Photovoltaic cell and preparation method
By using alternately attached high-refractive index material film layers in photovoltaic cells, the aging and thermal effects of photovoltaic cells under sun exposure are solved, and a higher level of Stability and performance.
Patent Information
- Application Number
- CN202411170542.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-26
AI Technical Summary
The organic materials of photovoltaic cells age rapidly under sun exposure, resulting in power attenuation and shortening of service life. The resonance of ultraviolet and infrared rays accelerates molecular motion and structural damage, affecting component performance.
The light cut-off film stack is constructed with alternately attached high-refractive index material film layers to cut off ultraviolet and infrared rays, and the visible light transmittance is increased through the light resistant film stack layer, thereby improving the stability and performance of photovoltaic cells.
Effectively prevent the entry of ultraviolet and infrared rays, reduce material aging and thermal effects, improve the stability and performance of photovoltaic cells, and extend the service life.
Smart Images

Figure CN118695625B_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of battery technology, and specifically relates to a photovoltaic cell and a preparation method thereof. Background Art
[0002] At present, most of the film layers of photovoltaic cells are organic materials. The ultraviolet light in sunlight has a short wavelength and high photon energy. After long-term exposure to the sun, the macromolecules of the organic material will break, causing the material to age rapidly and the polarity to change, resulting in rapid power decay of the solar photovoltaic module, which seriously affects the power generation efficiency and service life of the photovoltaic module. The infrared rays in sunlight have a significant thermal effect and can resonate with most molecules in the photovoltaic module, converting light energy into heat energy, thereby accelerating molecular movement and mutual friction, generating heat, causing serious temperature rise inside the module, leading to damage to the photovoltaic module structure and affecting the performance of the photovoltaic module. At the same time, infrared rays will also cause ion migration in the photovoltaic cell, and permanent ion migration will destroy the photovoltaic module structure and cause the performance of the photovoltaic module to decline. Summary of the invention
[0003] The embodiments of the present application provide a photovoltaic cell and a preparation method, which can cut off ultraviolet rays and infrared rays while increasing the transmittance of visible light, which is beneficial to improving the stability and performance of the photovoltaic cell.
[0004] In a first aspect, an embodiment of the present application provides a photovoltaic cell, the photovoltaic cell comprising:
[0005] a first substrate;
[0006] A first light-cutting film stack layer, the first light-cutting film stack layer is arranged on the front side of the first substrate; the first light-cutting film stack layer comprises at least one first material film layer and at least one second material film layer attached alternately, the refractive index of the first material film layer is higher than the refractive index of the second material film layer; the first light-cutting film stack layer is used to cut off light in a first wavelength range in the incident light;
[0007] A light anti-reflection film stack, the light anti-reflection film stack is arranged on the upper surface of the first light cut-off film stack, the light anti-reflection film stack includes at least one third material film layer and at least one fourth material film layer alternately attached, the refractive index of the third material film layer is higher than the refractive index of the fourth material film layer; the light anti-reflection film stack is used to increase the transmittance of light in the second wavelength range of the incident light;
[0008] a second light-cutting film stack layer, the second light-cutting film stack layer being arranged on the reverse side of the first substrate, the second light-cutting film stack layer comprising at least one fifth material film layer and at least one sixth material film layer attached alternately, the refractive index of the fifth material film layer being higher than the refractive index of the sixth material film layer; the second light-cutting film stack layer being used for cutting off light in a third wavelength range of the incident light;
[0009] A battery assembly, wherein the battery assembly is arranged on the lower surface of the second light-cutting film stack layer;
[0010] The thickness of the first light cutoff film stack layer is in the range of 3.4-3.6 um, the thickness of the light anti-reflection film stack layer is in the range of 0.5-0.8 um, and the thickness of the second light cutoff film stack layer is in the range of 1.0-1.6 um.
[0011] In a possible example, the battery assembly includes an encapsulation film, a top electrode, an electron transport layer, a light absorption layer, a hole transport layer, a bottom electrode and butyl rubber; the top electrode is connected to the encapsulation film and the electron transport layer, respectively; the light absorption layer is connected to the electron transport layer and the hole transport layer, respectively; the bottom electrode is connected to the hole transport layer; the encapsulation film and the butyl rubber are used to seal the battery assembly.
[0012] In a possible example, the photovoltaic cell includes a second substrate, wherein the second substrate is connected to the bottom electrode; and a hemispherical protrusion is formed on a lower surface of the second substrate.
[0013] In a possible example, the photovoltaic cell includes a heat dissipation material film layer; the heat dissipation material film layer is arranged on the lower surface of the second substrate.
[0014] In a possible example, the photovoltaic cell includes a polymer material layer; the polymer material layer is deposited on an upper surface of the light anti-reflection film stack.
[0015] In a possible example, the first wavelength range is 800-1500 nm, the second wavelength range is 380-760 nm, and the third wavelength range is 300-380 nm.
[0016] In a possible example, the first material film layer includes at least one of the following: TiO2, CeO2, Nb2O5, SiN m 、SiO x N y and ZnO, the second material film layer includes at least one of the following: SiO2 and MgF2. The third material film layer includes at least one of the following: Nb2O5, Si3N4, SiON x, SnO2, the fourth material film layer includes: SiO2. The fifth material film layer includes at least one of the following: TiO2, CeO2, Nb2O5, SnO2, SiN m 、SiO x N y , ZnO, and the sixth material film layer includes at least one of the following: SiO2 and MgF2.
[0017] In a possible example, the molar ratio of Ce to Ti in the first material film layer ranges from 0.95:1 to 1.05:1.
