Array substrate and preparation method thereof, and display panel
By increasing the defect state density of the edge part on the array substrate, the opening of the edge thin film transistor is suppressed, and the camel effect and sub-threshold electrical properties of the low-temperature polysilicon thin film transistor are solved, and the charging capacity of the product is improved.
Patent Information
- Application Number
- CN202411178911.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-27
AI Technical Summary
Low-temperature polycrystalline silicon thin film transistors have problems such as camel effect and poor electrical properties in the subthreshold region, resulting in limited charging capacity of high-spec products.
By designing the defect state density of the edge part on the array substrate is greater than that of the main body part, the defect state density of the edge part is significantly increased by ion bombardment, thereby suppressing the opening of the edge thin film transistor under the same gate voltage and reducing the camel effect.
It effectively improves the camel effect of thin film transistors, improves the electrical properties of thin film transistors, and enhances the charging ability of high-spec products.
Smart Images

Figure CN118695682B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of display technology, and in particular to an array substrate and a display panel. Background Art
[0002] Low-temperature polysilicon thin-film transistors are key components for active drive and peripheral circuits of display devices such as liquid crystal displays and organic light-emitting diodes. At present, low-temperature polysilicon thin-film transistors have a hump effect, and the electrical properties of the subthreshold region are poor, which limits the charging capacity of high-specification products; the cause of the hump effect: the low-temperature polysilicon thin-film transistors manufactured by the current process can be regarded as consisting of edge thin-film transistors on both sides and a main thin-film transistor in the middle in parallel. The threshold voltage (Vth) of the edge thin-film transistor is negative relative to the main thin-film transistor, resulting in an abnormal increase in the subthreshold current of the main thin-film transistor. Summary of the invention
[0003] The embodiments of the present application provide an array substrate and a method for manufacturing the same, as well as a display panel, which can reduce the risk of a hump effect in a thin film transistor.
[0004] On the one hand, an embodiment of the present application provides an array substrate, which includes:
[0005] substrate; and
[0006] A thin film transistor, arranged on the substrate, the thin film transistor comprising an active layer, a gate insulating layer, a gate, a source electrode and a drain electrode, the active layer comprising a channel, a first contact portion and a second contact portion, the channel comprising a main portion and an edge portion, the gate insulating layer at least covers a side of the channel away from the substrate, the gate is arranged on a side of the gate insulating layer away from the substrate, the source electrode is connected to the first contact portion, and the drain electrode is connected to the second contact portion;
[0007] In a plan view of the array substrate, one of the edge portions is located at one side of the main body portion;
[0008] Wherein, in the second direction, the edge portion has a slope angle less than 90 degrees; and the defect state density of the edge portion is greater than the defect state density of the main body portion.
[0009] Optionally, in some embodiments of the present application, the defect state density of the edge portion is greater than or equal to 5 times the defect state density of the main portion.
[0010] Optionally, in some embodiments of the present application, the defect state density of the main body is between 1×10 20 / eV to 3×10 20 Between / eV.
[0011] Optionally, in some embodiments of the present application, the carrier mobility of the edge portion is less than the carrier mobility of the main portion.
[0012] Optionally, in some embodiments of the present application, the material of the channel includes polysilicon, and the crystallinity of the edge portion is less than that of the main portion.
[0013] Optionally, in some embodiments of the present application, the slope angle of the edge portion is between 30 degrees and 80 degrees.
[0014] Optionally, in some embodiments of the present application, the thickness of the main body is between 300 angstroms and 600 angstroms.
[0015] Optionally, in some embodiments of the present application, one edge portion is located on one side of the main body portion, and the other edge portion is located on the other side of the main body portion.
[0016] Optionally, in some embodiments of the present application, in a planar view of the array substrate, in a first direction, the first contact portion, the channel, and the second contact portion are arranged in sequence; in a second direction perpendicular to the first direction, one edge portion is located on one side of the main body portion, and the other edge portion is located on the other side of the main body portion.
[0017] Optionally, in some embodiments of the present application, the array substrate further includes a light-shielding layer, a buffer layer, an interlayer dielectric layer, a planarizing layer and a pixel electrode, the light-shielding layer is located on the substrate, the buffer layer covers the light-shielding layer and the substrate, the active layer is arranged on a side of the buffer layer away from the substrate, the gate insulating layer covers the active layer, the interlayer dielectric layer covers the gate, the source and the drain are arranged on a side of the interlayer dielectric layer away from the substrate, the planarizing layer covers the source and the drain, the pixel electrode is arranged on a side of the planarizing layer away from the substrate, and the pixel electrode is connected to the source or the drain.
