A graphene-improved resin-based hard carbon material

By using graphene improved resin-based hard carbon material in sodium ion batteries, combining the mesoporous and layered structure of single-layer graphene oxide and resin-based hard carbon material, the insufficient performance of sodium ion battery materials in the prior art is solved. Problem, high sodium storage capacity, excellent magnification and good cycle stability are achieved.

CN118693271BActive Publication Date: 2024-11-29JIANGSU ZENIO NEW ENERGY BATTERY TECH CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411171471.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-29
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

The existing sodium ion battery negative electrode materials are difficult to take into account both high specific capacity, excellent first-time Coulomb efficiency and good rate performance, and the phenolic resin-based hard carbon materials have problems such as low initial Coulomb efficiency, limited circulation capacity and toxic synthesis process.

Method used

Using graphene-improved resin-based hard carbon material, a single layer of graphene oxide and resin-based hard carbon material are connected by covalent bonds to form a mesoporous structure and a layered structure, and cross-linking and ester are used for cross-linking of amino and carboxyl groups. The transformation reaction forms a mesh structure and pore structure to improve the flexibility and structural stability of the material.

Benefits of technology

The high sodium storage capacity, excellent rate performance, good cycle stability and high first-time Coulomb efficiency of graphene improved resin-based hard carbon materials in sodium ion batteries are achieved, and the overall performance of the material is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118693271B_ABST
    Figure CN118693271B_ABST
Patent Text Reader

Abstract

The present application relates to the field of battery technology, and specifically to a graphene-modified resin-based hard carbon material. The graphene-modified resin-based hard carbon material comprises: a resin-based hard carbon material; a monolayer of graphene oxide, wherein the monolayer of graphene oxide is covalently bonded to the surface of the resin-based hard carbon material. The graphene-modified resin-based hard carbon material provided by the present invention has good flexibility and structural stability. The graphene-modified resin-based hard carbon material is applied to a sodium ion battery, and the sodium ion battery exhibits good cycle stability and high first coulombic efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a graphene-modified resin-based hard carbon material. Background Art

[0002] Hard carbon has the advantages of high specific capacity, low potential and stable cycle performance, and has become one of the most promising negative electrode materials for sodium ion batteries. However, when hard carbon is carbonized at a temperature below 1000°C, its specific surface area is high, which shows a very low first coulombic efficiency. Therefore, the commonly used method is to carbonize at a temperature above 1300°C to reduce the specific surface area of ​​hard carbon, thereby improving the first coulombic efficiency of hard carbon. However, this not only increases the additional preparation cost, but also high-temperature carbonization will increase the degree of graphitization of hard carbon, reduce heteroatoms, and reduce porosity, which will lead to poor rate performance of hard carbon. In order to solve the problem that the existing sodium ion battery negative electrode materials cannot take into account the specific capacity, first coulombic efficiency and rate performance at the same time, it is necessary to develop new hard carbon negative electrode materials.

[0003] Phenolic resin is a hard carbon precursor that can produce high-purity carbon. It can also be known from the relevant literature that it has good application prospects. Benefiting from the high carbon content, adjustable chemical structure and mature commercial production technology of phenolic resin, it is considered to be one of the most promising precursors for commercial sodium storage. The hard carbon prepared by phenolic resin has a low specific surface area and a larger low-potential platform capacity. However, phenolic resin-based hard carbon has the shortcomings of low initial Coulomb efficiency, limited cycling capacity, toxic synthesis process and insufficient flexibility. Summary of the invention

[0004] In view of this, the present invention provides a graphene-modified resin-based hard carbon material. The graphene-modified resin-based hard carbon material has good flexibility and structural stability. The graphene-modified resin-based hard carbon material is applied to a sodium ion battery, and the sodium ion battery exhibits good cycle stability and high first coulomb efficiency.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] In a first aspect, the present invention provides a graphene-modified resin-based hard carbon material, the graphene-modified resin-based hard carbon material comprising:

[0007] A resin-based hard carbon material having a layered structure;

[0008] The monolayer graphene oxide is connected to the surface of the resin-based hard carbon material through a covalent bond.

[0009] Preferably, the graphene-modified resin-based hard carbon material has a mesoporous structure, and the pore size of the mesoporous structure is 2 to 50 nm.

[0010] Preferably, the pore size of the mesoporous structure is 2 to 20 nm.

[0011] Preferably, the specific surface area of ​​the graphene-modified resin-based hard carbon material is 10 to 20 g / cm 2 .

[0012] Preferably, the interlayer spacing of the resin-based hard carbon material is 0.40 to 0.42 nm.

[0013] In an embodiment of the present invention, the covalent bond comprises an N—C bond and / or a C—O bond.

[0014] In a second aspect, the present invention provides a method for preparing the above-mentioned graphene-improved resin-based hard carbon material, comprising the following steps:

[0015] S1, mixing resin prepolymer, cross-linking agent, monolayer graphene oxide and ethanol uniformly to obtain a mixed solution;

[0016] S2, heating the mixed solution to obtain a cured resin;

[0017] S3, grinding the cured resin into powder, and pre-carbonizing the powder under an inert gas atmosphere to obtain a pre-carbonized product;

[0018] S4, subjecting the pre-carbonized product to high-temperature carbonization treatment under an inert gas atmosphere to obtain a graphene-modified resin-based hard carbon material.

[0019] In an embodiment of the present invention, the resin prepolymer includes at least one of a phenolic resin prepolymer, a urea-formaldehyde resin prepolymer, an epoxy resin prepolymer, a melamine resin prepolymer, and a lignin phenolic resin prepolymer.

[0020] In an embodiment of the present invention, the cross-linking agent is a cross-linking agent having an amino group and a carboxyl group.

[0021] Preferably, the cross-linking agent is p-aminobenzoic acid.

[0022] Preferably, the cross-linking agent having amino and carboxyl groups undergoes a dehydration condensation reaction with the carboxyl groups of the monolayer graphene oxide to generate N-C bonds.

[0023] Preferably, the crosslinking agent having amino and carboxyl groups undergoes an esterification reaction with the hydroxyl group of the resin prepolymer to form a C—O bond.

[0024] Preferably, the mass ratio of the resin prepolymer, the cross-linking agent and the single-layer graphene oxide is (5-10): (1-5): (1-2).

[0025] Preferably, the concentration of the mixed solution is 0.05 to 1 g / mL.

[0026] Preferably, the temperature of the heating treatment is 120 to 180° C., and the time of the heating treatment is 1 to 10 hours.

