art mainly use conductive graphite, acetylene black and carbon nanotubes as conductive agents. Acetylene black is a chain composed of spherical amorphous carbon particles. It is the most widely used conductive agent at present, but in order to achieve the purpose of enhancing the mutual contact between electrode active substances, the required addition amount is relatively large. Carbon nanotubes are linear one-dimensional carbonaceous materials with better conductivity and less addition amount, but there is a disadvantage of difficulty in dispersion when used as a conductive agent. In addition, the conductive pastes currently on the market have poor stability, and the effective substances in the conductive pastes are unevenly distributed, resulting in rough surfaces of the metal conductive paste itself and the formed metal conductive film or electronic circuit, poor adhesion between conductive particles, and easy to cause poor conductivity of the circuit. In view of the above problems, the present invention provides a method for preparing a highly conductive carbon nanotube conductive paste. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a highly conductive carbon nanotube conductive paste to solve the problems existing in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a method for preparing a highly conductive carbon nanotube conductive paste, comprising the following preparation steps:
[0006] (1) First, 20 nm nano-spherical nickel powder is immersed in a hydrochloric acid aqueous solution for 2 h for hydroxylation, and the solid-liquid ratio of nickel powder to hydrochloric acid aqueous solution is 1:5 to obtain hydroxylated spherical nano-metal nickel powder; a certain amount of phenolic resin 2402, hexamethylenetetramine, ethylene glycol and anhydrous ethanol are weighed, and then 1-3% of the mass of phenolic resin 2402 hydroxylated spherical nano-metal nickel powder is weighed for use; then, the weighed phenolic resin 2402 hexamethylenetetramine and hydroxylated spherical nano-metal nickel powder are mixed evenly, and then ethylene glycol is added, and a glass rod is stirred at 150-250 rpm for 20-40 min, finally adding anhydrous ethanol, stirring with a glass rod at 150-250rpm for 1-2h to obtain a resin liquid; finally, stirring the obtained resin liquid at a speed of 6500-7500rpm for 10-20min using a high-speed shear emulsifier, and then curing at 200°C for 6-12h to obtain a cured resin; placing the cured resin in a horizontal tubular atmosphere furnace, passing pure argon at a rate of 0.5L / min, and heating to 900-1200°C at a heating rate of 5°C / min, and keeping it at this temperature for 3h for carbonization, and obtaining a carbon nanotube phenolic resin after the reaction is completed;
[0007] (2) Dispersing 1-5 parts of graphene oxide in 5 parts of deionized water, and preparing a graphene oxide dispersion liquid by 20kHz ultrasonic treatment for 20 minutes; then adding 0.05-0.15 parts of ammonia water and 0.3-0.5 parts of polyvinyl pyrrolidone (K-30) to the graphene oxide dispersion liquid, stirring at 200 rpm for 20 minutes to prepare a mixed solution; adding 0.05 parts of silver nitrate to 5 parts of deionized water, stirring at 300 rpm for 10 minutes to prepare a silver nitrate aqueous solution; mixing the prepared mixed solution with the silver nitrate aqueous solution, Then, after mixing with ultrasound at a power of 30-40kHz for 30 minutes, the mixture was transferred to a hydrothermal reactor at a temperature of 100-140°C and reacted for 8-14 hours to obtain a crude composite material; the crude composite material was centrifuged, washed twice with deionized water, and freeze-dried; the dried product was subjected to ball milling modification in a ball milling jar at a speed of 400-600rpm for 50-70 minutes, and then heat treated at 500-700°C and 0.085MPa for 20-120 minutes to obtain a silver-doped The invention discloses a method for preparing heterographene; weighing 1-10 parts of dodecylamine and dissolving them in acetonitrile with a volume of 7 times that of dodecylamine to obtain a dodecylamine solution; weighing 2-20 parts of isoamyl nitrite and dissolving them in acetonitrile with a volume of 7 times that of isoamyl nitrite to obtain an isoamyl nitrite solution; adjusting the dodecylamine solution and the isoamyl nitrite solution with acetonitrile to make the volumes of the two equal; then weighing 2-3 parts of silver-doped graphene and ultrasonically dispersing them in 25 parts of acetonitrile with an ultrasonic power of 20 kHz for 20 minutes, then adding 0.1-1 parts of formic acid and controlling the temperature to -60°C to obtain silver-doped graphene. under the protection of inert gas, dripping two solutions of dodecylamine solution and isoamyl nitrite solution into the silver-doped graphene suspension at the same time and speed, wherein the mass ratio of dodecylamine: nitrite: graphene is 1:1:0.1-10, the reaction temperature is -60-30°C, and stirring is carried out slowly at 60rpm, and the reaction is continued for 6-24h. After the reaction is completed, the temperature is naturally restored to room temperature, and the solvent is recovered by vacuum distillation. After filtering, the filtrate is taken, washed twice with deionized water, and then dried at room temperature for 6-12h to obtain fatty amine silver-doped graphene;
[0008] (3) The weight parts of the raw materials of the conductive paste are as follows: 3-6 parts of fatty amine silver-doped graphene, 10-20 parts of EM-110 water-based polyester resin emulsion, 15-25 parts of carbon nanotube phenolic resin, 1-3 parts of fatty acid glyceride, 3-7 parts of dimethyl silicone oil, 10-12 parts of methyl triacetoxy silane, and 5-10 parts of hydroxyethyl cellulose. The raw materials are mixed and blended at 2000 rpm to prepare a conductive paste.