[0018] On the other hand, an embodiment of the present application further provides a method for preparing an array substrate, which comprises the following steps:
[0019] forming a semiconductor layer and a photoresist layer in sequence on a substrate;
[0020] patterning the photoresist layer to form a photoresist pattern;
[0021] Using the photoresist pattern as a mask, etching the semiconductor layer to form an active layer, wherein the active layer includes a channel, a first contact portion and a second contact portion, wherein the channel includes a main portion and an edge portion, wherein the edge portion has a slope angle less than 90 degrees, wherein the main portion is covered by the photoresist pattern and the edge portion is exposed;
[0022] Using the photoresist pattern as a mask, bombarding the edge of the active layer with ions so that the defect state density of the edge is greater than the defect state density of the main body;
[0023] Removing the photoresist pattern, and sequentially forming a gate insulating layer and a gate on the active layer, wherein the gate insulating layer at least covers a side of the channel away from the substrate, and the gate is disposed on a side of the gate insulating layer away from the substrate;
[0024] A source electrode and a drain electrode insulated from the gate electrode are formed on the gate electrode, the source electrode is connected to the first contact portion, and the drain electrode is connected to the second contact portion.
[0025] Optionally, in some embodiments of the present application, the activity of the ions is less than that of oxygen plasma.
[0026] On the other hand, an embodiment of the present application further provides a display panel, which includes the array substrate as described in any one of the above embodiments.
[0027] The array substrate of the embodiment of the present application includes a thin film transistor, which includes an active layer, a gate insulating layer, a gate, a source and a drain. The active layer includes a channel, a first contact portion and a second contact portion. The channel includes a main body portion and an edge portion. The gate insulating layer at least covers a side of the channel away from the substrate. The gate is arranged on a side of the gate insulating layer away from the substrate. The source is connected to the first contact portion, and the drain is connected to the second contact portion. The edge portion has a slope angle less than 90 degrees. The defect state density of the edge portion is greater than the defect state density of the main body portion.
[0028] The embodiment of the present application adopts a setting in which the defect state density of the edge portion is greater than the defect state density of the main portion. Since the defect state density of the edge portion is larger, the edge portion is more difficult to turn on under the same gate voltage, and the edge thin film transistor is suppressed, thereby achieving the effect of improving the hump effect of the thin film transistor. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 is a partial plan view of an array substrate provided by one or more embodiments of the present application;
[0030] Figure 2 yes Figure 1 Schematic diagram of the cross-sectional structure along line AA;
[0031] Figure 3 yes Figure 1 Schematic diagram of the cross-sectional structure along line BB;
[0032] Figure 4is a schematic flow chart of a method for preparing an array substrate provided in an embodiment of the present application;
[0033] Figure 5 is a schematic diagram of step B1 of the method for preparing an array substrate provided in an embodiment of the present application;
[0034] Figure 6 is a schematic diagram of step B2 of the method for preparing an array substrate provided in an embodiment of the present application;
[0035] Figure 7 is a schematic diagram of step B3 of the method for preparing an array substrate provided in an embodiment of the present application;
[0036] Figure 8 is a schematic diagram of step B4 of the method for preparing an array substrate provided in an embodiment of the present application;
[0037] Figure 9a is a schematic diagram of step B51 of the method for preparing an array substrate provided in an embodiment of the present application;
[0038] Figure 9b is a schematic diagram of step B52 of the method for preparing an array substrate provided in an embodiment of the present application;
[0039] Fig.9c is a schematic diagram of step B53 of the method for preparing an array substrate provided in an embodiment of the present application;
[0040] Fig.10 is a schematic diagram of step B6 of the method for preparing an array substrate provided in an embodiment of the present application;
[0041] Fig.11 is a schematic diagram of step B7 of the method for preparing an array substrate provided in an embodiment of the present application;
[0042] Fig.12 1 is a comparison diagram of transfer curves of thin film transistors of comparative example 1, comparative example 2 and the experimental example of the present application at a drain voltage Vd=0.1V and a drain voltage Vd=10V;
[0043] Fig.13 It is a schematic diagram of the structure of the display panel provided in the embodiment of the present application. DETAILED DESCRIPTION
[0044] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present application. In addition, it should be understood that the specific implementation methods described herein are only used to illustrate and explain the present application, and are not used to limit the present application. In the present application, the various embodiments can be combined with each other but will not be repeated one by one, and in the absence of contrary instructions, the directional words used, such as "upper" and "lower", usually refer to the upper and lower parts of the device in actual use or working state, specifically the drawing direction in the drawings; while "inside" and "outside" refer to the outline of the device; the terms "first", "second", "third", etc. are used only as markings, and no numerical requirements are imposed or order is established.
[0045] The embodiments of the present application provide an array substrate and a method for manufacturing the same, as well as a display panel, which are described in detail below. It should be noted that the description order of the following embodiments is not intended to limit the preferred order of the embodiments.