[0018] In a second aspect, an embodiment of the present application provides a method for preparing a photovoltaic cell, comprising:
[0019] A first light-cutting film stack layer is plated on the front surface of the first substrate, wherein the first light-cutting film stack layer comprises at least one first material film layer and at least one second material film layer which are alternately attached, and the refractive index of the first material film layer is higher than the refractive index of the second material film layer; the first light-cutting film stack layer is used to cut off light in a first wavelength range in the incident light;
[0020] A light anti-reflection film stack is plated on the first light cut-off film stack, wherein the light anti-reflection film stack comprises at least one third material film layer and at least one fourth material film layer alternately attached, wherein the refractive index of the third material film layer is higher than the refractive index of the fourth material film layer; the light anti-reflection film stack is used to increase the transmittance of light in the second wavelength range of the incident light;
[0021] A second light-cutting film stack layer is plated on the reverse side of the first substrate, wherein the second light-cutting film stack layer comprises at least one fifth material film layer and at least one sixth material film layer which are alternately attached, wherein the refractive index of the fifth material film layer is higher than the refractive index of the sixth material film layer; the second light-cutting film stack layer is used to cut off light in the third wavelength range of the incident light;
[0022] Bonding the plated first substrate to the battery assembly;
[0023] Plating a heat dissipation material film layer on the lower surface of the second substrate;
[0024] The second substrate is bonded to the battery assembly.
[0025] In a possible example, the step of coating the first light-cutting film stack layer on the front surface of the first substrate includes:
[0026] The second material film layer and the first material film layer are alternately plated on the front surface of the first substrate.
[0027] A third aspect of the present application provides an electronic device, comprising: a processor and a memory; and one or more programs, wherein the one or more programs are stored in the memory and configured to be executed by the processor, and the programs include instructions for some or all of the steps described in the second aspect.
[0028] A fourth aspect of an embodiment of the present application provides a computer-readable storage medium, wherein the computer-readable storage medium is used to store a computer program, wherein the computer program enables a computer to execute instructions of some or all of the steps described in the second aspect of the embodiment of the present application.
[0029] A fifth aspect of the embodiments of the present application provides a computer program product, wherein the computer program product includes a non-transitory computer-readable storage medium storing a computer program, and the computer program is operable to cause a computer to execute some or all of the steps described in the second aspect of the embodiments of the present application. The computer program product may be a software installation package.
[0030] It can be seen that in the embodiment of the present application, the photovoltaic cell includes a first substrate, a first light cutoff film stack layer, a light anti-reflection film stack layer, a second light cutoff film stack layer and a battery assembly, the first light cutoff film stack layer is arranged on the front side of the first substrate, the light anti-reflection film stack layer is arranged on the upper surface of the first light cutoff film stack layer, the second light cutoff film stack layer is arranged on the reverse side of the first substrate, and the battery assembly is arranged on the lower surface of the second light cutoff film stack layer; the first light cutoff film stack layer includes at least one first material film layer and at least one second material film layer alternately attached, and the refractive index of the first material film layer is higher than the refractive index of the second material film layer; The first light-cutting film stack is used to cut off the light in the first wavelength range of the incident light; the light-reflecting film stack includes at least one third material film layer and at least one fourth material film layer attached alternately, and the refractive index of the third material film layer is higher than the refractive index of the fourth material film layer; the light-reflecting film stack is used to increase the transmittance of the light in the second wavelength range of the incident light; the second light-cutting film stack includes at least one fifth material film layer and at least one sixth material film layer attached alternately, and the refractive index of the fifth material film layer is higher than the refractive index of the sixth material film layer; the second light-cutting film stack is used to cut off the light in the third wavelength range of the incident light. The infrared rays can be cut off by the first light-cutting film stack, the ultraviolet rays can be cut off by the second light-cutting film stack, and the transmittance of visible light can be increased by the light-reflecting film stack, which is beneficial to improving the stability and performance of photovoltaic cells. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0032] Figure 1 is a schematic structural diagram of a photovoltaic cell provided in an embodiment of the present application;
[0033] Figure 2 is a schematic structural diagram of a battery assembly provided in an embodiment of the present application;
[0034] Figure 3 is a schematic diagram of a substrate provided in an embodiment of the present application;
[0035] Figure 4 is a schematic diagram of another substrate provided in an embodiment of the present application;
[0036] Figure 5 It is a schematic diagram of a process for preparing a photovoltaic cell provided in an embodiment of the present application;
[0037] Figure 6 It is a schematic diagram of a material film layer provided in an embodiment of the present application. DETAILED DESCRIPTION
[0038] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0039] The terms "first", "second", etc. in the specification and claims of this application and the above-mentioned drawings are used to distinguish different objects, rather than to describe a specific order. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not limited to the listed steps or units, but optionally includes steps or units that are not listed, or optionally includes other steps or units inherent to these processes, methods, products or devices.
[0040] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0041] In the embodiments of the present application, "and / or" describes the association relationship of the associated objects, indicating that three relationships may exist. For example, A and / or B can represent the following three situations: A exists alone; A and B exist at the same time; B exists alone. Among them, A and B can be singular or plural.
[0042] In the embodiment of the present application, the symbol " / " can indicate that the objects associated with each other are in an "or" relationship. In addition, the symbol " / " can also indicate a division sign, that is, performing a division operation. For example, A / B can indicate A divided by B.
[0043] In the embodiments of the present application, "at least one item" or similar expressions refer to any combination of these items, including any combination of single items or plural items, and refer to one or more, and multiple refers to two or more. For example, at least one item of a, b, or c can represent the following seven situations: a, b, c, a and b, a and c, b and c, a, b, and c. Among them, each of a, b, and c can be an element or a set containing one or more elements.
[0044] In the embodiments of the present application, "equal to" can be used in conjunction with greater than, and is applicable to the technical solution adopted when greater than, and can also be used in conjunction with less than, and is applicable to the technical solution adopted when less than. When equal to is used in conjunction with greater than, it is not used in conjunction with less than; when equal to is used in conjunction with less than, it is not used in conjunction with greater than.
