A composite film suitable for Prussian blue positive electrode material and its preparation method and application
By using bionic gel composite film in Prussian blue materials, the cycle stability problem in sodium ion batteries is solved, the stability and crystallization water balance between the electrode and electrolyte interface are achieved, the cycle life of the battery is extended and the cycle life is improved. Battery performance.
Patent Information
- Application Number
- CN202411159382.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-22
AI Technical Summary
The cyclic stability problems of Prussian blue materials in sodium ion batteries mainly stem from the instability of body phase structure and interface structure and the detachment of crystal water in the crystal lattice, resulting in structural damage and electrochemical degradation during charging and discharge of the material. .
Using a bionic gel composite film, an electrolyte membrane with high adhesion and responsiveness is prepared by loading trimethylsilicone isocyanate or 2-trifluoromethylnicotinic acid methyl ester into the polymer, which is not only It can balance crystal water and be used as a separator, simplifying the battery preparation process and reducing costs.
Effectively curb the dissolution of metal elements in Prussian blue material, ensure the stability of the interface between the electrode and the electrolyte, achieve dynamic balance of crystallization water, improve the interface stability and dynamic characteristics of the material, and extend the cycle life of sodium ion batteries. , and improves the ion transmission efficiency of the battery.
Smart Images

Figure CN118703012B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a composite film suitable for Prussian blue positive electrode material and a preparation method and application thereof, belonging to the technical field of batteries. Background Art
[0002] The shortage of lithium resources limits its application in energy storage systems. In contrast, sodium-ion batteries are comparable to lithium-ion batteries in terms of large-scale energy storage, and sodium resources are highly abundant and widely distributed geographically, which can alleviate the shortage of lithium resources. In addition, sodium-ion batteries also have the advantages of low energy storage cost per kilowatt-hour, cheap and readily available materials, simple post-operation and maintenance, and environmental friendliness.
[0003] Currently, the commonly used positive electrode materials for sodium-ion batteries include layered oxides, Prussian blue compounds and polyanion compounds. Among them, Prussian blue materials have multiple significant advantages as positive electrode materials for sodium-ion batteries, such as high theoretical capacity (up to 170 mAh / g), adjustable working voltage, large interstitial position (about 4.6 Å), low cost, non-toxic and harmless, and easy material preparation. However, the cyclic stability of Prussian blue materials has become a key bottleneck restricting their further large-scale application, mainly due to the instability of the bulk structure and interface structure and the problem of crystalline water escaping from the lattice.
[0004] In order to improve the stable cycle life of Prussian blue materials, domestic and foreign scholars have conducted a lot of research on improving the preparation process, element doping, surface coating and other structural optimization, with the aim of improving the crystallinity of the material and reducing the lattice distortion during the charge and discharge process. However, the cycle stability problem of Prussian blue materials has not been completely solved. Summary of the invention
[0005] To solve the above problems, the present invention provides a biomimetic gel composite membrane suitable for Prussian blue positive electrode materials, which can respond to and balance crystal water, has strong adhesion, and can act as a diaphragm. When an electrolyte salt is added thereto, it can act as both an electrolyte and a diaphragm, solving the effect of the release of Prussian blue crystal water on the positive electrode material interface and the electrochemical performance of the battery. More importantly, when the material is used as a diaphragm or electrolyte membrane to prepare a battery, not only the performance of the battery is improved, but also when the electrolyte membrane is used, there is no need to add additional electrolyte and / or diaphragm, which simplifies the preparation of the battery and reduces the cost.
[0006] The first object of the present invention is to provide a composite membrane, wherein the composite membrane contains a polymer and a filler loaded in the polymer;
[0007] The filler is selected from trimethylsilyl isocyanate and / or 2-trifluoromethylnicotinate;
[0008] The preparation method of the polymer comprises the following steps:
[0009] S1. Mixing the first solution and the second solution to obtain product A; wherein the solute of the first solution is selected from one or more of dopamine salt, hydroxydopamine salt, methyldopamine salt, and methoxydopamine salt, and the solute of the second solution is selected from one or more of methacrylic anhydride, polyisobutylene succinic anhydride, and ethylene bisstearic acid amide;
[0010] S2. Heat the product A of S1 and hydroxyethyl methacrylate in the presence of an initiator to obtain the polymer.