[0027] Preferably, the temperature of the pre-carbonization treatment is 300-800° C., and the time of the pre-carbonization treatment is 5-15 hours.

[0028] Preferably, the temperature of the high temperature carbonization treatment is 1200-1800° C., and the time of the high temperature carbonization treatment is 1-5 hours.

[0029] In a third aspect, the present invention provides a negative electrode sheet, which includes the above-mentioned graphene-modified resin-based hard carbon material, or the graphene-modified resin-based hard carbon material prepared by the above-mentioned preparation method.

[0030] In a fourth aspect, the present invention provides a sodium ion battery, which comprises the negative electrode sheet of the present invention.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] The present invention uses a cross-linking agent with amino and carboxyl groups as the key to the cross-linking of the resin improved by graphene oxide, and uses the chemical reaction between functional groups to complete the cross-linking of the resin prepolymer and the modification of graphene oxide in one step. First, the amino group of the cross-linking agent and the carboxyl functional group of the graphene oxide are spontaneously dehydrated and condensed to form an amide bond, and the cross-linking agent is connected to the graphene oxide single-layer nanosheet, and then the carboxyl group of the cross-linking agent and the hydroxyl group of the resin prepolymer are linked by an ester bond generated by an esterification reaction, and finally the graphene oxide in-situ polymerized resin material is formed.

[0033] First, the cross-linking agent not only acts as a bridge to connect the graphene oxide nanosheets and the resin prepolymer to form a network structure, but also inhibits the directional growth of the carbon layer in the subsequent carbonization, so that it forms a layered graphite-like domain structure, which is conducive to the expansion of the interlayer spacing;

[0034] Secondly, the in-situ polymerization of graphene oxide modified resin increases the overall flexibility and conductivity of the material while preventing wrinkles in the nanosheets themselves and enhancing structural stability;

[0035] Thirdly, ethanol serves as a cross-linking reaction solvent and also as a pore-forming agent. The cross-linked product is finally carbonized to obtain a resin hard carbon material improved with graphene oxide having a large number of pores.

[0036] The graphene-modified resin-based hard carbon material of the present invention has a large interlayer spacing, good flexibility and outstanding structural stability. The graphene-modified resin-based hard carbon material is applied to a sodium ion battery, and the sodium ion battery exhibits high sodium storage capacity, excellent rate, excellent reversible specific capacity, good cycle stability and high first coulombic efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 . SEM of the graphene-modified resin-based hard carbon material in Example 1.

[0038] Figure 2 . Pore size distribution of the graphene-modified resin-based hard carbon material in Example 1.

[0039] Figure 3 . Transmission electron microscopy image of the graphene-modified resin-based hard carbon material in Example 1. DETAILED DESCRIPTION

[0040] The present invention discloses a graphene-modified resin-based hard carbon material. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve it. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art, and they are all considered to be included in the present invention. The method and application of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.

[0041] In the description of the present invention, it should be noted that the terms "first", "second", etc. are only used for descriptive purposes, and do not indicate or imply relative importance.

[0042] In the description of the present invention, a list of items connected by the term "at least one of" or other similar terms may mean any combination of the listed items. For example, if items A, B are listed, the phrase "at least one of A, B" means only A; only B; or A and B. In another example, if items A, B, C are listed, the phrase "at least one of A, B, C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may include a single element or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements.

[0043] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range or the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0044] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0045] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0046] If there is no special explanation, the "include" and "comprising" mentioned in this application represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0047] Specifically, the present invention adopts the following technical solutions:

[0048] In a first aspect, the present invention provides a graphene-modified resin-based hard carbon material, the graphene-modified resin-based hard carbon material comprising:

[0049] A resin-based hard carbon material having a layered structure;

[0050] The monolayer graphene oxide is connected to the surface of the resin-based hard carbon material through a covalent bond.

[0051] Preferably, the graphene-modified resin-based hard carbon material has a mesoporous structure, and the pore size of the mesoporous structure is 2 to 50 nm. Exemplarily, the pore size of the mesoporous structure is any value among 2 nm, 5 nm, 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, or any value within the range of any two of the above values. The mesoporous structure provides a sodium ion transmission channel, which is beneficial to the migration of sodium ions and can improve the kinetic performance. If the pore size is too small, it is difficult for sodium ions to embed; if the pore size is too large, it will lead to an increase in specific surface area, affecting the first coulomb efficiency.

[0052] Preferably, the pore size of the mesoporous structure is 2 to 20 nm.

[0053] Preferably, the specific surface area of ​​the graphene-modified resin-based hard carbon material is 10 to 20 g / cm 2For example, the specific surface area of ​​the graphene-modified resin-based hard carbon material is 10 g / cm 2 , 11 g / cm 2 , 12 g / cm 2 , 13 g / cm 2 , 14g / cm 2 , 15 g / cm 2 , 16 g / cm 2 , 17 g / cm 2 , 18 g / cm 2 、19 g / cm 2 , 20 g / cm 2 Any value in the range or any value in the range of any two of the above values. Within the above specific surface area range, there are more active sites for sodium ion storage, which is beneficial to the sodium storage capacity. However, if the specific surface area is too large, the initial gram capacity will increase and the initial efficiency will be reduced; if the specific surface area is too small, there will be fewer active sites for sodium ions, which is not conducive to the sodium storage capacity.

[0054] Preferably, the interlayer spacing of the resin-based hard carbon material is 0.40 to 0.42 nm. Exemplarily, the interlayer spacing of the resin-based hard carbon material is any value among 0.40 nm, 0.402 nm, 0.404 nm, 0.406 nm, 0.408 nm, 0.41 nm, 0.412 nm, 0.414 nm, 0.416 nm, 0.418 nm, 0.42 nm, or any value within the range of any two of the above values. Within the above interlayer spacing range, it is beneficial for sodium ions to be deintercalated and diffused, providing a channel for sodium ions to enter the pores, which is beneficial to the improvement of platform area capacity and cycle stability. When the interlayer spacing is less than the above range, the potential barrier is too large, sodium ions are difficult to embed, and it is not conducive to the improvement of rate performance and kinetic performance.

[0055] In an embodiment of the present invention, the covalent bond comprises an N—C bond and / or a C—O bond.

[0056] In an embodiment of the present invention, the N–C bond is generated by a dehydration condensation reaction between a cross-linking agent having an amino group and a carboxyl group of a monolayer of graphene oxide; the C–O bond is generated by an esterification reaction between a cross-linking agent having a carboxyl group and a hydroxyl group of a precursor of a resin-based hard carbon material; and the precursor of the resin-based hard carbon material is a resin prepolymer.

