A sulfonated mesoporous silica in-situ modified anode catalyst layer and its preparation method and application

By using sulfonated mesoporous silica in situ modification technology in the positive electrode catalyst layer of hydrogen fuel cell, the copolymerization segment network structure is formed, which solves the problem of insufficient mechanical strength and durability of the catalyst layer, and achieves efficient protons and Reaction gas transmittance and heat resistance.

CN118693294BActive Publication Date: 2024-11-08THINKRE MEMBRANE MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411160717.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-08
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

The mechanical strength and durability of the positive electrode catalyst layer in hydrogen fuel cells are insufficient, resulting in cracking and a decrease in the transmittance of protons and reaction gases, affecting the efficiency and reliability of the overall fuel cell.

Method used

Using an anode catalyst layer modified in situ by adding platinum carbon catalyst, ionomer, solvent, sulfonated mesoporous silica, methylhydrodichlorosilane and olefins to the catalyst slurry Propylsulfonic acid is subjected to staged heat treatment to form a copolymerized segment network structure, improving the compatibility and mechanical strength of the catalyst layer, while maintaining proton conductivity and oxygen permeability.

Benefits of technology

The mechanical strength and durability of the catalyst layer are significantly improved, cracking is avoided, and high proton and reactive gas transmittance is maintained, which improves the heat resistance and durability of the hydrogen fuel cell.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure ODHC2M4DPGHWFWPEEJ262D4LOUX8VGDLXQO0CVC4
    Figure ODHC2M4DPGHWFWPEEJ262D4LOUX8VGDLXQO0CVC4
Patent Text Reader

Abstract

The present invention discloses an anode catalyst layer of sulfonated mesoporous silica in situ modified, and a preparation method and application thereof. The anode catalyst layer comprises a platinum carbon catalyst, an ionomer, a solvent, sulfonated mesoporous silica, methyl hydrogen dichlorosilane, vinyl triethoxysilane and allyl sulfonic acid. The preparation method comprises the following steps: (1) grinding and mixing the raw materials comprising the platinum carbon catalyst, the ionomer, the solvent, the sulfonated mesoporous silica, methyl hydrogen dichlorosilane, vinyl triethoxysilane and allyl sulfonic acid in a grinding mixer to obtain a catalyst slurry; (2) coating the catalyst slurry on a base film PET or a proton exchange membrane, heat treating in stages, vacuum drying, and cooling to room temperature to obtain an anode catalyst layer of sulfonated mesoporous silica in situ modified.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of hydrogen fuel cells, and in particular to an anode catalyst layer of sulfonated mesoporous silica in-situ modified, and a preparation method and application thereof. Background Art

[0002] The most important part of a hydrogen fuel cell is the catalyst. The catalytic efficiency of the catalyst directly determines the power of the entire fuel cell; at the same time, the amount of platinum (Pt) in the catalyst also plays an important role in the cost of the entire fuel cell. In fact, the distribution of Pt in the fuel cell is uneven (8 / 9 of the Pt / C catalyst is distributed at the positive electrode of the fuel cell). This is because in a hydrogen fuel cell, the HOR reaction H2→2e - +2H + (Two electron transfer, fast kinetic process), ORR reaction O2+4e occurs at the positive electrode - +4H + →2H2O (four electron transfer, slow kinetics). According to theoretical calculations and comparison of the two reaction kinetics, the ORR reaction rate at the positive electrode is 6 orders of magnitude lower than the HOR reaction at the negative electrode, so the reaction rate of the overall reaction depends on the positive electrode. The chemical reaction rate is proportional to the amount of Pt catalyst used, so the amount of catalyst used at the positive electrode is about 8 times that of the negative electrode.