[0009] Furthermore, the concentration of the aqueous hydrochloric acid solution in step (1) is 10%.
[0010] Furthermore, in the step (1), the mass ratio of phenolic resin 2402, hexamethylenetetramine, ethylene glycol and anhydrous ethanol is 3-5:0.3-1:5-12:10.
[0011] Furthermore, the mass ratio of the mixed solution to the silver nitrate aqueous solution in step (2) is 5:1-20.
[0012] Furthermore, in step (2), the centrifugal speed is 12000 rpm and the time is 10 min.
[0013] Furthermore, the freeze drying in step (2) is freeze drying at -40°C for 2h.
[0014] Furthermore, the inert gas in step (2) is nitrogen.
[0015] Furthermore, the dripping time in step (2) is controlled within 1-2 hours.
[0016] Furthermore, the reduced pressure distillation pressure in step (2) is 1.3-2.0 kPa.
[0017] Furthermore, the blending and stirring time in step (3) is 10-20 minutes.
[0018] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0019] The present invention uses phenolic resin as a raw material, generates carbon nanotubes in situ, and combines hybrid fillers to prepare a conductive paste to achieve a durable and high conductive effect.
[0020] Firstly, the present invention uses phenolic resin 2402 as a raw material for conductive paste, and utilizes nano-metal nickel powder to catalyze the in-situ generation of carbon nanotubes therein; spherical nano-metal nickel powder is selected, and its surface is enriched with hydroxyl groups through chemical modification, and carbon nanotubes are prepared on the basis of phenolic resin as a carbon source and carrier; carbon nanotubes have the advantages of high conductivity and large aspect ratio, etc., and the carbon nanotubes in-situ generated in phenolic resin have higher compatibility with the resin and better interface bonding, which improves the disadvantage of weak bonding affinity of carbon nanotubes and improves their adhesion and durability of conductive paste;
[0021] Secondly, the hydrothermal method is used to modify graphene, and the metallic silver particles are intercalated in the form of nano-needles. The silver-doped graphene is less likely to agglomerate. On this basis, the graphene is modified using aliphatic diazonium salts, so that the surface of the silver-doped graphene has aliphatic amines, and the inorganic and organic substances are combined to form a hybrid filler; then the hybrid filler is subjected to physical and mechanical modification by ball milling, so that the metallic silver and graphene are more closely combined and the coupling effect is better. Finally, a vacuum heat treatment is performed to make it more stable and less prone to oxidation; the hybrid filler is added to the conductive slurry, because the graphene in the hybrid filler has There are fatty amines, which are hydrogen-bonded with the hydroxyl groups on the surface of the modified metal nickel powder in the conductive paste, so that the surface of the nickel powder is wrapped by carbon nanotubes and hybrid fillers, which not only improves the dispersibility of the hybrid filler, but also makes the coated metal nickel powder less prone to oxidation, thereby obtaining good durability; the hybrid filler, carbon nanotubes and metal nickel powder are combined in pairs to stably maintain the flaky structure, the two metals of silver and nickel work synergistically, the carbon nanotubes and graphene work synergistically, the inorganic and organic are combined, and are evenly dispersed in the paste. At the same time, the chemical bond bridging between the substances makes the conductive effect of the paste even better. DETAILED DESCRIPTION
[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0023] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of a highly conductive carbon nanotube conductive paste prepared in the following examples are as follows:
[0024] Conductivity: The conductive pastes of the embodiments and comparative examples were printed on substrates using a screen printing process, with a screen mesh of 200 meshes, a screen tension of 30, and a film thickness of 25 μm; the substrate printed with the conductive paste was placed in a vacuum and dried at 85°C for 30 minutes; the dried substrate printed with the conductive paste was evenly placed in a laminating device, the temperature was set to 85°C, and the lamination time was 10 seconds. The resistivity of the prepared film was tested using a four-probe square resistance tester.
[0025] Durability: The conductive pastes of the embodiment and the comparative example were printed on the substrate by screen printing process, with a screen mesh of 200 meshes, a screen tension of 30, and a film thickness of 25 μm; the substrate printed with the conductive paste was placed in a vacuum and dried at 85°C for 30 minutes; the dried substrate printed with the conductive paste was evenly placed in a laminating device, the temperature was set to 85°C, and the lamination time was 10 seconds. The prepared film was placed at room temperature for 30 days, and then the resistivity of the film was tested by a four-probe square resistance tester.