[0045] In order to better understand the solutions of the embodiments of the present application, the electronic devices, related concepts and backgrounds that may be involved in the embodiments of the present application are first introduced below.
[0046] The electronic device of the embodiment of the present application is a device with a wireless communication function, which can be called a terminal, a user equipment (UE), a mobile station (MS), a mobile terminal (MT), an access electronic device, a vehicle-mounted electronic device, an industrial control electronic device, a UE unit, a UE station, a mobile station, a remote station, a remote electronic device, a mobile device, a UE electronic device, a wireless communication device, a UE agent or a UE device, etc. The electronic device can be fixed or mobile. It should be noted that the electronic device can support at least one wireless communication technology, such as LTE, new radio (NR), wideband code division multiple access (WCDMA), etc. For example, the electronic device may be a mobile phone, a tablet computer, a desktop computer, a laptop computer, an all-in-one computer, a vehicle-mounted terminal, a virtual reality (VR) electronic device, an augmented reality (AR) electronic device, a wireless terminal in industrial control, a wireless terminal in self-driving, a wireless terminal in remote medical surgery, a wireless terminal in smart grid, a wireless terminal in transportation safety, a wireless terminal in smart city, a wireless terminal in smart home, a cellular phone, a cordless phone, a session initiation protocol (SIP) phone, a wireless local loop (WLL) station, a personal digital assistant (PDA), a handheld device with wireless communication function, a terminal device or other processing device connected to a wireless modem, a wearable device, an electronic device in a future mobile communication network, or an electronic device in a future evolving public land mobile network (PLMN), etc. The electronic device may also be a battery assembly preparation device.
[0047] See also Figure 1 , Figure 1 Schematic diagram of the structure of a photovoltaic cell provided in the embodiment of the present application. Figure 1As shown, the photovoltaic cell includes: a first substrate 10 , a first light-cutting film stack layer 20 , a light-antireflection film stack layer 30 , a second light-cutting film stack layer 40 , a cell assembly 50 and a second substrate 60 .
[0048] Among them, the first light cutoff film stack layer 20 is arranged on the front side of the first substrate 10, the light anti-reflection film stack layer 30 is arranged on the upper surface of the first light cutoff film stack layer 20, the second light cutoff film stack layer 40 is arranged on the reverse side of the first substrate 10, and the battery assembly 50 is arranged on the lower surface of the second light cutoff film stack layer 40.
[0049] The first light cut-off film stack 20 includes at least one first material film layer and at least one second material film layer alternately attached, and the refractive index of the first material film layer is higher than the refractive index of the second material film layer; the first light cut-off film stack 20 is used to cut off the light in the first wavelength range of the incident light. The first light cut-off film stack 20 prevents this part of infrared light from entering the battery assembly by increasing the reflection effect of infrared light in the 800nm-1500nm band, causing the assembly to heat up. The thickness a of the second light cut-off film stack 40 is reasonably designed for infrared light in the 800-1500nm band, and the optical path difference of the reflected light is δ=na=λ / 4 as much as possible, so the phase difference is π, so that when two adjacent beams of light arrive at the same reflection interface, the peak and the trough are superimposed, then the reflected light intensity of this wavelength range is the weakest, and after the reflected light passes through several layers of interference, the reflected light intensity is almost 0, thereby reducing the accumulation of heat of the reflected light inside the photovoltaic cell, thereby reducing the thermal effect caused by infrared light. n represents the refractive index of the film layer. The thickness a of a single film layer in the first light-cutting film stack 20 is in the range of 200 nm to 375 nm.
[0050] Among them, the battery component 50 can be a perovskite photovoltaic component, or it can be a Topcon (tunneling oxide passivation contact), PERC (passivated emitter and back contact), HJT (heterojunction cell), amorphous silicon, microcrystalline silicon, GaAs (gallium arsenide), CdTe (cadmium telluride), CIGS (copper indium gallium selenide) and other photovoltaic components, which are not limited here.
[0051] The materials of the first substrate 10 and the second substrate 60 can be glass, plastic, metal, etc., which are not limited here.
[0052] The light anti-reflection film stack 30 includes at least one third material film layer and at least one fourth material film layer alternately attached, the refractive index of the third material film layer is higher than the refractive index of the fourth material film layer; the light anti-reflection film stack is used to increase the transmittance of light in the second wavelength range of the incident light. The perovskite photovoltaic module can select a 1.32eV bandgap width material so that its main absorption band is also mainly concentrated in the light band below 760nm, so that the absorption spectrum range of the perovskite light absorption layer can be consistent with the designed light anti-reflection film stack 30, thereby improving the power generation efficiency of the perovskite photovoltaic module.
[0053] Among them, the second light cut-off film stack 40 includes at least one fifth material film layer and at least one sixth material film layer alternately attached, and the refractive index of the fifth material film layer is higher than the refractive index of the sixth material film layer; the second light cut-off film stack is used to cut off the light in the third wavelength range of the incident light. The second light cut-off film stack 40 prevents this part of ultraviolet rays from entering the battery assembly by increasing the reflection effect on 330nm-380nm ultraviolet rays, causing material aging, affecting the service life and efficiency stability of the material. According to the wavelength range of ultraviolet rays mainly in the range of 300nm-380nm, the thickness b of each film layer in the first light cut-off film stack 20 is reasonably designed by using sub-bands, and the optical path difference of the reflected light is δ=nb=λ / 2 as much as possible, so the phase difference is 0, so that when two adjacent beams of light arrive at the same reflection interface, the peaks are superimposed, and the reflected light of this wavelength obtains the strongest reflection, and the incident light obtains strong reflection on each film layer. After several layers of reflection, the ultraviolet rays are almost all reflected back, thereby achieving the purpose of cutting off the ultraviolet light wave. n represents the refractive index of the film layer, and δ represents the optical path difference of the reflected light. The thickness b of a single film layer in the second light cutoff film stack 40 is in the range of 150nm-180nm.