[0057] In an embodiment of the present invention, the cross-linking agent is a cross-linking agent having an amino group and a carboxyl group; preferably, the cross-linking agent is p-aminobenzoic acid.

[0058] In a second aspect, the present invention provides a method for preparing the above-mentioned graphene-improved resin-based hard carbon material, comprising the following steps:

[0059] S1, mixing resin prepolymer, cross-linking agent, monolayer graphene oxide and ethanol uniformly to obtain a mixed solution;

[0060] S2, heating the mixed solution to obtain a cured resin;

[0061] S3, grinding the cured resin into powder, and pre-carbonizing the powder under an inert gas atmosphere to obtain a pre-carbonized product;

[0062] S4, subjecting the pre-carbonized product to high-temperature carbonization treatment under an inert gas atmosphere to obtain a graphene-modified resin-based hard carbon material.

[0063] In an embodiment of the present invention, the resin prepolymer includes at least one of a phenolic resin prepolymer, a urea-formaldehyde resin prepolymer, an epoxy resin prepolymer, a melamine resin prepolymer, and a lignin phenolic resin prepolymer.

[0064] In an embodiment of the present invention, the cross-linking agent is a cross-linking agent having an amino group and a carboxyl group.

[0065] Preferably, the cross-linking agent is p-aminobenzoic acid. As a modifier, a cross-linking agent such as p-aminobenzoic acid (PBPA) uses a chemical reaction between functional groups to complete the cross-linking of resins such as phenolic resin (PF) and the modification of graphene oxide in one step, thereby enhancing the structural stability while improving the overall flexibility and conductivity of the material. Cross-linking agents such as p-aminobenzoic acid not only act as a bridge to connect graphene oxide and resin, but also subsequent carbonization will inhibit the directional growth of the carbon layer, forming a graphite-like domain layered structure with a large interlayer spacing. The carbonized hard carbon material has a large interlayer spacing, good flexibility and outstanding structural stability, and the electrochemical performance shows high sodium storage capacity and excellent rate and cycle stability.

[0066] Preferably, the cross-linking agent having amino and carboxyl groups undergoes a dehydration condensation reaction with the carboxyl groups of the monolayer graphene oxide to generate N-C bonds.

[0067] Preferably, the crosslinking agent having amino and carboxyl groups undergoes an esterification reaction with the hydroxyl group of the resin prepolymer to form a C—O bond.

[0068] Preferably, the mass ratio of the resin prepolymer, the crosslinking agent and the monolayer graphene oxide is (5-10): (1-5): (1-2). Exemplarily, the mass ratio of the resin prepolymer, the crosslinking agent and the monolayer graphene oxide is any value among 7:2:1, 6:2:2 (i.e., 3:1:1), 5:5:1, 10:1:2, 6:3:1, 8:1:1 or any value within the range of values ​​composed of any two of the above values. The mass concentration of the monolayer graphene oxide is too high, the surface functional groups are more, and the crosslinking agent is consumed more, resulting in a slower reaction between the crosslinking agent and the resin prepolymer, a reduced degree of crosslinking, and reduced stability, thereby reducing the reversible capacity of the graphene-modified resin-based hard carbon material and reducing the first coulombic efficiency. Preferably, the mass ratio of the resin prepolymer, the crosslinking agent and the monolayer graphene oxide is (6-7): 2: (1-2).

[0069] Preferably, the concentration of the mixed solution is 0.05 to 1 g / mL. Exemplarily, the concentration of the mixed solution is any value in 0.05 g / mL, 0.1 g / mL, 0.2 g / mL, 0.3 g / mL, 0.4 g / mL, 0.5 g / mL, 0.6 g / mL, 0.7 g / mL, 0.8 g / mL, 0.9 g / mL, 1 g / mL or any value in the range of any two of the above values. If the concentration of the mixed solution is too high, the ethanol solvent is reduced, the solvent evaporates too quickly, and the reaction is not sufficient, resulting in the connection between the crosslinker and the monolayer graphene oxide and the incomplete crosslinking and curing of the resin prepolymer, which causes the electrochemical performance to be manifested as a decrease in capacity and a decrease in the first coulombic efficiency.

[0070] Preferably, the temperature of the heating treatment is 120-180°C, and the time of the heating treatment is 1-10h. Exemplarily, the temperature of the heating treatment is any value among 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, or any value within the range of any two of the above values, and the time of the heating treatment is any value among 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, or any value within the range of any two of the above values. During the heating treatment, the resin prepolymer, the crosslinking agent, and the monolayer graphene oxide undergo a crosslinking reaction, and at the same time, ethanol forms pores in the crosslinked product. As a solvent and a pore-forming agent, ethanol can form a large number of pore structures in the crosslinked product while accelerating the reaction by heating and evaporation. The heating treatment temperature is too high and the reaction is violent, resulting in a too fast cross-linking reaction, which is not conducive to the modification of the single-layer graphene oxide, resulting in insufficient connection between the graphene oxide sheet and the resin prepolymer, which is not conducive to the subsequent compaction and rate performance of the hard carbon.

[0071] In an embodiment of the present invention, the heating method of the heat treatment includes a water bath, an oil bath or a microwave.

[0072] In the embodiment of the present invention, the device used for grinding into powder is a small pulverizer and / or a vibration mill.

[0073] Preferably, the temperature of the pre-carbonization treatment is 300-800°C, and the time of the pre-carbonization treatment is 5-15h. Exemplarily, the temperature of the pre-carbonization treatment is any value in 300°C, 400°C, 500°C, 600°C, 700°C, 800°C or any value in the range of any two of the above values, and the time of the pre-carbonization treatment is any value in 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h or any value in the range of any two of the above values. The pre-carbonization treatment helps to eliminate some impurities and increase the order of the microstructure of the material. The surface becomes rougher in morphology, which brings higher reversible specific capacity and better rate performance. Adding the pre-carbonization treatment step is equivalent to increasing the transition process before high-temperature carbonization, which is beneficial to increase the cross-linking density of the polymer chain segment in the phenolic resin. If the pre-carbonization treatment time is too long, the morphology of the activated carbon will be basically stable, resulting in little effect of subsequent high-temperature carbonization on its morphology. The already formed pore structure will not shrink, resulting in a low initial efficiency.