[0026] Example 1; (1) First, 20 nm nano-spherical nickel powder is immersed in a 10% hydrochloric acid aqueous solution for 2 hours to perform hydroxylation, and the solid-liquid ratio of the nickel powder to the hydrochloric acid aqueous solution is 1:5, so as to obtain hydroxylated spherical nano-metal nickel powder; a certain amount of phenolic resin 2402, hexamethylenetetramine, ethylene glycol and anhydrous ethanol are weighed in a mass ratio of 3:0.3:5:10, and then 1% of the mass of phenolic resin 2402 is weighed for use; then, the weighed phenolic resin 2402 hexamethylenetetramine and hydroxylated spherical nano-metal nickel powder are first mixed evenly, Then, ethylene glycol was added, and the glass rod was stirred at 150 rpm for 20 minutes, and finally, anhydrous ethanol was added, and the glass rod was stirred at 150 rpm for 1 hour to obtain a resin liquid; finally, the obtained resin liquid was stirred at a speed of 6500 rpm for 10 minutes using a high-speed shear emulsifier, and then cured at 200°C for 6 hours to obtain a cured resin; the cured resin was placed in a horizontal tubular atmosphere furnace, pure argon was introduced at a rate of 0.5 L / min, and heated to 900°C at a heating rate of 5°C / min, and kept at this temperature for 3 hours for carbonization, and carbon nanotube phenolic resin was obtained after the reaction was completed;
[0027] (2) Disperse 1 part of graphene oxide in 5 parts of deionized water, and prepare a graphene oxide dispersion liquid by 20kHz ultrasonic treatment for 20 minutes; then add 0.05 parts of ammonia water and 0.3 parts of polyvinyl pyrrolidone (K-30) to the graphene oxide dispersion liquid, stir at 200 rpm for 20 minutes to prepare a mixed solution; add 0.05 parts of silver nitrate to 5 parts of deionized water, stir at 300 rpm for 10 minutes to prepare a silver nitrate aqueous solution; mix the prepared mixed solution and the silver nitrate aqueous solution in a mass ratio of 5:1, and then After mixing with 0kHz power ultrasound for 30min, the mixture was transferred to a hydrothermal reactor at a temperature of 100°C and reacted for 8h to obtain a crude composite material; the crude composite material was centrifuged at a centrifugal speed of 12000rpm for 10min, washed twice with deionized water, and freeze-dried at -40°C for 2h; the dried product was ball-milled in a ball milling jar at a ball milling speed of 400rpm for 50min, and then heat-treated at 500°C and 0.085MPa for 20min. The silver-doped graphene is obtained; 1 part of dodecylamine is weighed and dissolved in acetonitrile with a volume of 7 times that of dodecylamine to obtain a dodecylamine solution; 2 parts of isoamyl nitrite are weighed and dissolved in acetonitrile with a volume of 7 times that of isoamyl nitrite to obtain an isoamyl nitrite solution; the dodecylamine solution and the isoamyl nitrite solution are adjusted with acetonitrile to make the volumes of the two equal; then 2 parts of silver-doped graphene are weighed and ultrasonically dispersed in 25 parts of acetonitrile at an ultrasonic power of 20 kHz for 20 minutes, and then 0.1 parts of formic acid are added and the temperature is controlled at °C to obtain a silver-doped graphene suspension; Under the protection of gas, two solutions of dodecylamine solution and isoamyl nitrite solution were simultaneously and at the same speed dripped into the silver-doped graphene suspension, wherein the mass ratio of dodecylamine: nitrite: graphene was 1:1:0.1, the dropping time was controlled at 1h, the reaction temperature was -60°C, and the stirring was slow at 60rpm. The reaction lasted for 6h. After the reaction was completed, the temperature was naturally restored to room temperature, and the solvent was recovered by reduced pressure distillation at a pressure of 1.3kPa. The filtrate was filtered, washed twice with deionized water, and then dried at room temperature for 6h to obtain aliphatic amine silver-doped graphene;
[0028] (3) The weight parts of the raw materials constituting the conductive paste are as follows: 3 parts of fatty amine silver-doped graphene, 10 parts of EM-110 water-based polyester resin emulsion, 15 parts of carbon nanotube phenolic resin, 1 part of fatty acid glyceride, 3 parts of dimethyl silicone oil, 10 parts of methyl triacetoxy silane, and 5 parts of hydroxyethyl cellulose. The raw materials are mixed and stirred at 2000 rpm for 10 minutes to prepare a conductive paste.