[0011] Further, the preparation method of the polymer comprises: mixing product A, hydroxyethyl methacrylate and an initiator in an organic solvent, and reacting at 40-100° C. to obtain a polymer. Preferably, the reaction temperature is 60-80° C., such as 41° C., 45° C., 50° C., 55° C., 60° C., 65° C., 70° C., 75° C., 80° C., 85° C., 90° C., 95° C., 100° C., etc., including but not limited to the temperatures listed above.
[0012] Furthermore, the method for loading the filler into the polymer comprises the steps of dissolving the polymer with a volatile solvent, mixing the obtained solution with the filler, and removing the solvent.
[0013] Furthermore, in the polymer, the molar ratio of product A to hydroxyethyl methacrylate is 1:(1-5); and the filler accounts for 0.1wt%-5wt% of the total mass of the polymer.
[0014] Furthermore, the initiator is selected from organic peroxide initiators and / or azo initiators, including but not limited to azobisisobutyronitrile, dibenzoyl peroxide, etc.
[0015] Furthermore, the amount of the initiator used is 0.1-2 wt % of the total mass of the raw materials (product A, hydroxyethyl methacrylate and initiator).
[0016] Furthermore, the preparation method of the product A is:
[0017] (1) preparing solution A by using at least one of dopamine hydrochloride, hydroxypamine hydrochloride, methylpamine hydrochloride and methoxypamine hydrochloride as solute; preparing solution B by using at least one of methacrylic anhydride, polyisobutylene succinic anhydride and ethylene bisstearic acid amide as solute;
[0018] (2) Solution A and solution B are mixed and reacted, and during the reaction, the pH of the system is adjusted to acidic to obtain the product A.
[0019] Specifically:
[0020] a) preparing solution A: adding solute A to a well-stirred buffer solution to obtain solution A. Solute A is dopamine hydrochloride, hydroxydopamine hydrochloride, methyldopamine hydrochloride, or methoxydopamine hydrochloride; wherein the pH of solution A is alkaline;
[0021] b) preparing solution B: adding solute B into an organic solvent to obtain solution B. Solute B is methacrylic anhydride, polyisobutylene succinic anhydride, and ethylene bisstearic acid amide;
[0022] c) mixing solution A with solution B;
[0023] d) stirring for 10-12 hours, adding hydrochloric acid dropwise to adjust the pH value to less than 2, and extracting with an extractant;
[0024] e) After concentration by rotary evaporation, precipitation was performed by adding a precipitant, recrystallization was performed in hexane and drying was performed under high vacuum to obtain a light grey solid.
[0025] Furthermore, in step a), the pH value of the buffer solution is 8.5-10, the solvent is deionized water, and the buffer is sodium bicarbonate, sodium tetraborate, sodium citrate, disodium hydrogen phosphate, sodium dihydrogen phosphate, etc.
[0026] Furthermore, in step b), the organic solvent is tetrahydrofuran, ethyl acetate, isobutyl ether, etc.
[0027] Further, in step b), the concentration of solution B is 15-35 wt %.
[0028] Furthermore, in step c), the mixing is: adding solution B dropwise into solution A, and the whole process is carried out under an inert atmosphere, such as argon, helium, etc.
[0029] Furthermore, in step d), the extractant is ethyl acetate, isobutanol, or acetone.
[0030] Furthermore, in step e), the precipitant is hexane, 2-methylpentane, 3-methylpentane, 2,3-dimethylbutane, or the like.
[0031] Another object of the present invention is to provide a method for preparing a composite film, comprising the following steps:
[0032] (1) mixing a first solution and a second solution to obtain a product A; wherein the solute of the first solution is selected from one or more of dopamine salts, hydroxydopamine salts, methyldopamine salts, and methoxydopamine salts, and the solute of the second solution is selected from one or more of methacrylic anhydride, polyisobutylene succinic anhydride, and ethylene bisstearic acid amide;
[0033] (2) heating the product A and hydroxyethyl methacrylate in the presence of an initiator to obtain a polymer;
[0034] (3) mixing the polymer and the filler to form a film to obtain the composite film;
[0035] The filler is selected from trimethylsilyl isocyanate and / or 2-trifluoromethylnicotinate methyl ester.