[0054] Among them, the total number of layers of the first material film layer and the second material film layer in the first light cutoff film stack 20 is 18-26 layers, the thickness of the first light cutoff film stack 20 is in the range of 3.4-3.6um, the thickness of the first material film layer and the second material film layer is the same or different, and the number of layers of the first material film layer and the second material film layer is the same or different; wherein, the total number of layers of the third material film layer and the fourth material film layer in the light anti-reflection film stack 30 is 4-8 layers, the thickness of the light anti-reflection film stack 30 is in the range of 0.5-0.8um, the thickness of the third material film layer and the fourth material film layer is the same or different, and the number of layers of the third material film layer and the fourth material film layer is the same or different; the total number of layers of the fifth material film layer and the sixth material film layer in the second light cutoff film stack 40 is 6-12 layers, the thickness of the second light cutoff film stack 40 is in the range of 1.0-1.6um, the thickness of the fifth material film layer and the sixth material film layer is the same or different, and the number of layers of the fifth material film layer and the sixth material film layer is the same or different.
[0055] The first wavelength range is 800-1500 nm, the second wavelength range is 380-760 nm, and the third wavelength range is 330-380 nm.
[0056] Among them, after the visible light of 380-760nm passes through the light anti-reflection film stack 30 of the first substrate 10, very little visible light will be reflected out of the battery assembly 50, and most of the visible light will enter the battery assembly 50 and be absorbed by the battery assembly to generate electricity, or the battery assembly 50 will generate heat. When the infrared light enters the light anti-reflection film stack 30, part of the infrared light will be reflected out of the photovoltaic cell due to the reflection between the various film layers in the light anti-reflection film stack 30. After the infrared light enters the first light cutoff film stack 20, the near-infrared light in the wavelength range of 760-1500nm will be reflected out of the assembly due to the interference cutoff effect. The remaining mid- and far-infrared light accounts for a relatively small proportion of the entire infrared spectrum. The mid- and far-infrared light with a wavelength greater than 1500nm will pass through the various film stacks and enter the battery assembly 50. A part of this part of the infrared light passes through the battery assembly 50, and the other part will cause the molecular vibration of the material inside the battery assembly 50, generating heat energy, causing the temperature of the battery assembly 50 to rise. After the ultraviolet rays of 300-380nm enter the light anti-reflection film stack 30, part of the ultraviolet rays of 330-380nm will be reflected out due to the interface reflection of each film layer in the light anti-reflection film stack 30, and the other part of the ultraviolet rays of 300-330nm will be cut off by the interference of the second light cutoff film stack 40 when transmitting between the film layers of the second light cutoff film stack 40. At this time, only a very small amount of ultraviolet rays will enter the interior of the battery assembly 50.
[0057] It can be seen that the photovoltaic cell can cut off infrared rays through the first light-cutting film stack layer 20, cut off ultraviolet rays through the second light-cutting film stack layer 40, and at the same time increase the transmittance of light in the second wavelength range through the light-enhancing film stack layer 30, which is beneficial to improving the stability and performance of the photovoltaic cell.
[0058] See also Figure 2 , Figure 2 It is a schematic diagram of the structure of a battery assembly provided in an embodiment of the present application, wherein the battery assembly 50 includes a packaging film 51, a top electrode 52, an electron transport layer 53, a light absorption layer 54, a hole transport layer 55, a bottom electrode 56 and a butyl rubber 57; the top electrode 52 is connected to the packaging film 51 and the electron transport layer 53, respectively; the light absorption layer 54 is connected to the electron transport layer 53 and the hole transport layer 55, respectively; the bottom electrode 56 is connected to the hole transport layer 55; the packaging film 51 and the butyl rubber 57 are used to seal the battery assembly.
[0059] The packaging film 51 is used to adhere the battery assembly 50 and the second light-cutting film stack layer 40 ; the butyl rubber 57 is arranged on both sides of the battery assembly 50 to seal the battery assembly 50 and isolate it from water and oxygen.
[0060] The packaging film 51 is made of one or more materials such as POE (polyolefin elastomer), EVA (ethylene-vinyl acetate copolymer), TPO (thermoplastic polyolefin), etc.
[0061] The light absorbing layer 54 may be a perovskite light absorbing layer.
[0062] In a possible example, the second substrate 60 is connected to the bottom electrode 56 ; a hemispherical protrusion is formed on the lower surface of the second substrate 60 .
[0063] See also Figure 3 , Figure 3 is a schematic diagram of a substrate provided in an embodiment of the present application, wherein a hemispherical protrusion is formed on the lower surface of the second substrate 60. A hemispherical protrusion with a radius r is formed on the second substrate 60 by exposure, etching, and embossing processes. Compared with the non-protruding design of the substrate, d is the thickness of the second substrate, and the heat dissipation of the second substrate 60 is performed through the contact surface between the substrate and the air. The surface area of the convex-concave structure (2πr 2 ) compared to the surface area of non-convex and concave structures (πr 2 )Increased surface area△S=πr 2 , the surface area is doubled, indicating that the heat dissipation through the back side of the second substrate 60 can be doubled.