[0029] Example 2; (1) First, 20 nm nano-spherical nickel powder was immersed in a 10% hydrochloric acid aqueous solution for 2 h for hydroxylation, and the solid-liquid ratio of the nickel powder to the hydrochloric acid aqueous solution was 1:5, so as to obtain hydroxylated spherical nano-metal nickel powder; a certain amount of phenolic resin 2402, hexamethylenetetramine, ethylene glycol and anhydrous ethanol were weighed in a mass ratio of 4:0.65:8.5:10, and then 2% of the mass of phenolic resin 2402 was weighed for use; then, the weighed phenolic resin 2402 hexamethylenetetramine and hydroxylated spherical nano-metal nickel powder were mixed evenly, Then, ethylene glycol was added, and the glass rod was stirred at 200 rpm for 30 minutes, and finally, anhydrous ethanol was added, and the glass rod was stirred at 200 rpm for 1.5 hours to obtain a resin liquid; finally, the obtained resin liquid was stirred at a speed of 7000 rpm for 15 minutes using a high-speed shear emulsifier, and then cured at 200°C for 9 hours to obtain a cured resin; the cured resin was placed in a horizontal tubular atmosphere furnace, pure argon was introduced at a rate of 0.5 L / min, and the temperature was increased by 5°C / min to 1050°C, and the temperature was kept at this temperature for 3 hours for carbonization, and the carbon nanotube phenolic resin was obtained after the reaction was completed;
[0030] (2) Disperse 3 parts of graphene oxide in 5 parts of deionized water, and prepare a graphene oxide dispersion liquid by 20 kHz ultrasonic treatment for 20 min; then add 0.1 parts of ammonia water and 0.4 parts of polyvinyl pyrrolidone (K-30) to the graphene oxide dispersion liquid, stir at 200 rpm for 20 min to prepare a mixed solution; add 0.05 parts of silver nitrate to 5 parts of deionized water, stir at 300 rpm for 10 min to prepare a silver nitrate aqueous solution; mix the prepared mixed solution and the silver nitrate aqueous solution in a mass ratio of 5:10, and then After mixing with high-power ultrasound for 30 minutes, the mixture was transferred to a hydrothermal reactor at a temperature of 120°C and reacted for 11 hours to obtain a crude composite material; the crude composite material was centrifuged at a centrifugal speed of 12000 rpm for 10 minutes, washed twice with deionized water, and freeze-dried at -40°C for 2 hours; the dried product was ball-milled in a ball mill at a speed of 500 rpm for 60 minutes, and then heat-treated at 600°C and 0.085 MPa for 70 minutes to obtain a silver-doped miscellaneous graphene; weigh 5.5 parts of dodecylamine and dissolve it in acetonitrile with a volume of 7 times that of dodecylamine to obtain a dodecylamine solution; weigh 11 parts of isoamyl nitrite and dissolve it in acetonitrile with a volume of 7 times that of isoamyl nitrite to obtain an isoamyl nitrite solution; adjust the dodecylamine solution and the isoamyl nitrite solution with acetonitrile to make the volumes of the two equal; then weigh 2.5 parts of silver-doped graphene and ultrasonically disperse it in 25 parts of acetonitrile, with an ultrasonic power of 20 kHz and a time of 20 minutes, then add 0.65 parts of formic acid, control the temperature to -60°C, and obtain a silver-doped graphene suspension; Under nitrogen protection, two solutions of dodecylamine solution and isoamyl nitrite solution were simultaneously and at the same speed dripped into the silver-doped graphene suspension, wherein the mass ratio of dodecylamine: nitrite: graphene was 1:1:5, the dropping time was controlled at 1.5h, the reaction temperature was -15°C, and the stirring was slow at 60rpm. The reaction was continued for 15h. After the reaction was completed, the temperature was naturally restored to room temperature, and the solvent was recovered by reduced pressure distillation at a pressure of 1.6kPa. The filtrate was filtered, washed twice with deionized water, and then dried at room temperature for 9h to obtain aliphatic amine silver-doped graphene;
[0031] (3) The weight parts of the raw materials constituting the conductive paste are as follows: 4.5 parts of fatty amine silver-doped graphene, 15 parts of EM-110 water-based polyester resin emulsion, 20 parts of carbon nanotube phenolic resin, 2 parts of fatty acid glyceride, 5 parts of dimethyl silicone oil, 11 parts of methyl triacetoxysilane, and 7.5 parts of hydroxyethyl cellulose. The raw materials are mixed and stirred at 2000 rpm for 15 minutes to prepare a conductive paste.