[0074] In an embodiment of the present invention, the heating rate of the pre-carbonization treatment is 0.5-2°C / min. Exemplarily, the heating rate of the pre-carbonization treatment is any value among 0.5°C / min, 1°C / min, 1.5°C / min, 2°C / min, or any value within the range of any two of the above values.

[0075] Preferably, the temperature of the high-temperature carbonization treatment is 1200-1800°C, and the time of the high-temperature carbonization treatment is 1-5 hours. Exemplarily, the temperature of the high-temperature carbonization treatment is any value among 1200°C, 1300°C, 1400°C, 1500°C, 1600°C, 1700°C, 1800°C, or any value within the range of any two of the above values, and the time of the high-temperature carbonization treatment is any value among 1h, 2h, 3h, 4h, 5h, or any value within the range of any two of the above values. During the high-temperature carbonization treatment, the cross-linked structure after the pre-carbonization treatment will be maintained or the degree of cross-linking will continue to be enhanced, which is beneficial to improving the structural stability of the resin-based hard carbon material, and in the electrochemical characterization, it shows better cycle stability.

[0076] In an embodiment of the present invention, the heating rate of the high temperature carbonization treatment is 0.5 to 5°C / min. Exemplarily, the heating rate of the high temperature carbonization treatment is any value among 0.5°C / min, 1°C / min, 1.5°C / min, 2°C / min, 2.5°C / min, 3°C / min, 3.5°C / min, 4°C / min, 4.5°C / min, 5°C / min, or any value within the range of any two of the above values.

[0077] In an embodiment of the present invention, the inert gas in step S3 or S4 is any one or more inert gases such as nitrogen or argon, and its flow rate can be 50-100 mL / min. Exemplarily, the flow rate of the inert gas is any value among 50 mL / min, 60 mL / min, 70 mL / min, 80 mL / min, 90 mL / min, 100 mL / min, or any value within the range of any two of the above values.

[0078] In an embodiment of the present invention, the heating reactor for the pre-carbonization treatment in step S3 or the high-temperature carbonization treatment in step S4 includes a tubular furnace, an atmosphere box furnace, and the like.

[0079] In a third aspect, the present invention provides a negative electrode sheet, which includes the above-mentioned graphene-modified resin-based hard carbon material, or the graphene-modified resin-based hard carbon material prepared by the above-mentioned preparation method.

[0080] In an embodiment of the present invention, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on at least one side surface of the negative electrode current collector.

[0081] In an embodiment of the present invention, the negative electrode active material layer includes a negative electrode active material, and the negative electrode active material includes the above-mentioned graphene-modified resin-based hard carbon material.

[0082] In an embodiment of the present invention, the negative electrode active material layer further includes at least one of a conductive agent and a binder. The present application does not particularly limit the types of conductive agents and binders in the negative electrode active material layer, as long as the purpose of the present application can be achieved. As an example, the conductive agent in the negative electrode active material layer can be selected from at least one of carbon black, SuperP (SP), acetylene black, Ketjen black, carbon nanotubes, graphene, and carbon nanofibers. As an example, the binder in the negative electrode active material layer can be selected from at least one of carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), polymethacrylic acid (PMAA), carboxymethyl chitosan (CMCS), and sodium alginate (SA).

[0083] The present application has no particular restrictions on the mass ratio of the negative electrode active material, the conductive agent and the binder in the negative electrode active material layer, as long as the purpose of the present application can be achieved. For example, the mass percentage of each component in the negative electrode active material layer is: 70% to 98% of the negative electrode active material, 1% to 15% of the conductive agent, and 1% to 15% of the binder.

[0084] The present application has no particular restrictions on the preparation method of the negative electrode sheet, as long as the purpose of the present application can be achieved. Exemplarily, the preparation method of the negative electrode sheet includes: mixing the negative electrode active material, the conductive agent, the binder and the solvent to obtain the negative electrode slurry; coating the negative electrode slurry on the negative electrode current collector, drying, cold pressing and cutting to obtain the negative electrode sheet.

[0085] In a fourth aspect, the present invention provides a sodium ion battery, which comprises the negative electrode sheet of the present invention.

[0086] In the embodiment of the present invention, the battery structure includes but is not limited to button batteries, soft-pack batteries, cylindrical batteries, etc.

[0087] The present application has no particular restrictions on the positive electrode sheet, separator, and electrolyte in the battery, and those skilled in the art can select them according to actual needs as long as the purpose of the present application can be achieved.

[0088] The reagents, instruments or materials used in the present invention can be obtained through commercial channels.

[0089] The present invention will be further described below in conjunction with embodiments:

[0090] Example 1

[0091] This embodiment provides a method for preparing an organic in-situ modified phenolic resin-based hard carbon material, which can be used as a negative electrode material for sodium ion batteries. The preparation scheme is as follows:

[0092] (1) Mix 7 g of phenolic resin prepolymer, 2 g of p-aminobenzoic acid (PBPA), and 1 g of single-layer graphene oxide in a mass ratio of 7:2:1 and stir evenly;

[0093] (2) Add the above mixture to 200 mL of ethanol to prepare a mixed solution with a mass concentration of 0.05 g / mL, and heat it at 140 °C for 5 h for cross-linking and pore formation;

[0094] (3) The cured phenolic resin is taken out, ground into powder, heated to 500°C in an argon atmosphere, and subjected to low-temperature pre-carbonization pyrolysis treatment for 10 h;

[0095] (4) After cooling, the material obtained in the above step is further heated to 1400°C in an argon atmosphere and subjected to high-temperature carbonization treatment for 2 h to obtain a PBPA-modified phenolic resin-based hard carbon material (PBPA-HC).

[0096] like Figure 1 SEM and Figure 2 As shown in the pore size distribution diagram, the modified hard carbon material has a loose porous structure with a large number of mesopores (2–50 nm).

[0097] Depend on Figure 3 From the transmission electron microscope image, we can see that the thin edge area shows the ordered layered structure of graphene, and the internal area shows the disordered layered structure of resin-based hard carbon material.

[0098] Example 2a

[0099] Compared with Example 1, the only difference in this example is that the amount and mass ratio of the phenolic resin prepolymer, p-aminobenzoic acid and monolayer graphene oxide are adjusted.