[0036] Furthermore, in step (3), the mixing includes: dissolving the polymer in a solvent, mixing with the filler, and removing the solvent after mixing evenly.
[0037] Furthermore, in step (3), the preparation of the film comprises: coating the mixture of the polymer and the filler at a set thickness, and heat treating the film at a set temperature. Preferably, the set temperature is 70-90°C. For example, 71°C, 72°C, 73°C, 74°C, 75°C, 76°C, 77°C, 78°C, 79°C, 80°C, 81°C, 82°C, 83°C, 84°C, 85°C, 86°C, 87°C, 88°C, 89°C, etc., including but not limited to the temperatures listed above.
[0038] Another object of the present invention is to provide an electrolyte membrane, comprising: the composite membrane or the composite membrane obtained by the above preparation method, and an electrolyte salt supported in the polymer.
[0039] Furthermore, the electrolyte membrane comprises at least one of the following:
[0040] (1) The mass percentage of the electrolyte salt to the polymer is 1wt%-10wt%;
[0041] (2) The mass percentage of filler to polymer is 0.1wt%-5wt%.
[0042] Another object of the present invention is to provide a method for preparing an electrolyte membrane, comprising the following steps:
[0043] (01) mixing a first solution and a second solution to obtain a product A; wherein the solute of the first solution is selected from one or more of dopamine salts, hydroxydopamine salts, methyldopamine salts, and methoxydopamine salts, and the solute of the second solution is selected from one or more of methacrylic anhydride, polyisobutylene succinic anhydride, and ethylene bisstearic acid amide;
[0044] (02) heating the product A and hydroxyethyl methacrylate in the presence of an initiator to obtain a polymer;
[0045] (03) mixing the polymer with a filler and an electrolyte salt to form a film, thereby obtaining the electrolyte membrane;
[0046] The filler is selected from trimethylsilyl isocyanate and / or 2-trifluoromethylnicotinate methyl ester.
[0047] Furthermore, the electrolyte salt includes but is not limited to sodium hexafluorophosphate, sodium bis(fluorosulfonyl)imide, sodium tetrafluoroborate, sodium perchlorate or sodium difluorophosphate.
[0048] Another object of the present invention is to provide a battery separator, which contains the composite membrane, the composite membrane obtained by the above preparation method, the electrolyte membrane or the electrolyte membrane obtained by the above preparation method.
[0049] The present invention also provides a sodium ion battery, wherein the sodium ion battery comprises:
[0050] I. A positive electrode sheet, a negative electrode sheet, an electrolyte and the above composite film or a composite film obtained by the above preparation method containing a Prussian blue positive electrode material; or
[0051] II. A positive electrode sheet and a negative electrode sheet containing a Prussian blue positive electrode material and the above electrolyte membrane or the electrolyte membrane obtained by the above preparation method.
[0052] Furthermore, the sodium ion battery contains a positive electrode sheet, a negative electrode sheet and a composite membrane. In this case, the battery system also needs to contain an organic solution (electrolyte) of electrolyte salt, and the composite membrane acts as a diaphragm. The most preferred battery structure is: an electrolyte membrane, a positive electrode sheet arranged on one side of the electrolyte membrane along the thickness direction, and a negative electrode sheet arranged on the side of the electrolyte membrane away from the positive electrode sheet along the thickness direction. In this case, the electrolyte membrane acts as both an electrolyte and a diaphragm, that is, the sodium ion battery has and only has a positive electrode sheet, a negative electrode sheet and an electrolyte membrane. Since the electrolyte membrane has high adhesion properties, the positive electrode sheet and the negative electrode sheet can be adhered to both sides thereof respectively.
[0053] Furthermore, when an additional electrolyte needs to be added to the system, the electrolyte can be any electrolyte familiar to those skilled in the art without any special restrictions. The solvent is at least one of ethyl methyl carbonate, diethyl carbonate, propylene carbonate, ethylene carbonate, dimethyl carbonate and diethylene glycol dimethanol ether; the electrolyte salt is at least one of sodium perchlorate, sodium bis(oxalate)borate, and sodium hexafluorophosphate.
[0054] The preparation method of the sodium ion battery in the present invention comprises:
[0055] I. Assembling the positive electrode sheet, the negative electrode sheet, the electrolyte and the composite membrane to obtain the sodium ion battery; or
[0056] II. Compressing the positive electrode sheet, the negative electrode sheet and the electrolyte membrane to obtain the sodium ion battery.