[0032] Example 3; (1) First, 20 nm nano-spherical nickel powder was immersed in a 10% hydrochloric acid aqueous solution for 2 h for hydroxylation, and the solid-liquid ratio of nickel powder to hydrochloric acid aqueous solution was 1:5 to obtain hydroxylated spherical nano-metal nickel powder; a certain amount of phenolic resin 2402, hexamethylenetetramine, ethylene glycol and anhydrous ethanol were weighed in a mass ratio of 5:1:12:10, and 3% of the mass of phenolic resin 2402 was weighed for standby use; then, the weighed phenolic resin 2402 hexamethylenetetramine and hydroxylated spherical nano-metal nickel powder were mixed evenly, and then added Ethylene glycol was added, and the glass rod was stirred at 250 rpm for 40 min, and finally anhydrous ethanol was added, and the glass rod was stirred at 250 rpm for 2 h to obtain a resin liquid; finally, the obtained resin liquid was stirred at a speed of 7500 rpm for 20 min using a high-speed shear emulsifier, and then cured at 200°C for 12 h to obtain a cured resin; the cured resin was placed in a horizontal tubular atmosphere furnace, pure argon was introduced at a rate of 0.5 L / min, and the temperature was increased by 5°C / min to 1200°C, and the temperature was kept at this temperature for 3 h for carbonization, and the carbon nanotube phenolic resin was obtained after the reaction was completed;
[0033] (2) Disperse 5 parts of graphene oxide in 5 parts of deionized water, and prepare a graphene oxide dispersion liquid by 20kHz ultrasonic treatment for 20 minutes; then add 0.15 parts of ammonia water and 0.5 parts of polyvinyl pyrrolidone (K-30) to the graphene oxide dispersion liquid, stir at 200 rpm for 20 minutes to prepare a mixed solution; add 0.05 parts of silver nitrate to 5 parts of deionized water, stir at 300 rpm for 10 minutes to prepare a silver nitrate aqueous solution; mix the prepared mixed solution and the silver nitrate aqueous solution in a mass ratio of 5:20, and then After mixing with 0kHz power ultrasound for 30min, the mixture was transferred to a hydrothermal reactor at a temperature of 140°C and reacted for 14h to obtain a crude composite material; the crude composite material was centrifuged at a centrifugal speed of 12000rpm for 10min, washed twice with deionized water, and freeze-dried at -40°C for 2h; the dried product was ball-milled in a ball mill jar at a speed of 600rpm for 70min, and then heat-treated at 700°C and 0.085MPa for 120min. The silver-doped graphene is obtained; 10 parts of dodecylamine are weighed and dissolved in acetonitrile with a volume of 7 times that of dodecylamine to obtain a dodecylamine solution; 20 parts of isoamyl nitrite are weighed and dissolved in acetonitrile with a volume of 7 times that of isoamyl nitrite to obtain an isoamyl nitrite solution; the dodecylamine solution and the isoamyl nitrite solution are adjusted with acetonitrile to make the volumes of the two equal; then 3 parts of silver-doped graphene are weighed and ultrasonically dispersed in 25 parts of acetonitrile, the ultrasonic power is 20kHz, the time is 20min, and then 1 part of formic acid is added, and the temperature is controlled to -60°C to obtain a silver-doped graphene suspension; Under nitrogen protection, two solutions of dodecylamine solution and isoamyl nitrite solution were simultaneously and at the same speed dripped into the silver-doped graphene suspension, wherein the mass ratio of dodecylamine: nitrite: graphene was 1:1:10, the dropping time was controlled at 2h, the reaction temperature was 30°C, and the stirring was slow at 60rpm. The reaction lasted for 24h. After the reaction was completed, the temperature was naturally restored to room temperature, and the solvent was recovered by reduced pressure distillation at a pressure of 2.0kPa. The filtrate was filtered, washed twice with deionized water, and then dried at room temperature for 12h to obtain aliphatic amine silver-doped graphene.
[0034] (3) The weight parts of the raw materials constituting the conductive paste are as follows: 6 parts of fatty amine silver-doped graphene, 20 parts of EM-110 water-based polyester resin emulsion, 25 parts of carbon nanotube phenolic resin, 3 parts of fatty acid glyceride, 7 parts of dimethyl silicone oil, 12 parts of methyl triacetoxy silane, and 10 parts of hydroxyethyl cellulose. The raw materials are mixed and stirred at 2000 rpm for 20 minutes to prepare a conductive paste.
[0035] Comparative Example 1; The difference between Comparative Example 1 and Example 2 is that step (1) is different, and step (1) is changed to: weigh a certain amount of phenolic resin 2402, hexamethylenetetramine, ethylene glycol and anhydrous ethanol, the mass ratio of which is 4:0.65:8.5:10, and then weigh 2% of the mass of phenolic resin 2402 hydroxylated spherical nano-metal nickel powder for use; then first mix the weighed phenolic resin 2402 hexamethylenetetramine and nano-metal nickel powder evenly, then add ethylene glycol, stir with a glass rod at 200rpm for 30min, and finally add anhydrous ethanol. The obtained resin liquid was stirred at 7000 rpm for 15 min using a high-speed shear emulsifier, and then cured at 200°C for 9 h to obtain a cured resin; the cured resin was placed in a horizontal tubular atmosphere furnace, pure argon was introduced at a rate of 0.5 L / min, and heated to 1050°C at a heating rate of 5°C / min, and kept at this temperature for 3 h for carbonization, and carbon nanotube phenolic resin was obtained after the reaction was completed; the remaining steps were the same as in Example 2.