[0003] The catalyst Pt / C is made of ionomers adhered between the proton exchange membrane (PEM) and the gas diffusion layer (GDL). The surface of the catalyst Pt is wrapped by the ionomer, and oxygen must first permeate through the ionomer before it can contact the catalyst Pt, thereby triggering the ORR reaction. The catalyst layer is the place where the electrochemical reaction occurs inside the fuel cell, where protons and electrons are transferred, as well as the reaction gas and product water gas-liquid two-phase flow transfer occurs. However, while improving the oxygen permeability and catalytic efficiency of the catalyst layer, its strength is easily affected, and it is prone to cracking under long-term use, and its durability is insufficient. Summary of the invention

[0004] In view of the problems existing in the background technology, the purpose of the present invention is to provide a sulfonated mesoporous silica in-situ modified anode catalyst layer and a preparation method thereof, which catalyst layer maintains good diffusion capacity of protons, reaction gases and water, which affect the catalytic efficiency of the catalyst layer, while still maintaining good mechanical strength and durability.

[0005] In order to achieve the above-mentioned object, the present invention provides an anode catalyst layer of sulfonated mesoporous silica in situ modification, which comprises a platinum carbon catalyst, an ionomer, a solvent, sulfonated mesoporous silica, methyl hydrogen dichlorosilane, vinyl triethoxysilane and allyl sulfonic acid; the particle size of the sulfonated mesoporous silica is 50-100 nm; the ionomer is one or a combination of poly (PDD-co-PSVE) and poly (TFE-PDD-PSVE); the mass ratio of the platinum carbon catalyst, the ionomer, the solvent, the sulfonated mesoporous silica, methyl hydrogen dichlorosilane, vinyl triethoxysilane and allyl sulfonic acid is 4-9:10-20:45-55:2-4:0.5-0.6:0.8-1:1-1.5.

[0006] Optionally, the platinum-carbon catalyst is one or a combination of a carbon-supported Pt catalyst, a carbon-supported Pt alloy catalyst, and a carbon-supported Pt monolayer catalyst.

[0007] Optionally, the solvent is a combination of deionized water and alcohol, and the alcohol is one or a combination of ethanol, methanol, isopropanol, n-propanol and n-pentanol.

[0008] The present invention also provides a method for preparing the anode catalyst layer of the sulfonated mesoporous silica in-situ modified as described above.

[0009] Optionally, the staged heat treatment comprises: the first stage is heating at normal pressure, at a temperature of 80-90°C, for 3-4 hours; and the second stage is heating under vacuum, at a temperature of 100-120°C, a vacuum degree of 0.5 MPa, for 3-3.5 hours.

[0010] The present invention also provides an application of the sulfonated mesoporous silica in-situ modified anode catalyst layer as described above or the sulfonated mesoporous silica in-situ modified anode catalyst layer prepared by the preparation method as described above, which is applied to hydrogen fuel cells.

[0011] The beneficial effects of the present invention are as follows:

[0012] 1. There are still a certain number of hydroxyl groups on the surface of the sulfonated mesoporous silica in the catalyst slurry, which undergo hydrolysis grafting reaction with vinyl triethoxysilane, and the surface of the sulfonated mesoporous silica has vinyl groups. Under the platinum catalysis of the platinum carbon catalyst, after heating, a hydrosilylation reaction occurs between allyl sulfonic acid, methyl hydrogen dichlorosilane and the vinyl groups on the surface of the sulfonated mesoporous silica, and copolymer segments with sulfonated mesoporous silica as the core are obtained. Longer high molecular weight segments are copolymerized on the surface of the sulfonated mesoporous silica, and a network structure similar to "modified microspheres" is formed in the ionomer. On the one hand, the compatibility of the sulfonated mesoporous silica in the catalyst layer is improved, and the copolymer segments on its surface are grafted with sulfonic acid groups, which is beneficial to maintaining the proton pass rate; on the other hand, the copolymer segments are interspersed in the ionomer, and the mechanical strength of the catalyst layer and the bonding strength with the base membrane are improved without reducing the proton conductivity and oxygen permeability of the membrane. In the prior art, adding surface-modified sulfonated mesoporous silica generally only increases the mechanical strength, affects the proton conductivity and oxygen permeability of the catalyst layer, and reduces the bonding strength between the catalyst layer and the base membrane.