[0057] Furthermore, in the sodium ion battery, the thickness ratio of the positive electrode sheet, the negative electrode sheet, and the electrolyte membrane is (15-40): (15-40): (1-5).
[0058] Specifically:
[0059] Prepare a positive electrode active slurry by using a formulated amount of a Prussian blue positive electrode material, a conductive agent and a binder;
[0060] The positive electrode active slurry is coated on at least one side of the current collector along the thickness direction, dried to obtain a positive electrode active layer, and pressed to obtain a positive electrode sheet;
[0061] The positive electrode sheet, electrolyte membrane and negative electrode sheet are stacked in order and pressed.
[0062] Furthermore, the positive electrode plate of the present invention comprises a current collector and a positive electrode active layer disposed on at least one side of the current collector along the thickness direction, and the positive electrode active layer comprises a Prussian blue positive electrode material.
[0063] Furthermore, the positive electrode active layer comprises the following components in mass percentage: 75-95% of Prussian blue positive electrode material, 5-15% of conductive agent and 5-15% of binder.
[0064] Furthermore, the current collector is aluminum foil, or other materials that can be used as a current collector; preferably, the thickness of the current collector is in the range of 5-14 μm.
[0065] Furthermore, the conductive agent used in the present invention is selected from one or more of conductive carbon black, conductive graphite, carbon nanotubes and graphene.
[0066] Further, the binder can be a binder well known to those skilled in the art without any particular limitation, such as chitosan, xanthan gum, gellan gum, gum arabic, polyacrylonitrile, polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose, lithium carboxymethyl cellulose, sodium carboxymethyl cellulose, polymethacryloyl, polyacrylic acid, lithium polyacrylate, sodium polyacrylate, polyacrylamide, styrene-butadiene rubber, sodium alginate, polyethylene glycol, guar gum, guar gum polymer and guar gum copolymer. In the embodiment of the present invention, PVDF is selected.
[0067] Further, the thickness of the positive electrode active layer ranges from 100 to 300 μm, for example, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, 200 μm, 210 μm, 220 μm, 230 μm, 240 μm, 250 μm, etc., including but not limited to the thickness values listed above.
[0068] Beneficial effects of the present invention:
[0069] The composite membrane prepared by the present invention constructs a highly adhesive gel electrolyte based on the polymerization coupling synergistic induction effect of dopamine, and regulates the dynamic equilibrium response of crystal water between the material and the electrolyte by means of equilibrium response functional molecules, which will greatly improve the interface stability and kinetic characteristics of Prussian blue materials, thereby ensuring the development and application of low-cost, long-life sodium ion batteries. The composite membrane can be used as an electrolyte and a diaphragm at the same time, and has the following advantages: ① It can effectively curb the dissolution of metal elements in Prussian blue materials, and eliminate the possibility of coordination and catalytic reaction between electrolytes and them, thereby ensuring the stability of the electrode and electrolyte interface; ② It has accurate and sensitive crystal water equilibrium response capabilities, and can achieve dynamic equilibrium response of crystal water between the lattice of Prussian blue materials and electrolytes, effectively curbing the material structure destruction and electrolyte performance degradation caused by the release of hydrated sodium ions during the charge and discharge process; ③ Its high adhesion characteristics give Prussian blue materials-gel electrolytes fast interface kinetics, thereby achieving high ionic conductivity and efficient interface ion transport. BRIEF DESCRIPTION OF THE DRAWINGS
[0070] Figure 1 This is a physical picture of the electrolyte membrane prepared in Example 1.
[0071] Figure 2 This is the charge and discharge curve of the battery 1C assembled with the material prepared in Example 1. DETAILED DESCRIPTION
[0072] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0073] The first object of the present invention is to provide a composite membrane, wherein the composite membrane contains a polymer and a filler loaded in the polymer;
[0074] The filler is selected from trimethylsilyl isocyanate and / or 2-trifluoromethylnicotinate;
[0075] The preparation method of the polymer comprises the following steps:
[0076] S1. Mixing the first solution and the second solution to obtain product A; wherein the solute of the first solution is selected from one or more of dopamine salt, hydroxydopamine salt, methyldopamine salt, and methoxydopamine salt, and the solute of the second solution is selected from one or more of methacrylic anhydride, polyisobutylene succinic anhydride, and ethylene bisstearic acid amide;
[0077] S2. Heat the product A of S1 and hydroxyethyl methacrylate in the presence of an initiator to obtain the polymer.