[0036] Comparative Example 2: The difference between Comparative Example 2 and Example 2 is that step (1) is changed to: first, immerse nano-spherical nickel powder with a particle size of 20 nm in a 10% hydrochloric acid aqueous solution for 2 hours to carry out hydroxylation, and the solid-liquid ratio of the nickel powder to the hydrochloric acid aqueous solution is 1:5 to obtain hydroxylated spherical nano-metal nickel powder; weigh 10 parts of phenolic resin 2402 and 0.2 parts of hydroxylated spherical nano-metal nickel powder by mass of the phenolic resin 2402, and then add 0.2 parts of carbon nanotubes, and stir with a glass rod at 200 rpm for 30 minutes; stir the obtained resin liquid at a speed of 7000 rpm for 15 minutes using a high-speed shear emulsifier, and then cure it at 200°C for 9 hours to obtain a carbon nanotube phenolic resin; the remaining steps are the same as Example 2.
[0037] Comparative Example 3: The difference between Comparative Example 3 and Example 2 lies in the difference in steps (2) and (3). Steps (2) and (3) are changed to: (2) 5.5 parts of dodecylamine are weighed and dissolved in acetonitrile with a volume of 7 times that of dodecylamine to obtain a dodecylamine solution; 11 parts of isoamyl nitrite are weighed and dissolved in acetonitrile with a volume of 7 times that of isoamyl nitrite to obtain an isoamyl nitrite solution; acetonitrile is used to adjust the volumes of the dodecylamine solution and the isoamyl nitrite solution to be equal; then 2.5 parts of silver-doped graphene are weighed and ultrasonically dispersed in 25 parts of acetonitrile at an ultrasonic power of 20 kHz and a time of 20 m in, then add 0.65 parts of formic acid, control the temperature to -60 ° C, and obtain a graphene suspension; under nitrogen protection, drip the dodecylamine solution and the isoamyl nitrite solution into the graphene suspension at the same speed at the same time, the dripping time is controlled at 1.5h, the reaction temperature is -15 ° C, and the stirring is slow at 60rpm. The reaction is continued for 15h. After the reaction is completed, it is naturally restored to room temperature, and the solvent is recovered by vacuum distillation at a pressure of 1.6kPa. After filtering, the filtrate is taken, washed twice with deionized water, and then dried at room temperature for 9h to obtain fatty amine graphene;
[0038] (3) The weight parts of the raw materials constituting the conductive paste are: 4.5 parts of fatty amine graphene, 15 parts of EM-110 water-based polyester resin emulsion, 20 parts of carbon nanotube phenolic resin, 2 parts of fatty acid glyceride, 5 parts of dimethyl silicone oil, 11 parts of methyl triacetoxy silane, and 7.5 parts of hydroxyethyl cellulose. The raw materials are mixed and stirred at 2000 rpm for 15 minutes to prepare a conductive paste; the remaining steps are the same as in Example 2.
[0039] Comparative Example 4: The difference between Comparative Example 4 and Example 2 is that step (2) is different, and step (2) is changed to: 3 parts of graphene oxide are dispersed in 5 parts of deionized water, and 20kHz ultrasound is applied for 20 minutes to prepare a graphene oxide dispersion; then 0.1 parts of ammonia water and 0.4 parts of polyvinyl pyrrolidone (K-30) are added to the graphene oxide dispersion, and the mixture is stirred at 200 rpm for 20 minutes to prepare a mixed solution; 0.05 parts of silver nitrate are added to 5 parts of deionized water, and the mixture is stirred at 300 rpm for 10 minutes. The silver nitrate aqueous solution was prepared; the prepared mixed solution and the silver nitrate aqueous solution were mixed at a mass ratio of 5:10, and then mixed by 35kHz power ultrasound for 30 minutes, and then transferred to a hydrothermal reactor at a temperature of 120°C. After reacting for 11 hours, a crude composite material was obtained; the crude composite material was centrifuged at a centrifugal speed of 12000rpm for 10 minutes, washed twice with deionized water, and freeze-dried at -40°C for 2 hours to obtain silver-doped graphene; 5.5 parts of dodecylamine were weighed and dissolved in 7 times the volume of dodecylamine. nitrile to obtain a dodecylamine solution; weigh 11 parts of isoamyl nitrite and dissolve it in acetonitrile with a volume of 7 times that of isoamyl nitrite to obtain an isoamyl nitrite solution; adjust the dodecylamine solution and the isoamyl nitrite solution with acetonitrile to make the volumes of the two equal; then weigh 2.5 parts of silver-doped graphene and ultrasonically disperse it in 25 parts of acetonitrile, with an ultrasonic power of 20 kHz and a time of 20 min, then add 0.65 parts of formic acid and control the temperature to -60°C to obtain a silver-doped graphene suspension; under nitrogen protection, the dodecylamine solution and the isoamyl nitrite were mixed and stirred for 2 hours. Two solutions of amyl ester solution are dripped into the silver-doped graphene suspension at the same time and speed, wherein the mass ratio of dodecylamine: nitrite: graphene is 1:1:5, the dropping time is controlled at 1.5h, the reaction temperature is -15°C, and the stirring is slowly carried out at 60rpm. The reaction is continued for 15h. After the reaction is completed, the temperature is naturally restored to room temperature, and the solvent is recovered by reduced pressure distillation at a pressure of 1.6kPa. The filtrate is taken after filtration, washed twice with deionized water, and then dried at room temperature for 9h to obtain fatty amine silver-doped graphene; the remaining steps are the same as Example 2.