[0046] Please refer to Figures 1 to 3 , Figure 1 is a partial plan view of an array substrate provided by one or more embodiments of the present application, Figure 2 yes Figure 1 The cross-sectional structure diagram along the AA line is shown in the figure. Figure 3 yes Figure 1 Schematic diagram of the cross-sectional structure along line BB.
[0047] exist Figures 1 to 3 In the embodiment, the first direction DR1 may be a direction parallel to one side of the array substrate 100 in a plan view, for example, it may be a longitudinal direction of the array substrate 100, but is not limited thereto. The second direction DR2 may be a direction parallel to the other side of the array substrate 100 in a plan view, for example, it may be a transverse direction of the array substrate 100, but is not limited thereto. The third direction DR3 may be a thickness direction of the array substrate 100.
[0048] One or more embodiments of the present application provide an array substrate 100, which includes a substrate su and a thin film transistor tft. The thin film transistor tft is disposed on the substrate su.
[0049] The thin film transistor tft includes an active layer py, a gate insulating layer gi, a gate g01, a source s01 and a drain d01. The active layer py includes a channel gd, a first contact portion p1 and a second contact portion p2. The channel gd includes a main portion gd1 and an edge portion gd2. The gate insulating layer gi at least covers a side of the channel gd away from the substrate su. The gate g01 is disposed on a side of the gate insulating layer gi away from the substrate su. The source s01 is connected to the first contact portion p1, and the drain d01 is connected to the second contact portion p2.
[0050] Figure 1 The diagram is only a plan view of an embodiment of the present application, but is not limited thereto. Figure 1 In the plan view of the array substrate 100, in the first direction DR1, the first contact portion p1, the channel gd and the second contact portion p2 are arranged in sequence; in the second direction DR2 perpendicular to the first direction DR1, an edge portion gd2 is located on one side of the main body portion gd1.
[0051] In the second direction DR2 , the edge portion gd2 has a slope angle α less than 90 degrees. The defect state density of the edge portion gd2 is greater than the defect state density of the main portion gd1 .
[0052] The embodiment of the present application adopts a setting in which the defect state density of the edge portion gd2 is greater than the defect state density of the main portion gd1. Since the defect state density of the edge portion gd2 is larger, the edge portion gd2 is more difficult to turn on under the same gate voltage, and the edge thin film transistor is suppressed, thereby achieving the effect of improving the hump effect of the thin film transistor TFT.
[0053] It needs to be explained that defect state density is a concept in the energy band theory of semiconductor physics. When a semiconductor deviates from an ideal crystal (due to various defects), electron orbits (energy states) will be generated in the band gap. The state density refers to the number of energy states in a unit energy interval in the energy band.
[0054] Among them, the defect state density can be measured by deep energy level transient spectroscopy and charge pump method, and can also be indirectly measured by X-ray diffraction testing of crystallinity.
[0055] For example, the testing method of deep energy level transient spectroscopy is: first, non-equilibrium carriers are injected into the semiconductor material, and then light excitation or electric field excitation is used to make the carriers transition to the conduction band or valence band, and then the changes in the spectrum are measured to study the electron transition process and the properties of deep energy level defects.
[0056] For example, the charge-pumping technique can be referred to in the literature "Local oxide capacitance as a crucial parameter for characterization of hot-carrier degradation in long-channel n-MOSFETs", author: I Starkov, H Enichlmair; journal name: Journal of Vacuum Science & Technology. B, Microelectronics and Nanometer Structures: Processing, Measurement, and Phenomena; journal volume number: 31; start and end page numbers: 1180-1187; publication date: 2013; DOI: 10.1116 / 1.4774106.
[0057] Also, please refer to Figure 1 The thin film transistor tft includes a main thin film transistor t1 and edge thin film transistors t2 located on both sides of the main thin film transistor t1. The main thin film transistor t1 and the edge thin film transistor t2 have a common gate, a common source and a common drain. The channel of the main thin film transistor t1 is the main part gd1, and the channel of the edge thin film transistor t2 is the edge part gd2.
[0058] Optionally, the thin film transistor tft may be an N-type thin film transistor or a P-type thin film transistor.
[0059] In the thin film transistor TFT disclosed in the embodiment of the present application, the embodiment of the present application is explained by taking the gate g01 as a metal layer, and the source s01 and the drain d01 as the same metal layer as an example, but is not limited to this. For example, the gate g10, the source s01 and the drain d01 can be set in the same layer, that is, they are prepared and formed using the same mask template; or one of the source s01 and the drain d01 can be set in the same layer as the gate g01; or all three can be set in different layers.
[0060] It should be understood that the array substrate 100 of the embodiment of the present application is used for a liquid crystal panel. The array substrate 100 of the embodiment of the present application can be based on a fringe field switching (Fringe Field Switching, FFS) technology driving architecture, can be based on a plane switching (In-Plane Switching, IPS) technology driving architecture, can be based on a vertical alignment (Vertical Alignment, VA) technology driving architecture, and so on.