[0100] This embodiment provides a method for preparing an organic in-situ modified phenolic resin-based hard carbon material, which can be used as a negative electrode material for sodium ion batteries. The preparation scheme is as follows:

[0101] (1) 6 g of phenolic resin prepolymer, 2 g of p-aminobenzoic acid (PBPA), and 2 g of single-layer graphene oxide were mixed in a mass ratio of 3:1:1 and stirred evenly;

[0102] (2) Add the above mixture to 200 mL of ethanol to prepare a mixed solution with a mass concentration of 0.05 g / mL, and heat it at 140 °C for 5 h for cross-linking and pore formation;

[0103] (3) The cured phenolic resin is taken out, ground into powder, heated to 500°C in an argon atmosphere, and subjected to low-temperature pre-carbonization pyrolysis treatment for 10 h;

[0104] (4) After cooling, the material obtained in the above step is further heated to 1400°C in an argon atmosphere and subjected to high-temperature carbonization treatment for 2 h to obtain a PBPA-modified phenolic resin-based hard carbon material (PBPA-HC).

[0105] Example 2b

[0106] Compared with Example 1, the only difference in this example is that the amount and mass ratio of the phenolic resin prepolymer, p-aminobenzoic acid and monolayer graphene oxide are adjusted.

[0107] This embodiment provides a method for preparing an organic in-situ modified phenolic resin-based hard carbon material, which can be used as a negative electrode material for sodium ion batteries. The preparation scheme is as follows:

[0108] (1) Mix 5 g of phenolic resin prepolymer, 5 g of p-aminobenzoic acid (PBPA), and 1 g of single-layer graphene oxide in a mass ratio of 5:5:1 and stir evenly;

[0109] (2) 10 g of the above mixture was added to 200 mL of ethanol to prepare a mixed solution with a mass concentration of 0.05 g / mL, and heated at 140 °C for 5 h for cross-linking and pore formation;

[0110] (3) The cured phenolic resin is taken out, ground into powder, heated to 500°C in an argon atmosphere, and subjected to low-temperature pre-carbonization pyrolysis treatment for 10 h;

[0111] (4) After cooling, the material obtained in the above step is further heated to 1400°C in an argon atmosphere and subjected to high-temperature carbonization treatment for 2 h to obtain a PBPA-modified phenolic resin-based hard carbon material (PBPA-HC).

[0112] Example 2c

[0113] Compared with Example 1, the only difference in this example is that the amount and mass ratio of the phenolic resin prepolymer, p-aminobenzoic acid and monolayer graphene oxide are adjusted.

[0114] This embodiment provides a method for preparing an organic in-situ modified phenolic resin-based hard carbon material, which can be used as a negative electrode material for sodium ion batteries. The preparation scheme is as follows:

[0115] (1) Mix 10 g of phenolic resin prepolymer, 1 g of p-aminobenzoic acid (PBPA), and 2 g of single-layer graphene oxide in a mass ratio of 10:1:2 and stir evenly;

[0116] (2) 10 g of the above mixture was added to 200 mL of ethanol to prepare a mixed solution with a mass concentration of 0.05 g / mL, and heated at 140 °C for 5 h for cross-linking and pore formation;

[0117] (3) The cured phenolic resin is taken out, ground into powder, heated to 500°C in an argon atmosphere, and subjected to low-temperature pre-carbonization pyrolysis treatment for 10 h;

[0118] (4) After cooling, the material obtained in the above step is further heated to 1400°C in an argon atmosphere and subjected to high-temperature carbonization treatment for 2 h to obtain a PBPA-modified phenolic resin-based hard carbon material (PBPA-HC).

[0119] Example 3a

[0120] Compared with Example 1, the only difference in this example is that the amount of ethanol and the concentration of the mixed solution are adjusted.

[0121] This embodiment provides a method for preparing an organic in-situ modified phenolic resin-based hard carbon material, which can be used as a negative electrode material for sodium ion batteries. The preparation scheme is as follows:

[0122] (1) Mix 7 g of phenolic resin prepolymer, 2 g of p-aminobenzoic acid (PBPA), and 1 g of single-layer graphene oxide in a mass ratio of 7:2:1 and stir evenly;

[0123] (2) Add the above mixture to 100 mL of ethanol to prepare a mixed solution with a mass concentration of 0.1 g / mL, and heat it at 140 °C for 5 h for cross-linking and pore formation;

[0124] (3) The cured phenolic resin is taken out, ground into powder, heated to 500°C in an argon atmosphere, and subjected to low-temperature pre-carbonization pyrolysis treatment for 10 h;

[0125] (4) After cooling, the material obtained in the above step is further heated to 1400°C in an argon atmosphere and subjected to high-temperature carbonization treatment for 2 h to obtain a PBPA-modified phenolic resin-based hard carbon material (PBPA-HC).

[0126] Example 3b

[0127] Compared with Example 1, the only difference in this example is that the amount of ethanol and the concentration of the mixed solution are adjusted.

[0128] This embodiment provides a method for preparing an organic in-situ modified phenolic resin-based hard carbon material, which can be used as a negative electrode material for sodium ion batteries. The preparation scheme is as follows:

[0129] (1) Mix 7 g of phenolic resin prepolymer, 2 g of p-aminobenzoic acid (PBPA), and 1 g of single-layer graphene oxide in a mass ratio of 7:2:1 and stir evenly;

[0130] (2) Add the above mixture to 10 mL of ethanol to prepare a mixed solution with a mass concentration of 1 g / mL, and heat it at 140 °C for 5 h for cross-linking and pore formation;

[0131] (3) The cured phenolic resin is taken out, ground into powder, heated to 500°C in an argon atmosphere, and subjected to low-temperature pre-carbonization pyrolysis treatment for 10 h;

[0132] (4) After cooling, the material obtained in the above step is further heated to 1400°C in an argon atmosphere and subjected to high-temperature carbonization treatment for 2 h to obtain a PBPA-modified phenolic resin-based hard carbon material (PBPA-HC).

[0133] Example 4a

[0134] Compared with Example 1, the only difference in this example is that the heating temperature in step (2) is adjusted.

[0135] This embodiment provides a method for preparing an organic in-situ modified phenolic resin-based hard carbon material, which can be used as a negative electrode material for sodium ion batteries. The preparation scheme is as follows:

[0136] (1) Mix 7 g of phenolic resin prepolymer, 2 g of p-aminobenzoic acid (PBPA), and 1 g of single-layer graphene oxide in a mass ratio of 7:2:1 and stir evenly;

[0137] (2) Add the above mixture to 200 mL of ethanol to prepare a mixed solution with a mass concentration of 0.05 g / mL, and heat it at 180°C for 1 h for cross-linking and pore formation;

[0138] (3) The cured phenolic resin is taken out, ground into powder, heated to 500°C in an argon atmosphere, and subjected to low-temperature pre-carbonization pyrolysis treatment for 10 h;

[0139] (4) After cooling, the material obtained in the above step is further heated to 1400°C in an argon atmosphere and subjected to high-temperature carbonization treatment for 2 h to obtain a PBPA-modified phenolic resin-based hard carbon material (PBPA-HC).