[0040] Comparative Example 5: The difference between Comparative Example 5 and Example 2 is that steps (2) and (3) are different. Steps (2) and (3) are changed to: 3 parts of graphene oxide are dispersed in 5 parts of deionized water, and 20kHz ultrasound is applied for 20 minutes to prepare a graphene oxide dispersion; then 0.1 parts of ammonia water and 0.4 parts of polyvinyl pyrrolidone (K-30) are added to the graphene oxide dispersion, and the mixture is stirred at 200 rpm for 20 minutes to prepare a mixed solution; 0.05 parts of silver nitrate are added to 5 parts of deionized water, and the mixture is stirred at 300 rpm for 10 minutes to prepare a silver nitrate aqueous solution; the prepared mixed solution and the silver nitrate aqueous solution are mixed. The mixture was mixed with the liquid in a mass ratio of 5:10, and then mixed with ultrasound at a power of 35kHz for 30 minutes, and then transferred to a hydrothermal reactor at a temperature of 120°C. After reacting for 11 hours, a crude composite material was obtained; the crude composite material was centrifuged at a centrifugal speed of 12000rpm for 10 minutes, washed twice with deionized water, and freeze-dried at -40°C for 2 hours; the dried product was ball-milled in a ball milling jar at a speed of 500rpm for 60 minutes, and then heat-treated at 600°C and 0.085MPa for 70 minutes to obtain silver-doped graphene;
[0041] (3) The weight parts of the raw materials constituting the conductive paste are: 4.5 parts of silver-doped graphene, 15 parts of EM-110 water-based polyester resin emulsion, 20 parts of carbon nanotube phenolic resin, 2 parts of fatty acid glyceride, 5 parts of dimethyl silicone oil, 11 parts of methyl triacetoxy silane, and 7.5 parts of hydroxyethyl cellulose. The raw materials are mixed and stirred at 2000 rpm for 15 minutes to prepare a conductive paste; the remaining steps are the same as in Example 2.
[0042] Effect example
[0043] Table 1 below shows the performance analysis results of a highly conductive carbon nanotube conductive paste using Examples 1 to 3 of the present invention and Comparative Examples 1 to 5.
[0044] Table 1
[0045]
[0046] From the comparison of the durability experimental data of the embodiment and the comparative example, it can be found that the present invention uses phenolic resin 2402 as the raw material of the conductive paste, and uses nano-metal nickel powder to catalyze the in-situ generation of carbon nanotubes; spherical nano-metal nickel powder is selected, and its surface is rich in hydroxyl groups through chemical modification, and carbon nanotubes are prepared on the basis of phenolic resin as a carbon source and carrier; carbon nanotubes have the advantages of high conductivity and large aspect ratio, and the carbon nanotubes generated in situ in the phenolic resin have higher compatibility with the resin, better interface bonding, and improve the disadvantage of weak binding affinity of carbon nanotubes, and improve its adhesion and the durability of the conductive paste. The hydrothermal method is used to modify graphene, and the metal silver particles are intercalated and doped with nano-needle layers, and the silver-doped graphene is less likely to agglomerate. On this basis, the graphene is modified by aliphatic diazonium salt, so that the surface of the silver-doped graphene has aliphatic amines, and inorganic and organic substances are combined to form hybrid fillers. Then the hybrid filler is subjected to physical and mechanical modification by ball milling, so that the metal silver and graphene are more closely combined and the coupling effect is more excellent, and finally vacuum heat treatment is performed to make it more stable and not easy to oxidize; the hybrid filler is added to the conductive slurry, because the graphene in the hybrid filler has aliphatic amine, and the hydroxyl group on the surface of the modified metal nickel powder in the conductive slurry is hydrogen bonded, so that the surface of the nickel powder is wrapped by carbon nanotubes and hybrid fillers, which improves the dispersibility of the hybrid filler, and also makes the metal nickel powder coated and not easy to oxidize, thereby obtaining good durability. From the comparison of the experimental data of the conductivity of the embodiment and the comparative example, it can be found that the present invention uses hybrid fillers, carbon nanotubes and metal nickel powder as raw materials to combine two by two, stably maintain the sheet structure, the two metals of silver and nickel work synergistically, the carbon nanotubes and graphene work synergistically, the inorganic and organic are combined, and are evenly dispersed in the slurry, and at the same time the chemical bond bridging between the substances makes the conductive effect of the slurry even better.