[0061] In some embodiments, the array substrate 100 may also be used for an electroluminescent display panel, such as an organic light emitting diode display panel, a micro light emitting diode display panel, a sub-millimeter light emitting diode display panel, or a quantum dot light emitting diode display panel, etc. In addition, in other embodiments, the array substrate 100 may also be used for an electrophoretic panel, etc.
[0062] The array substrate 100 of the embodiment of the present application is described below based on the FFS architecture, but is not limited thereto.
[0063] Please refer to Figure 2 and Figure 3 In one or more embodiments of the present application, the array substrate 100 further includes a light shielding layer Ls, a buffer layer buf, an interlayer dielectric layer Ld, a planarization layer Pn and a pixel electrode pix.
[0064] The light shielding layer Ls is located on the substrate su. The buffer layer buf covers the light shielding layer Ls and the substrate su. The active layer py is arranged on the side of the buffer layer buf away from the substrate su. The gate insulating layer gi covers the active layer py, and the interlayer dielectric layer Ld covers the gate g01. The source s01 and the drain d01 are arranged on the side of the interlayer dielectric layer Ld away from the substrate su. The planar layer Pn covers the source s01 and the drain d01, and the pixel electrode pix is arranged on the side of the planar layer Pn away from the substrate su. The pixel electrode pix is connected to the source s01 or the drain d01.
[0065] Optionally, in one or more embodiments, the array substrate 100 may further include a common electrode layer com and a passivation layer Pv, wherein the common electrode layer com is disposed on a side of the flat layer Pn away from the substrate su. The passivation layer Pv covers the common electrode layer com. The pixel electrode pix is disposed on a side of the passivation layer Pv away from the substrate su.
[0066] Optionally, in some embodiments, the substrate su may be a rigid substrate or a flexible substrate. The material of the substrate su includes one of glass, sapphire, silicon, silicon dioxide, polyethylene, polypropylene, polystyrene, polylactic acid, polyethylene diphthalate, polyethylene terephthalate, polyethylene naphthalate, polycarbonate, polyether sulfone, aromatic fluorotoluene containing polyarylate, polycyclic olefin, polyimide or polyurethane.
[0067] In some embodiments, the material of the light shielding layer Ls may be an inorganic metal material, such as chromium, molybdenum, manganese, etc., or a metal oxide material, such as CrO x 、MoO x 、MnO 2 etc., or a mixed film layer formed by metal and metal oxide; it can also be an organic black resin material, such as black polystyrene, black photoresist, etc.
[0068] In some embodiments, the buffer layer buf, the gate insulating layer gi, the interlayer dielectric layer Ld and the passivation layer Pv may be formed by a plurality of inorganic layers stacked in an alternating manner. For example, the buffer layer buf, the gate insulating layer gi, the interlayer dielectric layer Ld and the passivation layer Pv may be formed as a double layer formed by stacking an inorganic layer including at least one of silicon oxide, silicon nitride, silicon oxynitride, aluminum oxide, magnesium oxide and titanium oxide, or a multilayer formed by alternately stacking an inorganic layer including at least one of silicon oxide, silicon nitride, silicon oxynitride, aluminum oxide, magnesium oxide and titanium oxide. However, the present disclosure is not limited thereto, and the buffer layer buf, the gate insulating layer gi, the interlayer dielectric layer Ld and the passivation layer Pv may be formed as a single inorganic layer including the above-mentioned insulating material.
[0069] Furthermore, in one or more embodiments, the interlayer dielectric layer Ld may be made of an organic insulating material such as polyimide (PI).
[0070] In some embodiments, the material of the active layer py may include polycrystalline silicon or single crystal silicon. The first contact p1 and the second contact p2 are N-type contacts. The first contact p1 and the second contact p2 each include a heavily doped region and a lightly doped region. The heavily doped region is located on a side of the lightly doped region away from the channel gd. The source s01 is connected to the heavily doped region of the first contact p1, and the drain d01 is connected to the heavily doped region of the second contact p2.
[0071] In some embodiments, the gate g01, the source s01 and the drain d01 may be formed using a metal element selected from chromium, copper, aluminum, gold, silver, zinc, molybdenum, tantalum, titanium, tungsten, manganese, nickel, iron, neodymium, cobalt, an alloy containing any of the above metal elements as a component, or an alloy combining any of the above metal elements, etc. In addition, the gate, source and drain may have a single-layer structure or a stacked structure of two or more layers.
[0072] In some embodiments, the material of the planar layer Pn may be an organic transparent film layer, such as transparent photoresist, acrylic resin, epoxy resin, phenolic resin, polyamide resin or polyimide resin.
[0073] In some embodiments, the material of the pixel electrode pix and the common electrode layer com can be oxides such as indium tin oxide and indium zinc oxide; it can also be metals, alloys, compounds and mixtures thereof with various conductive properties, such as gold, silver or platinum.