[0064] Among them, the lower surface structure of the second substrate 60 can be circular, elliptical, polygonal and other forms. The main function of this design method is to increase the contact area between the surface of the second substrate 60 and the air, and considering that infrared light with a wavelength greater than 1500nm can pass through the first light cutoff film stack layer, the light anti-reflection film stack layer, the second light cutoff film stack layer, and the battery assembly, by increasing the surface area of the second substrate 60, the surface area of infrared light with a wavelength greater than 1500nm that is radiated outward by thermal radiation is correspondingly increased, thereby quickly cooling the battery assembly 50.
[0065] It can be seen that in this example, by forming hemispherical protrusions on the lower surface of the second substrate 60 , the heat dissipation efficiency of the photovoltaic cell is improved.
[0066] In a possible example, the photovoltaic cell includes a heat dissipation material film layer 70 ; the heat dissipation material film layer 70 is disposed on the lower surface of the second substrate 60 .
[0067] Among them, iron oxide, chromium oxide, boron carbide, silicon carbide, silicon nitride, silicon oxynitride, silicon oxide and other semiconductor ceramic materials with high infrared emissivity are plated on the surface of the substrate by PVD (Physical Vapor Deposition), CVD (Chemical Vapor Deposition) and other coating methods, and carbon paste, graphite, graphene and other materials with high infrared emissivity can also be formed on the surface by screen printing, coating and other methods. The infrared emissivity of these materials is 0.8-0.9, which can greatly improve the infrared radiation effect on the object and quickly reduce the temperature of the battery assembly 50.
[0068] See also Figure 4 , Figure 4 Schematic diagram of another substrate provided in an embodiment of the present application, a heat dissipation material film layer 70 with a thickness of Rr is formed on the lower surface of the convex-concave points of the second substrate 60, so at this time the surface area of the convex-concave structure (2πR 2 ) compared to the surface area of non-convex and concave structures (πr 2 )Increased surface area△S=2πR 2 -πr 2 >πr 2 When the temperature of an object rises, it can be conducted to the air as much as possible through the protrusions. The increase in surface area greatly improves the conduction effect. On the other hand, high-emissivity materials can radiate mid- and far-infrared rays outward through thermal radiation, which can greatly improve the cooling effect of the material and effectively prevent the temperature of the battery assembly 50 from continuing to rise.
[0069] It can be seen that in this example, the heat dissipation material film layer 70 can improve the radiation effect of the photovoltaic cell on infrared rays, which is beneficial to improving the heat dissipation efficiency of the photovoltaic cell.
[0070] In a possible example, the photovoltaic cell includes a polymer material layer; the polymer material layer is deposited on the surface of the light anti-reflection film stack 30 .
[0071] Among them, a fluorosilicone polymer material with a thickness of 5-8nm is deposited on the light anti-reflection film stack 30 to form a polymer material layer. The polymer material layer can form a molecular bond with the film layer, which can reduce the dynamic friction coefficient of the light anti-reflection film stack 30 and improve the scratch resistance of the light anti-reflection film stack 30.
[0072] It can be seen that in this example, the scratch resistance of the light anti-reflection film stack 30 can be improved by the polymer material layer.
[0073] In a possible example, the first material film layer includes at least one of the following: TiO2, CeO2, Nb2O5, SiN m 、SiOx N y and ZnO, the second material film layer includes at least one of the following: SiO2 and MgF2. The third material film layer includes at least one of the following: Nb2O5, Si3N4, SiON x , SnO2, the fourth material film layer includes: SiO2; the fifth material film layer includes at least one of the following: TiO2, CeO2, Nb2O5, SnO2, SiN m 、SiO x N y , ZnO, and the sixth material film layer includes at least one of the following: SiO2 and MgF2.
[0074] Among them, SiN m The ratio of Si atoms to N atoms in SiO is 1:m. x N y The ratio of Si, O atoms and N is 1:x:y. There is no limit on the values of m, x, and y. For example, if m is 1, then SiN m is SiN, x is 2, y is 2, then SiO x N y It is SiO2N2.
[0075] The molar ratio of Ce to Ti in the fifth material film layer is in the range of 0.95:1 to 1.05:1.
[0076] Among them, due to Ce3 + Ions can capture positive holes to form Ce4 + Ion, Ce4 + Ions are electron capture centers. When high-energy radiation acts on the substrate and generates positive holes or free electrons, they are first captured by cerium ions, causing their valence state to change. The absorption band caused by the valence change of cerium ions is located in the ultraviolet spectrum. In addition to the absorption of ultraviolet rays by cerium ions, Ti4 + There is also strong absorption, Ce4 + and Ti4 + Ion compounding has high ultraviolet absorption rate and does not affect visible light transmittance. Therefore, the absorption effect of TiO2-CeO2 film on ultraviolet rays is more obvious. When the molar ratio of Ce to Ti in the first material film layer is 1:1, the obtained TiO2-CeO2 film has the strongest absorption of ultraviolet rays. As the thickness of the film layer increases, the amount of Ti-O-Ce formed increases, which can form sufficient impurity energy levels and enhance the ability of the valence band to accept electrons. At the same time, it is easier to force electrons to transition to the conduction band, causing the absorption edge and the cutoff edge to redshift, and the ultraviolet absorption capacity is enhanced. It can be seen that the second light cutoff film stack 40 cuts off ultraviolet rays by both reflection and absorption.
[0077] In order to improve the photocatalytic oxidation effect, a highly active noble metal is doped in the nano TiO2-CeO2 film layer to improve the photocatalytic activity of TiO2-CeO2, thereby improving the ultraviolet absorption capacity of the TiO2-CeO2 film. The noble metal can be Ag, Au, Pt, Pd, Nb, etc., which are not limited here.
[0078] It can be seen that in this example, infrared rays can be cut off by the first light-cutting film stack 20, ultraviolet rays can be reflected and absorbed by the second light-cutting film stack 40, and the transmittance of visible light can be increased by the light-enhancing film stack 30, which is beneficial to improving the stability and performance of the photovoltaic cell.