[0013] 2. The sulfonated mesoporous silica obtained by the above method was used to in-situ modify the catalyst layer. It was found that the sulfonated mesoporous silica not only improved the mechanical strength of the catalyst membrane layer and avoided cracking, but also maintained a relatively high proton and reaction gas permeability, and the heat resistance and durability were also improved. DETAILED DESCRIPTION

[0014] In order to make the above-mentioned objects, features and advantages of the invention more obvious and easy to understand, the specific embodiments of the invention are described in detail below.

[0015] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0016] The anode catalyst layer of the in-situ modified sulfonated mesoporous silica according to the present invention comprises a platinum carbon catalyst, an ionomer, a solvent, a sulfonated mesoporous silica, methyl hydrogen dichlorosilane, vinyl triethoxysilane and allyl sulfonic acid. The platinum carbon catalyst may be one or a combination of a carbon-supported Pt catalyst, a carbon-supported Pt alloy catalyst, and a carbon-supported Pt monolayer catalyst. The particle size of the sulfonated mesoporous silica may be 50-100 nm. The ionomer may be one or a combination of poly (PDD-co-PSVE) and poly (TFE-PDD-PSVE).

[0017] In the anode catalyst layer of the sulfonated mesoporous silica in situ modification according to the present invention, the mass ratio of the platinum carbon catalyst, ionomer, solvent, sulfonated mesoporous silica, methyl hydrogen dichlorosilane, vinyl triethoxysilane and allyl sulfonic acid may be 4-9:10-20:45-55:2-4:0.5-0.6:0.8-1:1-1.5.

[0018] In the anode catalyst layer of the sulfonated mesoporous silica in-situ modified according to the present invention, the agent may be a combination of deionized water and alcohol, and the alcohol may be one or a combination of ethanol, methanol, isopropanol, n-propanol and n-pentanol.

[0019] According to the method for preparing the anode catalyst layer of the sulfonated mesoporous silica in situ modification of the present invention, it comprises the following steps: (1) grinding and mixing the raw materials including platinum carbon catalyst, ionomer, solvent, sulfonated mesoporous silica, methyl hydrogen dichlorosilane, vinyl triethoxysilane and allyl sulfonic acid in a grinding mixer to obtain a catalyst slurry; (2) coating the catalyst slurry on the base film PET or proton exchange membrane, heat treating in stages, vacuum drying, cooling to room temperature, and obtaining the anode catalyst layer of the sulfonated mesoporous silica in situ modification. The staged heat treatment comprises: the first stage is heating at normal pressure, the temperature is 80-90°C, the time is 3-4h; the second stage is vacuum heating, the temperature is 100-120°C, the vacuum degree is 0.5Mpa, and the time is 3-3.5h.

[0020] The anode catalyst layer in-situ modified with sulfonated mesoporous silica according to the present invention can be applied to hydrogen fuel cells.

[0021] The following examples specifically illustrate the anode catalyst layer of the sulfonated mesoporous silica in-situ modified anode catalyst layer and its preparation method and application. Main raw materials and equipment used: Unless otherwise specified, the raw materials and equipment of each embodiment and comparative example are the same; materials without specific models or types are from the same common models purchased on the market, and no specific restrictions are imposed.

[0022] Raw materials:

[0023] Platinum carbon catalyst, TEC10E40E, TANAKA, Japan;

[0024] poly (PDD-co-PSVE), Toyota, Japan;

[0025] Sulfonated mesoporous silica, homemade, particle size 50-100nm, pore size 2-50nm, specific surface area 700-800m 2 / g, acid content 2.8-3.1mmol / g;

[0026] Methylhydrodichlorosilane, superior grade, Nanxing Chemical (Jiangsu) Co., Ltd.;

[0027] Vinyl triethoxysilane, model 151, Momentive, USA;

[0028] Allyl sulfonic acid, homemade: Sodium allyl sulfonate (Guangdong Fangxin Biotechnology Co., Ltd., AR98.5%) was mixed in 30wt% hydrochloric acid solution, stirred at 50-60℃ for 2h, cooled and allowed to stand for stratification, the oil phase was extracted, mixed with deionized water, washed and stratified, and the oil phase was vacuum dried to obtain allyl sulfonic acid.