[0074] In one or more embodiments of the present application, the thickness of the edge portion gd2 is gradually changing, and the thickness of the main body gd1 is uniform. The thickness of the edge portion gd2 increases gradually from the edge of the edge portion gd2 to the main body gd1.
[0075] It should be understood that the increasing thickness of the edge portion gd2 does not mean that the thickness of the edge portion gd2 increases by 100%, because due to the limitation of the process technology, the thickness of the edge portion gd2 cannot be 100% accurate. Also based on the limitation of the process technology, the thickness of the main body gd1 tends to be uniform, that is, the thickness of the main body gd1 is generally uniform.
[0076] In one or more embodiments of the present application, the defect state density of the edge portion gd2 is greater than or equal to 5 times the defect state density of the main portion gd1.
[0077] It should be understood that the greater the defect state density of the edge portion gd2, the better the effect of suppressing the turning on of the edge thin film transistor t2, thereby suppressing the hump effect; otherwise, the worse.
[0078] Therefore, in order to significantly suppress the hump effect, the defect state density of the edge portion gd2 is selected to be greater than or equal to 5 times the defect state density of the main portion gd1.
[0079] For example, the defect state density of the edge portion gd2 may be 5 times, 6 times, 7 times, 8 times, 9 times, or 10 times the defect state density of the main portion gd1.
[0080] In some embodiments of the present application, the defect state density of the main body gd1 is between 1×10 20 / eV (electron volt) to 3×10 20 / eV, for example, it can be 1×10 20 / eV, 2×10 20 / eV or 3×10 20 / eV, and so on.
[0081] In some embodiments of the present application, the carrier mobility of the edge portion gd2 is smaller than the carrier mobility of the main portion gd1.
[0082] It can be understood that the carrier mobility of the edge portion gd2 is relatively small, which prolongs the time for the carriers to transit the base region, reduces the switching speed of the thin film transistor, and thus inhibits the turning on of the edge thin film transistor t2.
[0083] In some embodiments of the present application, the material of the channel gd includes polysilicon, and the crystallinity of the edge portion gd2 is less than that of the main portion gd1.
[0084] It is understood that the crystallinity of the channel refers to the order of the lattice structure arrangement inside the polysilicon material. Low crystallinity means that there are a large number of grain boundaries, defects and disordered structures in the material.
[0085] In the embodiment of the present application, the defect degree of the edge portion gd2 is greater than that of the main portion gd1. The increase in defects reduces the migration speed of the carrier channel, which means that a larger gate voltage is required for control at the same time. Therefore, the crystallinity of the edge portion gd2 is less than that of the main portion gd1, which can inhibit the start-up of the edge thin film transistor t2, thereby achieving the hump effect of the thin film transistor tft.
[0086] In some embodiments of the present application, the thickness of the main body portion gd1 is between 300 angstroms and 600 angstroms, for example, 300 angstroms, 350 angstroms, 400 angstroms, 450 angstroms, 500 angstroms, 550 angstroms or 600 angstroms.
[0087] It is understandable that if the thickness of the channel gd is too thin, uneven film formation will result, while if it is too thick, it will be difficult to crystallize, resulting in poor crystal quality of polysilicon. Therefore, based on the above considerations, the thickness of the channel gd is selected to be between 300 angstroms and 600 angstroms.
[0088] In some embodiments of the present application, the slope angle α of the edge portion gd2 is between 30 degrees and 80 degrees.
[0089] It should be noted that, since the thickness of the main part gd1 of the active layer py is small, if the slope angle α of the edge part gd2 is too steep, the edge part gd2 will not be easily hit by ions in the subsequent ion bombardment step, and it is difficult to make the side of the edge part gd2 close to the gate g01 have a large degree of defects. If the slope angle α is too gentle, it will take up too much space.
[0090] Therefore, considering the difficulty of forming defects in the edge portion gd2 and the space occupancy requirements, the slope angle α of the edge portion gd2 is set between 30 degrees and 80 degrees, for example, it can be 30 degrees, 35 degrees, 40 degrees, 45 degrees, 50 degrees, 55 degrees, 65 degrees, 70 degrees, 75 degrees or 80 degrees.
[0091] In some embodiments of the present application, in the second direction DR2, one edge portion gd2 is located on one side of the main portion gd1, and another edge portion gd2 is located on the other side of the main portion gd1. Of course, in some embodiments, only one edge portion gd2 may be included.
[0092] Optionally, the slope angles of the two edge portions gd2 may be the same or different, and this application does not limit this.
[0093] In some embodiments, the main body gd1 includes a first portion and a second portion, the first portion is located between the second portion and the edge portion gd2, wherein the defect state density of the first portion is between the defect state density of the edge portion gd2 and the defect state density of the second portion.