[0079] See also Figure 5 , Figure 5 1 is a schematic flow chart of a method for preparing a photovoltaic cell provided in an embodiment of the present application, the method comprising:
[0080] Step S501: coating a first light-cutting film stack layer on the front surface of the first substrate.
[0081] Among them, the first light-cutting film stack includes at least one first material film layer and at least one second material film layer alternately attached, the refractive index of the first material film layer is higher than the refractive index of the second material film layer; the first light-cutting film stack is used to cut off light in the first wavelength range of the incident light.
[0082] Among them, in the production of the film layers in the first light cutoff film stack, the light anti-reflection film stack and the second light cutoff film stack, the present scheme adopts magnetron sputtering. During magnetron sputtering, high-energy incident ions bombard the surface of the target material, causing the target atoms or molecules to be sputtered and deposited on the substrate with very high energy, and converting their own kinetic energy into heat energy, thereby enhancing the adhesion of the sputtered atoms to the substrate. Under the high-temperature and high-energy plasma state, the film layers are more firmly bonded and more dense, so that the coated film layer itself has a lower absorption rate of light.
[0083] Among them, the second material film layer and the first material film layer are alternately plated on the front side of the first substrate in sequence; the second material film layer is plated on the surface of the first substrate first because, on the one hand, the second material film layer can effectively prevent the metal ions in the substrate material from diffusing into the optical film layer and affecting the optical properties, and on the other hand, it can also increase the adhesion.
[0084] Step S502: coating a light anti-reflection film stack layer on the first light cutoff film stack layer.
[0085] The light anti-reflection film stack includes at least one third material film layer and at least one fourth material film layer alternately attached, the refractive index of the third material film layer is higher than the refractive index of the fourth material film layer; the light anti-reflection film stack is used to increase the transmittance of light in the second wavelength range of the incident light.
[0086] Step S503: coating a second light-cutting film stack layer on the reverse side of the first substrate.
[0087] Among them, the second light-cutting film stack includes at least one fifth material film layer and at least one sixth material film layer alternately attached, and the refractive index of the fifth material film layer is higher than the refractive index of the sixth material film layer; the second light-cutting film stack is used to cut off light in the third wavelength range of the incident light.
[0088] Among them, the sixth material film layer and the fifth material film layer are alternately plated on the reverse side of the first substrate; the reason for firstly plating the sixth material film layer on the surface of the first substrate is that, on the one hand, the sixth material film layer can effectively prevent the metal ions in the substrate material from diffusing into the optical film layer and affecting the optical properties, and on the other hand, it can also increase the adhesion.
[0089] Step S504, bonding the plated first substrate to the battery assembly.
[0090] The second light-cutoff film stack layer of the first substrate may be bonded to the battery assembly through a packaging adhesive film.
[0091] The top layer of the second light cutoff film stack is the fourth material film layer, which is used to match the POE material in the battery assembly and reduce the interface reflectivity. The refractive index of the POE material is similar to that of the fourth material film layer. According to the reflectivity calculation formula R=(n0-n1) 2 / (n0+n1) 2 It can be seen that after packaging, the interface reflectivity can be effectively reduced, n0 represents the refractive index of the packaging film, n1 represents the refractive index of the fourth material layer, which increases the incident light entering the battery component and increases the power generation of the component.
[0092] Step S505 , coating a heat dissipation material film layer on the lower surface of the second substrate.
[0093] Step S506, bonding the second substrate and the battery assembly together.
[0094] Wherein, the second substrate is bonded to the bottom electrode of the battery assembly.
[0095] It can be seen that in this example, infrared rays can be cut off by the first light-cutting film stack layer, ultraviolet rays can be cut off by the second light-cutting film stack layer, and the transmittance of visible light can be increased by the light-enhancing film stack layer, which is beneficial to improving the stability and performance of the photovoltaic cell.
[0096] See also Figure 6 , Figure 6 It is a schematic diagram of a material film layer provided in an embodiment of the present application, wherein the first light cutoff film stack layer includes a first material film layer and a second material film layer, the second light cutoff film stack layer includes a fifth material film layer and a sixth material film layer, and the light anti-reflection film stack layer includes a third material film layer and a fourth material film layer; wherein the first substrate is connected to the second material film layer of the first light cutoff film stack layer, the first substrate is connected to the sixth material film layer of the second light cutoff film stack layer, the top layer of the second light cutoff film stack layer is the sixth material film layer to match the packaging film connected to the battery assembly, and the first material film layer of the top layer of the first light cutoff film stack layer is connected to the fourth material film layer of the bottom layer of the light anti-reflection film stack layer.
[0097] In a possible example, the battery assembly includes an encapsulation film, a top electrode, an electron transport layer, a light absorption layer, a hole transport layer, a bottom electrode and butyl rubber;
[0098] The top electrode is connected to the packaging film and the electron transport layer respectively; the light absorption layer is connected to the electron transport layer and the hole transport layer respectively; the bottom electrode is connected to the hole transport layer;
[0099] The packaging adhesive film and the butyl adhesive are used to seal the battery assembly.
[0100] In a possible example, a hemispherical protrusion is formed on the lower surface of the second substrate.
[0101] In a possible example, the photovoltaic cell includes a heat dissipation material film layer; the heat dissipation material film layer is arranged on the lower surface of the second substrate.
[0102] In a possible example, the photovoltaic cell includes a polymer material layer; the polymer material layer is deposited on an upper surface of the light anti-reflection film stack.
[0103] In a possible example, the first wavelength range is 800-1500 nm, the second wavelength range is 380-760 nm, and the third wavelength range is 330-380 nm.