[0078] The Prussian blue compound of the present invention has the general formula A x M1 c [M2(CN)6] y ·zH2O, wherein A is one or more of Li, Na, K, Ca, Mg, Zn, Al, M1 and M2 are one or more of Fe, Co, Ni, Cu, Zn, Ti, V, Cr, Mn, 0<x≤2, 0<y≤1, 0≤c≤1, 0<z≤16. Especially refers to Na 1.78 Cu 0.2 Ni 0.2 Co 0.2 Mn 0.2 Fe 0.2 [Fe(CN)6]·2.0H2O,Na 1.87 Cu 0.25 Ni 0.25 Mn 0.25 Fe 0.25 [Fe(CN)6]·3.0H2O,K 0.3 Na 1.4 Mn 0.2 Ni 0.2 Fe 0.2 Co 0.2 Cu 0.2 [Fe(CN)6]·2.5H2O,K 0.7 Na 1.3 Mn 0.8 Cu 0.2 [Fe(CN)6]·2.5H2O,K 0.3 Na 1.4 Fe 0.4 Co 0.4 Cu 0.2 [Fe(CN)6]·2.5H2O,Na 1.87 Cu 0.25 Mn 0.5 Fe 0.25 [Fe(CN)6]·3H2O, etc.
[0079] The crystal water introduced by vacancy defects in Prussian blue cathode materials is a double-edged sword. On the one hand, interstitial water occupies the sodium storage active sites, blocks the sodium ion transmission channel, and reduces the specific capacity of Prussian blue materials; at the same time, during the battery charging process, as the sodium ions are released, they are converted into Na(OH2) +The unit comes out and enters the electrolyte, where it slowly decomposes and has a serious negative impact on the electrode material and the stability of the electrolyte; on the other hand, the stable existence of crystal water can reduce the volume change of Prussian blue cathode materials during the sodium ion extraction and insertion process, and can also occupy the supporting sites in the Prussian blue cathode materials to improve the structural stability. Although the crystal water content can be reduced to a certain extent through preparation process optimization and post-treatment, it is still impossible to completely eliminate the impact of residual crystal water during battery cycling. Moreover, the positive effect of crystal water on the stability of the Prussian blue skeleton cannot be ignored. Therefore, the dynamic equilibrium response problem of crystal water in the electrode and electrolyte is a key challenge that restricts the cycle life of Prussian blue cathode materials.
[0080] In the present invention:
[0081] (1) The special composite membrane is used to maintain the dynamic balance of crystal water in the electrolyte and the Prussian blue cathode material, ensuring that the water molecules in the hydrated sodium ions exist in the form of stable bound water, thus preventing the decomposition of the released crystal water or side reactions with the electrolyte. This not only prevents the crystal water from reaching the negative electrode and affecting the electrochemical performance, but also avoids the adverse effects of the release of crystal water on the stability of the Prussian blue cathode material skeleton;
[0082] (2) Dopamine is the main component of marine mussel foot protein and has the characteristics of strong adhesion to inorganic and organic surfaces. The present invention uses this biological characteristic to develop an adaptive bionic gel electrolyte. The prepared product has high adhesion, which gives the Prussian blue positive electrode material-gel electrolyte fast interfacial kinetic properties, thereby achieving high ionic conductivity and efficient interfacial ion transport.
[0083] Preferably, the preparation method of the polymer is: product A, hydroxyethyl methacrylate, and an initiator are mixed in an organic solvent, and reacted at 40-100° C. to obtain a polymer. Preferably, the reaction temperature is 60-80° C., such as 41° C., 45° C., 50° C., 55° C., 60° C., 65° C., 70° C., 75° C., 80° C., 85° C., 90° C., 95° C., 100° C., etc., including but not limited to the temperatures listed above.
[0084] Preferably, the organic solvent may be any volatile organic solvent, including but not limited to anhydrous N,N-dimethylformamide (DMF), acetone, alcohol solvents, and the like.