[0140] Example 4b

[0141] Compared with Example 1, the only difference in this example is that the heating temperature and time in step (2) are adjusted.

[0142] This embodiment provides a method for preparing an organic in-situ modified phenolic resin-based hard carbon material, which can be used as a negative electrode material for sodium ion batteries. The preparation scheme is as follows:

[0143] (1) Mix 7 g of phenolic resin prepolymer, 2 g of p-aminobenzoic acid (PBPA), and 1 g of single-layer graphene oxide in a mass ratio of 7:2:1 and stir evenly;

[0144] (2) Add the above mixture to 200 mL of ethanol to prepare a mixed solution with a mass concentration of 0.05 g / mL, and heat it at 120 °C for 10 h for cross-linking and pore formation;

[0145] (3) The cured phenolic resin is taken out, ground into powder, heated to 500°C in an argon atmosphere, and subjected to low-temperature pre-carbonization pyrolysis treatment for 10 h;

[0146] (4) After cooling, the material obtained in the above step is further heated to 1400°C in an argon atmosphere and subjected to high-temperature carbonization treatment for 2 h to obtain a PBPA-modified phenolic resin-based hard carbon material (PBPA-HC).

[0147] Example 5a

[0148] Compared with Example 1, the only difference in this example is that the temperature and time of the pre-carbonization pyrolysis treatment in step (3) are adjusted.

[0149] This embodiment provides a method for preparing an organic in-situ modified phenolic resin-based hard carbon material, which can be used as a negative electrode material for sodium ion batteries. The preparation scheme is as follows:

[0150] (1) Mix 7 g of phenolic resin prepolymer, 2 g of p-aminobenzoic acid (PBPA), and 1 g of single-layer graphene oxide in a mass ratio of 7:2:1 and stir evenly;

[0151] (2) Add the above mixture to 200 mL of ethanol to prepare a mixed solution with a mass concentration of 0.05 g / mL, and heat it at 140 °C for 5 h for cross-linking and pore formation;

[0152] (3) The cured phenolic resin was taken out, ground into powder, heated to 700 °C in an argon atmosphere, and subjected to low-temperature pre-carbonization pyrolysis treatment for 15 h;

[0153] (4) After cooling, the material obtained in the above step is further heated to 1400°C in an argon atmosphere and subjected to high-temperature carbonization treatment for 2 h to obtain a PBPA-modified phenolic resin-based hard carbon material (PBPA-HC).

[0154] Example 5b

[0155] Compared with Example 1, the only difference in this example is that the temperature and time of the pre-carbonization pyrolysis treatment in step (3) are adjusted.

[0156] This embodiment provides a method for preparing an organic in-situ modified phenolic resin-based hard carbon material, which can be used as a negative electrode material for sodium ion batteries. The preparation scheme is as follows:

[0157] (1) Mix 7 g of phenolic resin prepolymer, 2 g of p-aminobenzoic acid (PBPA), and 1 g of single-layer graphene oxide in a mass ratio of 7:2:1 and stir evenly;

[0158] (2) Add the above mixture to 200 mL of ethanol to prepare a mixed solution with a mass concentration of 0.05 g / mL, and heat it at 140 °C for 5 h for cross-linking and pore formation;

[0159] (3) The cured phenolic resin is taken out, ground into powder, heated to 300°C in an argon atmosphere, and subjected to low-temperature pre-carbonization pyrolysis treatment for 15 h;

[0160] (4) After cooling, the material obtained in the above step is further heated to 1400°C in an argon atmosphere and subjected to high-temperature carbonization treatment for 2 h to obtain a PBPA-modified phenolic resin-based hard carbon material (PBPA-HC).

[0161] Example 5c

[0162] Compared with Example 1, the only difference in this example is that the temperature and time of the pre-carbonization pyrolysis treatment in step (3) are adjusted.

[0163] This embodiment provides a method for preparing an organic in-situ modified phenolic resin-based hard carbon material, which can be used as a negative electrode material for sodium ion batteries. The preparation scheme is as follows:

[0164] (1) Mix 7 g of phenolic resin prepolymer, 2 g of p-aminobenzoic acid (PBPA), and 1 g of single-layer graphene oxide in a mass ratio of 7:2:1 and stir evenly;

[0165] (2) Add the above mixture to 200 mL of ethanol to prepare a mixed solution with a mass concentration of 0.05 g / mL, and heat it at 140 °C for 5 h for cross-linking and pore formation;

[0166] (3) The cured phenolic resin is taken out, ground into powder, heated to 800°C in an argon atmosphere, and subjected to low-temperature pre-carbonization pyrolysis treatment for 5 hours;

[0167] (4) After cooling, the material obtained in the above step is further heated to 1400°C in an argon atmosphere and subjected to high-temperature carbonization treatment for 2 h to obtain a PBPA-modified phenolic resin-based hard carbon material (PBPA-HC).

[0168] Example 6a

[0169] Compared with Example 1, the only difference in this example is that the temperature and time of the high-temperature carbonization treatment in step (4) are adjusted.

[0170] This embodiment provides a method for preparing an organic in-situ modified phenolic resin-based hard carbon material, which can be used as a negative electrode material for sodium ion batteries. The preparation scheme is as follows:

[0171] (1) Mix 7 g of phenolic resin prepolymer, 2 g of p-aminobenzoic acid (PBPA), and 1 g of single-layer graphene oxide in a mass ratio of 7:2:1 and stir evenly;

[0172] (2) Add the above mixture to 200 mL of ethanol to prepare a mixed solution with a mass concentration of 0.05 g / mL, and heat it at 140 °C for 5 h for cross-linking and pore formation;

[0173] (3) The cured phenolic resin is taken out, ground into powder, heated to 500°C in an argon atmosphere, and subjected to low-temperature pre-carbonization pyrolysis treatment for 10 h;

[0174] (4) After cooling, the material obtained in the above step is further heated to 1200°C in an argon atmosphere and subjected to high-temperature carbonization treatment for 5 h to obtain a PBPA-modified phenolic resin-based hard carbon material (PBPA-HC).

[0175] Example 6b

[0176] Compared with Example 1, the only difference in this example is that the temperature and time of the high-temperature carbonization treatment in step (4) are adjusted.