[0029] Example 1

[0030] (1) 4 g of platinum carbon catalyst, 10 g of poly (PDD-co-PSVE), 45 g of deionized water, 2 g of sulfonated mesoporous silica, 0.5 g of methylhydrogendichlorosilane, 0.8 g of vinyltriethoxysilane and 1 g of allyl sulfonic acid are ground and mixed in a grinding mixer to obtain a catalyst slurry; (2) The catalyst slurry is coated on a base film PET or a proton exchange membrane, and heat treated in stages: the first stage is heated at normal pressure, the temperature is 80°C, and the time is 3 h; the second stage is vacuum heated, the temperature is 100°C, the vacuum degree is 0.5 MPa, and the time is 3 h; (3) Vacuum drying is performed, and the temperature is cooled to room temperature to obtain an anode catalyst layer of sulfonated mesoporous silica in situ modified.

[0031] Example 2

[0032] (1) 9 g of platinum carbon catalyst, 20 g of poly (PDD-co-PSVE), 55 g of deionized water, 4 g of sulfonated mesoporous silica, 0.6 g of methylhydrogendichlorosilane, 1 g of vinyltriethoxysilane and 1.5 g of allyl sulfonic acid are ground and mixed in a grinding mixer to obtain a catalyst slurry; (2) The catalyst slurry is coated on a base film PET or a proton exchange membrane, and heat treated in stages: the first stage is heated at normal pressure, the temperature is 90°C, and the time is 4 h; the second stage is vacuum heated, the temperature is 120°C, the vacuum degree is 0.5 MPa, and the time is 3.5 h; (3) Vacuum drying is performed, and the temperature is cooled to room temperature to obtain an anode catalyst layer of sulfonated mesoporous silica in situ modified.

[0033] Example 3

[0034] (1) Grind and mix 6.5 g of platinum carbon catalyst, 15 g of poly (PDD-co-PSVE), 50 g of deionized water, 3 g of sulfonated mesoporous silica, 0.55 g of methylhydrogendichlorosilane, 0.9 g of vinyltriethoxysilane and 1.2 g of allyl sulfonic acid in a grinding mixer to obtain a catalyst slurry; (2) Coat the catalyst slurry on a base film PET or a proton exchange membrane, and perform heat treatment in stages: the first stage is heating at normal pressure, at a temperature of 85°C, for 3-4 h; the second stage is vacuum heating, at a temperature of 110°C, at a vacuum degree of 0.5 MPa, for 3.5 h; (3) Vacuum drying is performed, and cooling is performed to room temperature to obtain an anode catalyst layer of sulfonated mesoporous silica in situ modified.

[0035] Comparative Example 1

[0036] Except that nano-sized sulfonated mesoporous silica is not added, other aspects are the same as those of Example 3.

[0037] Comparative Example 2

[0038] Except that methyl hydrogen dichlorosilane, vinyl triethoxysilane and allyl sulfonic acid were not used, the other steps were the same as those in Example 3.

[0039] Comparative Example 3

[0040] (1) Grind and mix 0.5g of platinum carbon catalyst, 3g of sulfonated mesoporous silica, 1.45g of vinyl triethoxysilane and 1.2g of allyl sulfonic acid in a grinding mixer, heat to 100°C and keep for 2h, dry the product, and grind to obtain surface-modified sulfonated mesoporous silica; (2) Grind and mix the above-mentioned surface-modified sulfonated mesoporous silica and 6.5g of platinum carbon catalyst, 15g of poly (PDD-co-PSVE) and 50g of deionized water in a grinding mixer to obtain a catalyst slurry; (3) Coat the catalyst slurry on a base film PET or a proton exchange membrane, and heat treat in stages: the first stage is heated at normal pressure, at a temperature of 85°C, for 3-4h; the second stage is vacuum heated, at a temperature of 110°C, at a vacuum degree of 0.5Mpa, for 3.5h; (4) Vacuum drying, cooling to room temperature, and obtaining an anode catalyst layer of sulfonated mesoporous silica in situ modification.