[0094] It can be understood that the first part plays a transition role, reducing the risk of mutual interference between the edge thin film transistor t2 and the main thin film transistor t1 at the moment when the thin film transistor tft is turned on.
[0095] Optional, such as Figure 3 As shown, the width of the first portion is smaller than the width of the edge portion gd2 to reduce the influence on the main thin film transistor t1.
[0096] Please refer to Figure 4 The present application also provides a method for preparing an array substrate 100, which comprises the following steps:
[0097] Step B1, forming a semiconductor layer act and a photoresist layer pr in sequence on a substrate su.
[0098] Step B2, patterning the photoresist layer pr to form a photoresist pattern pr1.
[0099] Step B3, using the photoresist pattern pr1 as a mask, etching the semiconductor layer act to form an active layer py, the active layer py including a channel gd, a first contact portion and a second contact portion, the channel gd including a main portion gd1 and an edge portion gd2, the edge portion gd2 having a slope angle α less than 90 degrees, the main portion gd1 is covered by the photoresist pattern pr1, and the edge portion gd2 is exposed.
[0100] Step B4, using the photoresist pattern pr1 as a mask, bombarding the edge portion gd2 of the active layer py with ions to make the defect state density of the edge portion gd2 greater than the defect state density of the main portion gd1.
[0101] Step B5, remove the photoresist pattern pr1, and sequentially form a gate insulating layer gi and a gate g01 on the active layer py, wherein the gate insulating layer gi at least covers the side of the channel gd away from the substrate su, and the gate g01 is arranged on the side of the gate insulating layer gi away from the substrate su.
[0102] Step B6: forming a source s01 and a drain d01 on the gate g01 to be insulated therefrom, wherein the source s01 is connected to the first contact portion p1 , and the drain d01 is connected to the second contact portion p2 .
[0103] It should be understood that the method for preparing the array substrate 100 of the embodiment of the present application uses a photoresist pattern to protect the main body gd1 of the channel gd from ion bombardment, and uses ions to bombard the edge gd2 of the channel gd, so that the defect state density of the edge gd2 is increased. Since the defect state density of the edge gd2 is greater than the defect state density of the main body gd1, under the same gate voltage, the turning on of the edge thin film transistor t2 can be suppressed, thereby suppressing the hump effect of the thin film transistor tft.
[0104] The following is based on Figures 1 to 3 The preparation method is described in the corresponding embodiments, but is not limited thereto.
[0105] Please refer to Figure 5 , step B1, forming a semiconductor layer act and a photoresist layer pr in sequence on a substrate su.
[0106] Optionally, the material of the semiconductor layer act may be polycrystalline silicon.
[0107] Optionally, before forming the semiconductor layer act on the substrate su, the method further includes forming a light shielding layer Ls and a buffer layer buf on the substrate su. The semiconductor layer act is formed on the buffer layer buf.
[0108] Then proceed to step B2.
[0109] Please refer to Figure 6 , step B2, patterning the photoresist layer pr to form a photoresist pattern pr1.
[0110] The photoresist pattern pr1 is used to form a subsequent active layer py.
[0111] Then proceed to step B3.
[0112] Please refer to Figure 7 Step B3, using the photoresist pattern pr1 as a mask, etching the semiconductor layer act to form an active layer py. The active layer py includes a channel gd, a first contact portion, and a second contact portion. The channel gd includes a main portion gd1 and an edge portion gd2. The edge portion gd2 has a slope angle α less than 90 degrees. The main portion gd1 is covered by the photoresist pattern pr1, and the edge portion gd2 is exposed.
[0113] Optionally, during the etching of the semiconductor layer act, the side edge portion of the photoresist pattern pr1 forms a structure with a slope angle, and the side surface of the side edge portion is flush with the side surface of the edge portion gd2.
[0114] Then proceed to step B4.
[0115] Please refer to Figure 8 , step B4, using the photoresist pattern pr1 as a mask, using ions to bombard the edge portion gd2 of the active layer py so that the defect state density of the edge portion gd2 is greater than the defect state density of the main portion gd1.
[0116] Optionally, the activity of the ions is less than that of oxygen plasma, such as inert gas or less reactive gas, such as Ar, Ne, Kr, Xe or N 2 .
[0117] Compared with the comparative example of bombardment using oxygen plasma, oxygen plasma is more active and reacts more chemically with silicon. + Bombardment is carried out. Since the relative atomic mass of the Ar element is large, the effect of its physical bombardment is better, which can quickly increase the defect state density of the edge gd2 and reduce the crystallinity of the edge gd2; in addition, argon is an inert gas, which has basically no chemical reaction with silicon and has few side effects.