[0085] Preferably, the method of loading the filler into the polymer comprises: dissolving the polymer with a solvent, mixing the obtained solution with the filler, and removing the solvent to obtain a composite precursor.
[0086] Preferably, in the solution in which the polymer is dissolved, the concentration of the polymer is 0.1-1.0 g / ml.
[0087] Preferably, the filler accounts for 0.1wt%-5wt% of the total mass of the polymer. Experimental verification has found that the type and proportion of fillers have an impact on performance. When other conditions are the same, the adhesion strength of the prepared composite film increases with the increase of filler content, and the adhesion performance can still be maintained after cycling; at the same time, different contents will also affect the moisture content of the pole piece, and the moisture content of the pole piece reaches the optimal value at a specific content.
[0088] Preferably, the above solvent includes but is not limited to anhydrous DMF, dimethyl sulfoxide (DMSO), acetone and the like.
[0089] Preferably, the molar ratio of the product A to hydroxyethyl methacrylate is 1:(1-5).
[0090] Preferably, the salts include but are not limited to hydrochlorides, sulfates, nitrates and the like.
[0091] Preferably, the initiator is selected from organic peroxide initiators and / or azo initiators, including but not limited to azobisisobutyronitrile, dibenzoyl peroxide, and the like.
[0092] Preferably, the amount of the initiator used is 0.1-2 wt % of the total mass of the raw materials (product A, hydroxyethyl methacrylate and initiator).
[0093] Preferably, the preparation method of the product A is:
[0094] Solution A is prepared using at least one of dopamine hydrochloride, hydroxydopamine hydrochloride, methyldopamine hydrochloride, and methoxydopamine hydrochloride as a solute; solution B is prepared using at least one of methacrylic anhydride, polyisobutylene succinic anhydride, and ethylenebisstearic acid amide as a solute; wherein the pH of solution A is alkaline;
[0095] Solution A and solution B are mixed to react, and the pH of the system is adjusted to acidic during the reaction to obtain the product A.
[0096] Specifically:
[0097] a) preparing solution A: adding solute A into a well-stirred buffer solution to obtain solution A. Solute A is dopamine hydrochloride, hydroxydopamine hydrochloride, N-methyldopamine hydrochloride, or methoxydopamine hydrochloride;
[0098] b) preparing solution B: adding solute B into an organic solvent to obtain solution B. Solute B is methacrylic anhydride, polyisobutylene succinic anhydride, and ethylene bisstearic acid amide;
[0099] c) mixing solution A with solution B;
[0100] d) stirring for 10-12 hours, adding hydrochloric acid dropwise to adjust the pH value to less than 2, and extracting with an extractant;
[0101] e) After concentration by rotary evaporation, precipitation was performed by adding a precipitant, recrystallization was performed in hexane and drying was performed under high vacuum to obtain a light grey solid.
[0102] Preferably, in step a), the pH value of the buffer solution is 8.5-10, the solvent is deionized water, and the buffer is sodium bicarbonate, sodium tetraborate, sodium citrate, disodium hydrogen phosphate, sodium dihydrogen phosphate, etc.
[0103] Preferably, in step b), the organic solvent is tetrahydrofuran, ethyl acetate, isobutyl ether, etc.
[0104] Preferably, in step b), the concentration of solution B is 15-35 wt %.
[0105] Preferably, in step c), the mixing is: adding solution B dropwise into solution A, and the whole process is carried out under an inert atmosphere, such as argon, helium, etc.
[0106] Preferably, in step d), the extractant is ethyl acetate, isobutanol or acetone.
[0107] Preferably, in step e), the precipitant is hexane, 2-methylpentane, 3-methylpentane, 2,3-dimethylbutane or the like.
[0108] Another object of the present invention is to provide a method for preparing a composite film, comprising the following steps:
[0109] (1) mixing a first solution and a second solution to obtain a product A; wherein the solute of the first solution is selected from one or more of dopamine salts, hydroxydopamine salts, methyldopamine salts, and methoxydopamine salts, and the solute of the second solution is selected from one or more of methacrylic anhydride, polyisobutylene succinic anhydride, and ethylene bisstearic acid amide;
[0110] (2) heating the product A and hydroxyethyl methacrylate in the presence of an initiator to obtain a polymer;
[0111] (3) mixing the polymer and the filler to form a film to obtain the composite film;
[0112] The filler is selected from trimethylsilyl isocyanate and / or 2-trifluoromethylnicotinate methyl ester.