[0047] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A method for preparing a highly conductive carbon nanotube conductive paste, characterized in that: The method comprises the following preparation steps: (1) First, 20 nm nano-spherical nickel powder was immersed in a hydrochloric acid aqueous solution for 2 h, and the solid-liquid ratio of nickel powder to hydrochloric acid aqueous solution was 1:5 g / mL to obtain hydroxylated nano-spherical nickel powder; phenolic resin 2402, hexamethylenetetramine and hydroxylated nano-spherical nickel powder were mixed evenly, and the mass ratio of hydroxylated nano-spherical nickel powder to phenolic resin 2402 was 0.01-0.03:1, and then ethylene glycol was added, and stirred at 150-250 rpm for 20-40 min, and finally added Anhydrous ethanol, stirring at 150-250rpm for 1-2h, stirring at a speed of 6500-7500rpm for 10-20min, and then curing at 200℃ for 6-12h to obtain a cured resin; placing the cured resin in a horizontal tubular atmosphere furnace, passing pure argon at a rate of 0.5L / min, and heating to 900-1200℃ at a heating rate of 5℃ / min, and keeping it at this temperature for 3h for carbonization, and obtaining a carbon nanotube phenolic resin after the reaction is completed; (2) Disperse 1-5 parts of graphene oxide in 5 parts of deionized water, and prepare a graphene oxide dispersion liquid by 20kHz ultrasonic treatment for 20 minutes; then add 0.05-0.15 parts of ammonia water and 0.3-0.5 parts of polyvinyl pyrrolidone (K-30) to the graphene oxide dispersion liquid, and stir at 200 rpm for 20 minutes to prepare a mixed solution; add 0.05 parts of silver nitrate to 5 parts of deionized water, and stir at 300 rpm for 10 minutes to prepare a silver nitrate aqueous solution; The obtained crude composite material is centrifuged, washed twice with deionized water, and freeze-dried; the dried product is subjected to ball milling modification, the ball milling is carried out in a ball milling jar, the ball milling speed is 400-600rpm, the ball milling time is 50-70min, and then heated at 500-700℃ and 0.085MPa. Heat treatment for 20-120 minutes to obtain silver-doped graphene; weigh 1-10 parts of dodecylamine and dissolve it in acetonitrile with a volume of 7 times that of dodecylamine to obtain a dodecylamine solution; weigh 2-20 parts of isoamyl nitrite and dissolve it in acetonitrile with a volume of 7 times that of isoamyl nitrite to obtain an isoamyl nitrite solution; then weigh 2-3 parts of silver-doped graphene and ultrasonically disperse it in 25 parts of acetonitrile, with an ultrasonic power of 20kHz and a time of 20 minutes, then add 0.1-1 parts of formic acid and control the temperature to -60°C to obtain silver-doped graphene. under the protection of inert gas, adding two solutions, dodecylamine solution and isoamyl nitrite solution, to the silver-doped graphene suspension at the same time, wherein the mass ratio of dodecylamine: nitrite: graphene is 1:1:0.1-10, the reaction temperature is -60-30°C, and the stirring is slow at 60 rpm. The reaction is continued for 6-24 hours. After the reaction is completed, the temperature is naturally restored to room temperature, and the filtrate is filtered, washed twice with deionized water, and then dried at room temperature for 6-12 hours to obtain aliphatic amine silver-doped graphene; (3) The weight parts of the raw materials of the conductive paste are as follows: 3-6 parts of fatty amine silver-doped graphene, 10-20 parts of EM-110 water-based polyester resin emulsion, 15-25 parts of carbon nanotube phenolic resin, 1-3 parts of fatty acid glyceride, 3-7 parts of dimethyl silicone oil, 10-12 parts of methyl triacetoxy silane, and 5-10 parts of hydroxyethyl cellulose. The raw materials are mixed and blended at 2000 rpm to prepare a conductive paste.
2. The method for preparing a highly conductive carbon nanotube conductive paste according to claim 1, characterized in that: The concentration of the hydrochloric acid aqueous solution in step (1) is 10%.
3. The method for preparing a highly conductive carbon nanotube conductive paste according to claim 1, characterized in that: In the step (1), the mass ratio of phenolic resin 2402, hexamethylenetetramine, ethylene glycol and anhydrous ethanol is 3-5:0.3-1:5-12:
10.
4. The method for preparing a highly conductive carbon nanotube conductive paste according to claim 1, characterized in that: The mass ratio of the mixed solution to the silver nitrate aqueous solution in step (2) is 5:1-20.
5. The method for preparing a highly conductive carbon nanotube conductive paste according to claim 1, characterized in that: In step (2), the centrifugal speed is 12000 rpm and the time is 10 min.
6. The method for preparing a highly conductive carbon nanotube conductive paste according to claim 1, characterized in that: The freeze drying in step (2) is performed at -40°C for 2 hours.
7. The method for preparing a highly conductive carbon nanotube conductive paste according to claim 1, characterized in that: The inert gas in step (2) is nitrogen.
8. The method for preparing a highly conductive carbon nanotube conductive paste according to claim 1, characterized in that: The dropping time in step (2) is controlled within 1-2 hours.
9. The method for preparing a highly conductive carbon nanotube conductive paste according to claim 1, characterized in that: The mixing time in step (3) is 10-20 minutes.