[0104] In a possible example, the first material film layer includes at least one of the following: TiO2, CeO2, Nb2O5, SiN m 、SiO xN y and ZnO, the second material film layer includes at least one of the following: SiO2 and MgF2. The third material film layer includes at least one of the following: Nb2O5, Si3N4, SiON x , SnO2, the fourth material film layer includes: SiO2;
[0105] The fifth material film layer includes at least one of the following: TiO2, CeO2, Nb2O5, SnO2, SiN m 、SiO x N y , ZnO, and the sixth material film layer includes at least one of the following: SiO2 and MgF2.
[0106] In a possible example, the molar ratio of Ce to Ti in the first material film layer ranges from 0.95:1 to 1.05:1.
[0107] It should be noted that all relevant contents of each step involved in the above method embodiment can be referred to the functional description of the corresponding functional module and will not be repeated here.
[0108] The electronic device provided in this embodiment is used to execute the above-mentioned method for preparing the photovoltaic cell, and thus can achieve the same effect as the above-mentioned implementation method.
[0109] In the case of an integrated unit, the electronic device may include a processing module, a storage module and a communication module. The processing module may be used to control and manage the actions of the electronic device, for example, it may be used to support the electronic device to execute the steps performed by the above-mentioned functional unit. The storage module may be used to support the electronic device to execute stored program codes and data, etc. The communication module may be used to support the communication between the electronic device and other devices.
[0110] Among them, the processing module can be a processor or a controller. It can implement or execute various exemplary logic boxes, modules and circuits described in conjunction with the disclosure of this application. The processor can also be a combination that implements computing functions, such as a combination of one or more microprocessors, a combination of digital signal processing (DSP) and a microprocessor, etc. The storage module can be a memory. The communication module can specifically be a device that interacts with other electronic devices, such as a radio frequency circuit, a Bluetooth chip, a Wi-Fi chip, etc.
[0111] An embodiment of the present application also provides a computer storage medium, wherein the computer storage medium stores a computer program for electronic data exchange, wherein the computer program enables a computer to execute part or all of the steps of any method recorded in the above method embodiments, and the above computer includes a terminal device.
[0112] The present application also provides a computer program product, which includes a non-transitory computer-readable storage medium storing a computer program, and the computer program is operable to cause a computer to execute some or all of the steps of any method described in the method embodiment. The computer program product may be a software installation package, and the computer includes a control platform.
[0113] It should be noted that, for the aforementioned method embodiments, for the sake of simplicity, they are all expressed as a series of action combinations, but those skilled in the art should be aware that the present application is not limited by the described order of actions, because according to the present application, certain steps can be performed in other orders or simultaneously. Secondly, those skilled in the art should also be aware that the embodiments described in the specification are all preferred embodiments, and the actions and modules involved are not necessarily required by the present application.
[0114] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.
[0115] In the several embodiments provided in the present application, it should be understood that the disclosed device can be implemented in other ways. For example, the device embodiments described above are only schematic, such as the division of the above-mentioned units, which is only a logical function division. There may be other division methods in actual implementation, such as multiple units or components can be combined or integrated into another system, or some features can be ignored or not executed. Another point is that the mutual coupling or direct coupling or communication connection shown or discussed can be through some interfaces, and the indirect coupling or communication connection of devices or units can be electrical or other forms.
[0116] The units described above as separate components may or may not be physically separated, and the components shown as units may or may not be physical units, that is, they may be located in one place or distributed on multiple network units. Some or all of the units may be selected according to actual needs to achieve the purpose of the solution of this embodiment.
[0117] In addition, each functional unit in each embodiment of the present application may be integrated into one processing unit, or each unit may exist physically separately, or two or more units may be integrated into one unit. The above-mentioned integrated unit may be implemented in the form of hardware or in the form of software functional units.
[0118] If the above-mentioned integrated unit is implemented in the form of a software functional unit and sold or used as an independent product, it can be stored in a computer-readable memory. Based on this understanding, the technical solution of the present application, or the part that contributes to the prior art, or all or part of the technical solution can be embodied in the form of a software product. The computer software product is stored in a memory, including a number of instructions to enable a computer device (which can be a personal computer, server or network device, etc.) to execute all or part of the steps of the above-mentioned methods in each embodiment of the present application. The aforementioned memory includes: U disk, read-only memory (ROM, Read-Only Memory), random access memory (RAM, Random Access Memory), mobile hard disk, disk or optical disk and other media that can store program codes.
[0119] A person skilled in the art can understand that all or part of the steps in the various methods of the above embodiments can be completed by instructing related hardware through a program, and the program can be stored in a computer-readable memory, which can include: a flash drive, a read-only memory, a random access memory, a magnetic disk or an optical disk, etc.
[0120] The embodiments of the present application are introduced in detail above. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method and core idea of the present application. At the same time, for general technical personnel in this field, according to the idea of the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.