[0177] This embodiment provides a method for preparing an organic in-situ modified phenolic resin-based hard carbon material, which can be used as a negative electrode material for sodium ion batteries. The preparation scheme is as follows:

[0178] (1) Mix 7 g of phenolic resin prepolymer, 2 g of p-aminobenzoic acid (PBPA), and 1 g of single-layer graphene oxide in a mass ratio of 7:2:1 and stir evenly;

[0179] (2) Add the above mixture to 200 mL of ethanol to prepare a mixed solution with a mass concentration of 0.05 g / mL, and heat it at 140 °C for 5 h for cross-linking and pore formation;

[0180] (3) The cured phenolic resin is taken out, ground into powder, heated to 500°C in an argon atmosphere, and subjected to low-temperature pre-carbonization pyrolysis treatment for 10 h;

[0181] (4) After cooling, the material obtained in the above step is further heated to 1800°C in an argon atmosphere and subjected to high-temperature carbonization treatment for 1 h to obtain a PBPA-modified phenolic resin-based hard carbon material (PBPA-HC).

[0182] Comparative Example 1

[0183] Compared with Example 1, the difference in this comparative example is that p-aminobenzoic acid (PBPA) is not added in step (1), and the amount and mass ratio of the phenolic resin prepolymer and the monolayer graphene oxide are adjusted accordingly.

[0184] This comparative example provides a method for preparing a graphene oxide modified phenolic resin-based hard carbon material, which can be used as a negative electrode material for sodium ion batteries. The preparation scheme is as follows:

[0185] (1) 8 g of phenolic resin prepolymer and 2 g of single-layer graphene oxide were mixed in a mass ratio of 8:2 and stirred evenly;

[0186] (2) Add the above mixture to 200 mL of ethanol to prepare a mixed solution with a mass concentration of 0.05 g / mL, and heat it at 140 °C for 5 h for cross-linking and pore formation;

[0187] (3) The cured phenolic resin is taken out, ground into powder, heated to 500°C in an argon atmosphere, and subjected to low-temperature pre-carbonization pyrolysis treatment for 10 h;

[0188] (4) After cooling, the material obtained in the above step is further heated to 1400°C in an argon atmosphere and subjected to high-temperature carbonization treatment for 2 hours to obtain a phenolic resin-based hard carbon material modified with graphene oxide.

[0189] Comparative Example 2

[0190] Compared with Example 1, the difference in this comparative example is that in step (2), the pore-forming agent ethanol is replaced by deionized water.

[0191] This comparative example provides a method for preparing an organic in-situ modified phenolic resin-based hard carbon material, which can be used as a negative electrode material for sodium ion batteries. The preparation scheme is as follows:

[0192] (1) Mix 7 g of phenolic resin prepolymer, 2 g of p-aminobenzoic acid (PBPA), and 1 g of single-layer graphene oxide in a mass ratio of 7:2:1 and stir evenly;

[0193] (2) adding the above mixture into 200 mL of deionized water to prepare a mixed solution with a mass concentration of 0.05 g / mL, and heating at 140 °C for 5 h for cross-linking;

[0194] (3) The cured phenolic resin is taken out, ground into powder, heated to 500°C in an argon atmosphere, and subjected to low-temperature pre-carbonization pyrolysis treatment for 10 h;

[0195] (4) After cooling, the material obtained in the above step is further heated to 1400°C in an argon atmosphere and subjected to high-temperature carbonization treatment for 2 hours to obtain a PBPA-modified phenolic resin-based hard carbon material.

[0196] Performance Test 1

[0197] Specific surface area test: The specific surface area test was performed on the carbon materials in the above embodiments and comparative examples. The specific test method is: nitrogen molecules form a certain amount of adsorption layer on the solid surface under specific conditions (such as low temperature), and the pore structure and specific surface area of ​​the material can be characterized by measuring the changes in physical parameters caused by the adsorption and desorption of nitrogen by the solid material.

[0198] Interlayer spacing test: X-ray diffraction is an optical analysis method that is detected by an instrument. Monochromatic X-rays are irradiated onto a powder crystal sample. If the diffraction conditions are met, diffraction occurs at a diffraction angle of 2θ. If there are multiple grains in the sample and the diffraction conditions are met, the corresponding diffraction pattern is obtained. The XRD test of interlayer spacing involves the Bragg equation, that is, nλ=2dsinθ, where λ is the wavelength of the incident ray, d is the interplane spacing, θ is the diffraction angle, and n is the diffraction order.

[0199] The powder compaction density instrument of Yuanneng Technology was used to test the powder compaction of the hard carbon materials of Examples 1-6 and Comparative Examples 1-2.

[0200] The hard carbon material of the embodiment and the comparative example was used to prepare the negative electrode sheet. The hard carbon material, conductive carbon black (SP), carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR) were evenly mixed at a mass ratio of 95:1:1.5:2.5, and the mixture was applied on a copper foil. The coated electrode sheet was placed in a vacuum drying oven at 80°C and dried for 12 hours.

[0201] Take several steel needles with increasing diameters (0.5-5mm), use them as the center body, and wind the negative electrode sheet along them to observe whether the negative electrode material layer on the negative electrode sheet cracks or falls off, and record the steel needle diameter value when the negative electrode material layer does not crack or fall off. The smaller the steel needle diameter value, the better the flexibility of the negative electrode sheet.

[0202] The results are shown in Table 1.

[0203] Table 1

[0204]

[0205] Compared with Example 1, Comparative Example 1 removes the modified cross-linking effect of para-aminobenzoic acid PBPA. Although the single-layer graphene oxide can also undergo esterification reaction with the phenolic resin prepolymer, due to the absence of the PBPA cross-linking agent, the degree of cross-linking of the phenolic resin is reduced, and the structural stability is reduced, which manifests as lower electrode flexibility.

[0206] Compared with Example 1, although Comparative Example 2 was modified with para-aminobenzoic acid PBPA, due to the absence of ethanol as a pore-forming agent, the porosity of the hard carbon material was lower, and the pole piece flexibility was also lower.