[0118] In addition, it should be understood that, since the side portion of the photoresist pattern pr1 corresponds to and covers the side of the main body gd1 close to the edge portion gd2, and the thickness of the side portion is an increasing region, when plasma bombardment is performed, the plasma will penetrate the thinner side portion and damage the first portion of the main body gd1, and the degree of damage to the first portion of the main body gd1 is decreasing as the thickness of the side portion of the photoresist pattern pr1 increases. Based on this, the defect state density of the first portion of the main body gd1 is between the edge portion gd2 and the second portion of the main body gd1.
[0119] Of course, in some embodiments, the thickness of the side portions of the photoresist pattern pr1 is equal to the thickness of other portions, that is, the photoresist pattern pr1 has no inclined slope angle.
[0120] Then go to step B5.
[0121] Please refer to Figures 9a to 9c , step B5, remove the photoresist pattern pr1, and sequentially form a gate insulating layer gi and a gate g01 on the active layer py, wherein the gate insulating layer gi at least covers the side of the channel gd away from the substrate su, and the gate g01 is arranged on the side of the gate insulating layer gi away from the substrate su.
[0122] Optionally, after removing the photoresist pattern pr1, step B5 further includes:
[0123] Please refer to Figure 9a , step B51, performing the first light doping treatment on the entire surface of the active layer py.
[0124] Please refer to Figure 9b , step B52, performing heavy doping treatment on the heavily doped region of the active layer py.
[0125] Please refer to Fig.9c , step B53, sequentially forming a gate insulating layer gi and a gate g01 on the active layer py, and then using the gate g01 as a mask, performing a second light doping treatment on the lightly doped region of the active layer py to form a first contact portion p1, a second contact portion p2 and a channel gd.
[0126] Then go to step B6.
[0127] Please refer to Fig.10 , step B6, forming a source s01 and a drain d01 on the gate g01 and insulated therefrom, the source s01 being connected to the first contact portion p1, and the drain d01 being connected to the second contact portion p2.
[0128] Optionally, step B6 includes: forming an interlayer dielectric layer Ld on the gate g01; and then forming a source s01 and a drain d01 on the interlayer dielectric layer Ld.
[0129] In addition, the method for preparing the array substrate 100 of the embodiment of the present application further includes the following steps:
[0130] Please refer to Fig.11 Step B7: forming a planar layer Pn, a common electrode layer com, a passivation layer pv and a pixel electrode pix on the source electrode s01 and the drain electrode d01 in sequence. The pixel electrode pix is connected to the drain electrode d01 through a via hole.
[0131] Please note that, please refer to Fig.12 , Fig.12 It is a comparison diagram of transfer curves of thin film transistors of Comparative Example 1, Comparative Example 2 and the experimental embodiment of the preparation method of the present application at drain voltage Vd=0.1V and drain voltage Vd=10V.
[0132] Among them, the difference between Comparative Example 1, Comparative Example 2 and the experimental example is only whether plasma bombardment of the edge portion gd2 is used in the process. That is, the low-temperature polysilicon thin film transistor of Comparative Example 1 is a thin film transistor that is not bombarded with plasma, the low-temperature polysilicon thin film transistor of Comparative Example 2 is a thin film transistor bombarded with oxygen plasma, and the experimental example is a low-temperature polysilicon thin film transistor prepared by the preparation method of the array substrate of the embodiment of the present application, which is a thin film transistor tft bombarded with argon plasma.
[0133] according to Fig.12 It can be seen that compared with comparative example 1, regardless of the drain voltage Vd=0.1V or the drain voltage Vd=10V, comparative example 2 using oxygen plasma for bombardment has no obvious improvement on the hump effect; while the experimental examples using argon plasma for bombardment have a better improvement effect on the hump effect.
[0134] On the other hand, please refer to Fig.13 The embodiment of the present application further provides a display panel 1000, which includes the array substrate as described in any one of the above embodiments.
[0135] The display panel 1000 of the embodiment of the present application can be one of a liquid crystal panel, an electroluminescent display panel and an electrophoretic panel, for example, it can be an FFS liquid crystal display panel, an IPS liquid crystal display panel, a VA liquid crystal display panel, an organic light emitting diode display panel, a micro light emitting diode display panel, a sub-millimeter light emitting diode display panel, a quantum dot light emitting diode display panel or an electrophoretic panel, etc.
[0136] It should be noted that the structure of the thin film transistor of the array substrate 100 of the display panel 1000 of the embodiment of the present application is similar to or the same as the structure of the thin film transistor TFT of the array substrate 100 of any of the above embodiments.
[0137] Optional, Fig.13 The display panel 1000 of one embodiment of the present application is shown. The display panel 1000 is a liquid crystal panel and includes an array substrate 100 , an opposing substrate 200 disposed opposite to the array substrate 100 , and a liquid crystal layer 300 disposed between the array substrate 100 and the opposing substrate 200 .