Claims
1. A photovoltaic cell, characterized in that: The photovoltaic cell comprises: a first substrate; a first light-cutting film stack layer, the first light-cutting film stack layer being arranged on the front surface of the first substrate; the first light-cutting film stack layer comprising at least one first material film layer and at least one second material film layer attached alternately, the refractive index of the first material film layer being higher than the refractive index of the second material film layer; the first light-cutting film stack layer being used for cutting off light in a first wavelength range of incident light, the second material film layer being connected to the front surface of the first substrate, the first wavelength range being 800-1500nm; A light anti-reflection film stack, the light anti-reflection film stack is arranged on the upper surface of the first light cut-off film stack, the light anti-reflection film stack includes at least one third material film layer and at least one fourth material film layer alternately attached, the refractive index of the third material film layer is higher than the refractive index of the fourth material film layer; the light anti-reflection film stack is used to increase the transmittance of light in a second wavelength range of the incident light, the second wavelength range is 380-760nm; a second light-cutting film stack layer, the second light-cutting film stack layer being arranged on the reverse side of the first substrate, the second light-cutting film stack layer comprising at least one fifth material film layer and at least one sixth material film layer attached alternately, the refractive index of the fifth material film layer being higher than the refractive index of the sixth material film layer; the second light-cutting film stack layer is used for cutting off light in a third wavelength range of the incident light, the sixth material film layer being connected to the reverse side of the first substrate, the third wavelength range being 330-380 nm; A battery assembly, wherein the battery assembly is arranged on the lower surface of the second light-cutting film stack layer, and the battery assembly is a perovskite assembly; The thickness of the first light cutoff film stack layer is in the range of 3.4-3.6um, the thickness of the light anti-reflection film stack layer is in the range of 0.5-0.8um, and the thickness of the second light cutoff film stack layer is in the range of 1.0-1.6um. The total number of layers of the first material film layer and the second material film layer is in the range of 18-26 layers, the total number of layers of the third material film layer and the fourth material film layer is in the range of 4-8 layers, the total number of layers of the fifth material film layer and the sixth material film layer is in the range of 6-12 layers, and the top layer of the second light cutoff film stack layer is the fourth material film layer; The fifth material film layer includes at least one of the following: TiO2, CeO2, Nb2O5, SnO2, SiNm, SiOxNy, ZnO, the sixth material film layer includes at least one of the following: SiO2 and MgF2, and the molar ratio of Ce to Ti in the fifth material film layer ranges from 0.95:1 to 1.05:1; A second substrate is connected to the battery assembly; a hemispherical protrusion is formed on the lower surface of the second substrate, and the hemispherical protrusion is used to radiate light in a fourth wavelength range, wherein the minimum value in the fourth wavelength range is greater than 1500nm.
2. The photovoltaic cell according to claim 1, characterized in that: The battery assembly includes an encapsulation film, a top electrode, an electron transport layer, a light absorption layer, a hole transport layer, a bottom electrode and butyl rubber; The top electrode is connected to the packaging film and the electron transport layer respectively; the light absorption layer is connected to the electron transport layer and the hole transport layer respectively; the bottom electrode is connected to the hole transport layer; The packaging adhesive film and the butyl adhesive are used to seal the battery assembly.
3. The photovoltaic cell according to claim 1, characterized in that: The photovoltaic cell includes a film layer of heat dissipation material; The heat dissipation material film layer is arranged on the lower surface of the second substrate.
4. The photovoltaic cell according to claim 1, characterized in that: The photovoltaic cell comprises a polymer material layer; The polymer material layer is deposited on the upper surface of the light anti-reflection film stack.
5. The photovoltaic cell according to claim 1, characterized in that: The first material film layer includes at least one of the following: TiO2, CeO2, Nb2O5, SiN m 、SiO x N y and ZnO, the second material film layer comprises at least one of the following: SiO2 and MgF2; The third material film layer includes at least one of the following: Nb2O5, Si3N4, SiON x , SnO2, and the fourth material film layer includes: SiO2.
6. A method for preparing a photovoltaic cell, characterized in that: include: A first light-cutting film stack is plated on the front surface of the first substrate, wherein the first light-cutting film stack comprises at least one first material film layer and at least one second material film layer which are alternately attached, wherein the refractive index of the first material film layer is higher than the refractive index of the second material film layer; the first light-cutting film stack is used to cut off light in a first wavelength range in incident light, and the second material film layer is connected to the front surface of the first substrate, wherein the range of the first wavelength range is 800-1500nm; A light anti-reflection film stack is plated on the first light cut-off film stack, wherein the light anti-reflection film stack comprises at least one third material film layer and at least one fourth material film layer alternately attached, wherein the refractive index of the third material film layer is higher than the refractive index of the fourth material film layer; the light anti-reflection film stack is used to increase the transmittance of light in a second wavelength range of the incident light, wherein the second wavelength range is 380-760 nm; A second light-cutting film stack is plated on the reverse side of the first substrate, the second light-cutting film stack comprises at least one fifth material film layer and at least one sixth material film layer alternately attached, the refractive index of the fifth material film layer is higher than the refractive index of the sixth material film layer; the second light-cutting film stack is used to cut off light in a third wavelength range of the incident light, the sixth material film layer is connected to the reverse side of the first substrate, and the third wavelength range is 330-380nm; Bonding the plated first substrate to the battery assembly; Plating a heat dissipation material film layer on the lower surface of the second substrate; The second substrate is bonded to the battery assembly, wherein the battery assembly is a perovskite assembly, and a hemispherical protrusion is formed on the lower surface of the second substrate, wherein the hemispherical protrusion is used to radiate light in a fourth wavelength range, wherein the minimum value in the fourth wavelength range is greater than 1500 nm; The thickness of the first light cutoff film stack layer is in the range of 3.4-3.6um, the thickness of the light anti-reflection film stack layer is in the range of 0.5-0.8um, and the thickness of the second light cutoff film stack layer is in the range of 1.0-1.6um. The total number of layers of the first material film layer and the second material film layer is in the range of 18-26 layers, the total number of layers of the third material film layer and the fourth material film layer is in the range of 4-8 layers, and the total number of layers of the fifth material film layer and the sixth material film layer is in the range of 6-12 layers; The fifth material film layer includes at least one of the following: TiO2, CeO2, Nb2O5, SnO2, SiNm, SiOxNy, ZnO, the sixth material film layer includes at least one of the following: SiO2 and MgF2, and the molar ratio of Ce and Ti in the fifth material film layer ranges from 0.95:1 to 1.05:
1.
7. The method according to claim 6, characterized in that The method of coating a first light-cutting film stack layer on the front surface of the first substrate comprises: The second material film layer and the first material film layer are alternately plated on the front surface of the first substrate.