[0207] Performance Test 2

[0208] The hard carbon materials of Examples 1-6 and Comparative Examples 1-2 were used to prepare negative electrode sheets. The hard carbon material, conductive carbon black (SP), carboxymethyl cellulose (CMC), and styrene-butadiene rubber (SBR) were mixed evenly at a mass ratio of 95:1:1.5:2.5, and applied on copper foil. The coated electrode sheet was placed in a vacuum drying oven at 80°C and dried for 12 hours. CR2032 button cells were assembled in an argon-protected glove box. The electrolyte was 1 mol NaPF6-EC / DEC (volume ratio 1:1) + 5% FEC. The negative electrode sheet prepared above was used as the negative electrode, and the metal sodium sheet was used as the counter electrode. Using the Land battery test system, at a constant temperature of 25°C, discharge at a rate of 0.05C to 0.01V, and discharge at a constant current of 20μA to 0V, and record the rate discharge capacity + constant current discharge capacity = first discharge capacity at this time; continue to charge from 0V to 2V at a rate of 0.1C, and record the charging capacity at this time as the first charging capacity; first coulomb efficiency = first charging capacity / first discharge capacity × 100%.

[0209] The test results are shown in Table 2.

[0210] Table 2

[0211]

[0212] Performance Test 3

[0213] The button cell prepared above was subjected to constant current charge and discharge test at a current density of 250mA / g, a voltage range of 0~2V, and 500 cycles to test the reversible specific capacity and capacity retention rate. The specific test method is: using the Land battery test system, at a constant temperature of 25°C, 250mA / g current density constant current discharge to 0V, and then 250mA / g constant current charge to 2V, which is a complete charge and discharge cycle, recorded as cycle 1, and this process is repeated until the number of cycles is equal to 500, and the test is terminated. The discharge capacity of the 500th cycle is the reversible specific capacity, and the discharge specific capacity of the 500th cycle / the discharge specific capacity of the first cycle = the capacity retention rate.

[0214] See Table 3 for specific values.

[0215] Table 3

[0216]

[0217] The button-type half-cells of organic modified resin-derived carbon prepared in Examples 1 to 6 all have good cycle retention rates (~90%), showing excellent cycle stability, while the capacity retention rate of the comparative example is only about 70% to 80%.

[0218] Compared with Example 1, Comparative Example 1 removes the modified cross-linking effect of p-aminobenzoic acid PBPA, the structural stability is reduced, and the flexibility of the pole piece is low, resulting in lower reversible specific capacity and capacity retention rate.

[0219] Compared with Example 1, Comparative Example 2 does not have ethanol as a pore-forming agent, resulting in the overall structure of the material being not loose and porous enough, which is not conducive to the storage and migration of sodium ions, resulting in lower reversible specific capacity and capacity retention rate.

[0220] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A graphene-modified resin-based hard carbon material, characterized in that: The graphene-modified resin-based hard carbon material comprises: A resin-based hard carbon material having a layered structure; A single layer of graphene oxide, wherein the single layer of graphene oxide is connected to the surface of the resin-based hard carbon material via covalent bonds, wherein the covalent bonds include N-C bonds and C-O bonds; The preparation method of the graphene-improved resin-based hard carbon material comprises the following steps: S1, mixing a resin prepolymer, a cross-linking agent, a single-layer graphene oxide, and ethanol to obtain a mixed solution; S2, heating the mixed solution to obtain a cured resin; S3, grinding the solidified resin into powder, and pre-carbonizing the powder under an inert gas atmosphere to obtain a pre-carbonized product; S4, subjecting the pre-carbonized product to a high-temperature carbonization treatment under an inert gas atmosphere to obtain the graphene-modified resin-based hard carbon material; The cross-linking agent is a cross-linking agent having an amino group and a carboxyl group; The cross-linking agent having amino and carboxyl groups undergoes a dehydration condensation reaction with the carboxyl groups of the monolayer graphene oxide to form N–C bonds; The cross-linking agent having amino and carboxyl groups undergoes an esterification reaction with the hydroxyl group of the resin prepolymer to generate a C-O bond.

2. The graphene-modified resin-based hard carbon material according to claim 1, wherein: The graphene-modified resin-based hard carbon material has a mesoporous structure, and the pore size of the mesoporous structure is 2 to 50 nm; The specific surface area of ​​the graphene-modified resin-based hard carbon material is 10 to 20 g / cm 2 .

3. The graphene-modified resin-based hard carbon material according to claim 1, wherein: The interlayer spacing of the resin-based hard carbon material is 0.40-0.42 nm.

4. The method for preparing the graphene-modified resin-based hard carbon material according to any one of claims 1 to 3, characterized in that: The steps include: S1, mixing a resin prepolymer, a cross-linking agent, a single-layer graphene oxide, and ethanol to obtain a mixed solution; S2, heating the mixed solution to obtain a cured resin; S3, grinding the solidified resin into powder, and pre-carbonizing the powder under an inert gas atmosphere to obtain a pre-carbonized product; S4, subjecting the pre-carbonized product to a high-temperature carbonization treatment under an inert gas atmosphere to obtain the graphene-modified resin-based hard carbon material; The cross-linking agent is a cross-linking agent having an amino group and a carboxyl group; The cross-linking agent having amino and carboxyl groups undergoes a dehydration condensation reaction with the carboxyl groups of the monolayer graphene oxide to form N–C bonds; The cross-linking agent having amino and carboxyl groups undergoes an esterification reaction with the hydroxyl group of the resin prepolymer to generate a C-O bond.

5. The preparation method according to claim 4, characterized in that The resin prepolymer includes at least one of phenolic resin prepolymer, urea-formaldehyde resin prepolymer, epoxy resin prepolymer, melamine resin prepolymer, and lignin phenolic resin prepolymer.

6. The preparation method according to claim 4, characterized in that The mass ratio of the resin prepolymer, the cross-linking agent and the single-layer graphene oxide is (5-10): (1-5): (1-2); The concentration of the mixed solution is 0.05-1 g / mL.

7. The preparation method according to claim 4, characterized in that The temperature of the heating treatment is 120-180° C., and the time of the heating treatment is 1-10 hours; The temperature of the pre-carbonization treatment is 300-800°C, and the time of the pre-carbonization treatment is 5-15 hours; The temperature of the high-temperature carbonization treatment is 1200-1800° C., and the time of the high-temperature carbonization treatment is 1-5 hours.

8. A negative electrode sheet, characterized in that: The negative electrode sheet comprises the graphene-modified resin-based hard carbon material according to any one of claims 1 to 3, or the graphene-modified resin-based hard carbon material prepared by the preparation method according to any one of claims 4 to 7.

9. A sodium ion battery, characterized in that: The sodium ion battery comprises the negative electrode sheet according to claim 8.

Citation Information

Patent Citations

  • Ultramicroporous fluorine-doped hard carbon negative electrode material and preparation method thereof

    CN116040606A

  • Composite negative electrode material, preparation method thereof and sodium ion battery

    CN117727901A