[0138] The display panel of the embodiment of the present application includes a thin film transistor, which includes an active layer, a gate insulating layer, a gate, a source and a drain. The active layer includes a channel, a first contact portion and a second contact portion. The channel includes a main portion and an edge portion. The gate insulating layer at least covers a side of the channel away from the substrate su. The gate is arranged on a side of the gate insulating layer away from the substrate. The source is connected to the first contact portion, and the drain is connected to the second contact portion. The edge portion has a slope angle less than 90 degrees. The defect state density of the edge portion is greater than the defect state density of the main portion.
[0139] The embodiment of the present application adopts a setting in which the defect state density of the edge portion is greater than the defect state density of the main portion. Since the defect state density of the edge portion is larger, the edge portion is more difficult to turn on under the same gate voltage, and the edge thin film transistor is suppressed, thereby achieving the effect of improving the hump effect of the thin film transistor.
[0140] The above is a detailed introduction to an array substrate and a preparation method thereof, as well as a display panel provided in an embodiment of the present application. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea. At the same time, for technical personnel in this field, according to the idea of the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.
Claims
1. An array substrate, characterized in that: include: substrate; as well as A thin film transistor, arranged on the substrate, the thin film transistor comprising an active layer, a gate insulating layer, a gate, a source electrode and a drain electrode, the active layer comprising a channel, a first contact portion and a second contact portion, the channel comprising a main portion and an edge portion, the gate insulating layer at least covers a side of the channel away from the substrate, the gate is arranged on a side of the gate insulating layer away from the substrate, the source electrode is connected to the first contact portion, and the drain electrode is connected to the second contact portion; In a plan view of the array substrate, one of the edge portions is located at one side of the main body portion; Wherein, the edge portion has a slope angle less than 90 degrees; and the defect state density of the edge portion is greater than the defect state density of the main body portion.
2. The array substrate according to claim 1, characterized in that: The defect state density of the edge portion is greater than or equal to 5 times the defect state density of the main portion.
3. The array substrate according to claim 2, characterized in that: The defect state density of the main body is between 1×10 20 / eV to 3×10 20 Between / eV.
4. The array substrate according to claim 1, characterized in that: The carrier mobility of the edge portion is smaller than the carrier mobility of the main portion.
5. The array substrate according to claim 1, characterized in that: The material of the channel includes polysilicon, and the crystallinity of the edge portion is lower than that of the main portion.
6. The array substrate according to any one of claims 1 to 5, characterized in that: The slope angle of the edge portion is between 30 degrees and 80 degrees.
7. The array substrate according to claim 6, characterized in that: The thickness of the main body is between 300 angstroms and 600 angstroms.
8. The array substrate according to claim 6, characterized in that: One edge portion is located on one side of the main body portion, and the other edge portion is located on the other side of the main body portion.
9. The array substrate according to claim 8, characterized in that: In a planar view of the array substrate, in a first direction, the first contact portion, the channel and the second contact portion are arranged in sequence; in a second direction perpendicular to the first direction, one edge portion is located on one side of the main body portion, and the other edge portion is located on the other side of the main body portion.
10. The array substrate according to any one of claims 1 to 5, characterized in that: The array substrate further includes a light shielding layer, a buffer layer, an interlayer dielectric layer, a planarization layer and a pixel electrode, wherein the light shielding layer is located on the substrate, the buffer layer covers the light shielding layer and the substrate, the active layer is arranged on a side of the buffer layer away from the substrate, the gate insulating layer covers the active layer, the interlayer dielectric layer covers the gate, the source and the drain are arranged on a side of the interlayer dielectric layer away from the substrate, the planarization layer covers the source and the drain, the pixel electrode is arranged on a side of the planarization layer away from the substrate, and the pixel electrode is connected to the source or the drain.
11. A method for preparing an array substrate, characterized in that: The following steps are involved: forming a semiconductor layer and a photoresist layer in sequence on a substrate; patterning the photoresist layer to form a photoresist pattern; Using the photoresist pattern as a mask, etching the semiconductor layer to form an active layer, wherein the active layer includes a channel, a first contact portion and a second contact portion, wherein the channel includes a main portion and an edge portion, wherein the edge portion has a slope angle less than 90 degrees, wherein the main portion is covered by the photoresist pattern and the edge portion is exposed; Using the photoresist pattern as a mask, bombarding the edge of the active layer with ions so that the defect state density of the edge is greater than the defect state density of the main body; Removing the photoresist pattern, and sequentially forming a gate insulating layer and a gate on the active layer, wherein the gate insulating layer at least covers a side of the channel away from the substrate, and the gate is disposed on a side of the gate insulating layer away from the substrate; A source electrode and a drain electrode insulated from the gate electrode are formed on the gate electrode, the source electrode is connected to the first contact portion, and the drain electrode is connected to the second contact portion.
12. The method for preparing an array substrate according to claim 11, characterized in that: The activity of the ions is less than that of oxygen plasma.
13. A display panel, characterized in that: Comprising the array substrate as described in any one of claims 1-10.