[0041] Performance Testing

[0042] 1. The thickness of the catalyst layer in the examples and comparative examples was 0.2 mm.

[0043] 2. At 23°C and 0% relative humidity, the oxygen permeability of the catalyst layer after peeling off from the surface of the base membrane PET was tested using an instrument (Mocon OX-Tran®, Minneapolis, MN, USA); at 80°C and 95% relative humidity, the catalyst layer was loaded into the electrolyte membrane of the electrochemical cell, the test electrodes were connected to both sides of the electrolyte membrane, an external voltage was applied, and the proton conductivity was calculated.

[0044] 3. The mechanical strength and interlayer peeling strength of the catalyst layer and the composite membrane composed of the catalyst layer and proton exchange membrane (perfluorosulfonic acid ion membrane, N117, Nafion, DuPont, USA) were tested using a universal material testing machine (GB / T 20042.3-2022).

[0045] See Table 1 for specific data.

[0046] Table 1

[0047]

[0048] It can be seen from the data of the embodiments and comparative examples that the in-situ modification of nano-scale sulfonated mesoporous silica in the catalyst slurry in the preparation method of the present invention can significantly improve the mechanical strength of the catalyst layer, and also improve the interlayer peeling strength, and the proton conductivity and oxygen permeability remain excellent, indicating that the internal and surface mesoporous structures of the nano-scale sulfonated mesoporous silica promote the pore formation of the catalyst layer. The catalyst layer and the composite membrane composed of the proton exchange membrane all show good performance, and the durability and heat resistance are improved.

[0049] The above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the present invention.

Claims

1. A method for preparing an anode catalyst layer of sulfonated mesoporous silica in situ modification, It is characterized in that The method comprises the following steps: (1) grinding and mixing raw materials including a platinum carbon catalyst, an ionomer, a solvent, sulfonated mesoporous silica, methylhydrogendichlorosilane, vinyltriethoxysilane and allyl sulfonic acid in a grinding mixer to obtain a catalyst slurry; (2) coating the catalyst slurry on a base film PET or a proton exchange membrane, performing a heat treatment in stages, vacuum drying, and cooling to room temperature to obtain an anode catalyst layer of in-situ modified sulfonated mesoporous silica; the heat treatment in stages comprises: a first stage of normal pressure heating at a temperature of 80-90° C. for 3-4 hours; a second stage of vacuum heating at a temperature of 100-120° C., a vacuum degree of 0.5 Mpa, and a time of 3-4 hours. 3.5h; the particle size of the sulfonated mesoporous silica is 50-100nm; the ionomer is one or a combination of perfluoro(2,2-dimethyl-1,3-dioxole)-perfluorosulfonylethoxypropyl vinyl ether copolymer and tetrafluoroethylene-perfluoro(2,2-dimethyl-1,3-dioxole)-perfluorosulfonylethoxypropyl vinyl ether copolymer; the mass ratio of the platinum carbon catalyst, ionomer, solvent, sulfonated mesoporous silica, methyl hydrogen dichlorosilane, vinyl triethoxysilane and allyl sulfonic acid is 4-9:10-20:45-55:2-4:0.5-0.6:0.8-1:1-1.

5.

2. The method for preparing the anode catalyst layer of the sulfonated mesoporous silica in-situ modified according to claim 1, It is characterized in that The platinum-carbon catalyst is one or a combination of a carbon-supported Pt catalyst and a carbon-supported Pt alloy catalyst.

3. The method for preparing the anode catalyst layer of the sulfonated mesoporous silica in-situ modified according to claim 2, It is characterized in that The carbon-supported Pt catalyst is a carbon-supported Pt single-layer catalyst.

4. The method for preparing the anode catalyst layer of the sulfonated mesoporous silica in-situ modified according to claim 1, It is characterized in that The solvent is a combination of deionized water and alcohol, and the alcohol is one or a combination of ethanol, methanol, isopropanol, n-propanol and n-pentanol.

5. Application of the sulfonated mesoporous silica in-situ modified anode catalyst layer prepared by the preparation method according to any one of claims 1 to 4, It is characterized in that Used in hydrogen fuel cells.