[0113] Preferably, in step (3), the mixing comprises: dissolving the polymer in a solvent (such as methanol), mixing with the filler, and removing the solvent after mixing evenly.
[0114] Preferably, in step (3), the preparation of the film comprises: coating the mixture of the polymer and the filler at a set thickness, and heat treating the film at a set temperature. Preferably, the set temperature is 70-90°C. For example, 71°C, 72°C, 73°C, 74°C, 75°C, 76°C, 77°C, 78°C, 79°C, 80°C, 81°C, 82°C, 83°C, 84°C, 85°C, 86°C, 87°C, 88°C, 89°C, etc., including but not limited to the temperatures listed above.
[0115] Another object of the present invention is to provide an electrolyte membrane, which comprises: the above-mentioned composite membrane or the composite membrane obtained by the above-mentioned preparation method, and an electrolyte salt loaded in the composite (the loading method is the same as the operation of the filler, specifically, the polymer is mixed with the filler and the electrolyte salt, the solvent is removed, and the loading is completed).
[0116] Preferably, the electrolyte membrane comprises at least one of the following:
[0117] (1) The mass percentage of the electrolyte salt is 1wt%-10wt%;
[0118] (2) The mass percentage of the filler is 0.1wt%-5wt%.
[0119] Another object of the present invention is to provide a method for preparing an electrolyte membrane, comprising the following steps:
[0120] (01) mixing a first solution and a second solution to obtain a product A; wherein the solute of the first solution is selected from one or more of dopamine salts, hydroxydopamine salts, methyldopamine salts, and methoxydopamine salts, and the solute of the second solution is selected from one or more of methacrylic anhydride, polyisobutylene succinic anhydride, and ethylene bisstearic acid amide;
[0121] (02) heating the product A and hydroxyethyl methacrylate in the presence of an initiator to obtain a polymer;
[0122] (03) mixing the polymer with a filler and an electrolyte salt to form a film, thereby obtaining the electrolyte membrane;
[0123] The filler is selected from trimethylsilyl isocyanate and / or 2-trifluoromethylnicotinate methyl ester.
[0124] Preferably, the electrolyte salt includes at least one of sodium hexafluorophosphate, sodium bis(fluorosulfonyl)imide, sodium tetrafluoroborate, sodium perchlorate or sodium difluorophosphate.
[0125] Another object of the present invention is to provide a battery separator, which contains the composite membrane, the composite membrane obtained by the above preparation method, the electrolyte membrane or the electrolyte membrane obtained by the above preparation method.
[0126] The present invention also provides a sodium ion battery, wherein the sodium ion battery comprises:
[0127] I. A positive electrode sheet, a negative electrode sheet, an electrolyte and the above composite film or a composite film obtained by the above preparation method containing a Prussian blue positive electrode material; or
[0128] II. A positive electrode sheet and a negative electrode sheet containing a Prussian blue positive electrode material and the above electrolyte membrane or the electrolyte membrane obtained by the above preparation method.
[0129] In the present invention, the sodium ion battery contains a positive electrode sheet, a negative electrode sheet and a composite membrane. In this case, the battery system also needs to contain an organic solution (electrolyte) of electrolyte salt, and the composite membrane acts as a diaphragm. The most preferred battery structure is: an electrolyte membrane, a positive electrode sheet arranged on one side of the electrolyte membrane along the thickness direction, and a negative electrode sheet arranged on the side of the electrolyte membrane away from the positive electrode sheet along the thickness direction. In this case, the electrolyte membrane acts as both an electrolyte and a diaphragm, that is, the sodium ion battery has and only has a positive electrode sheet, a negative electrode sheet and an electrolyte membrane. Since the electrolyte membrane has high adhesion properties, the positive electrode sheet and the negative electrode sheet can be adhered to both sides thereof, respectively.
[0130] When an additional electrolyte needs to be added to the system, the electrolyte can be any electrolyte familiar to those skilled in the art without any special restrictions. The solvent is at least one of ethyl methyl carbonate, diethyl carbonate, propylene carbonate, ethylene carbonate, dimethyl carbonate and diethylene glycol dimethanol ether; the electrolyte salt is at least one of sodium perchlorate, sodium bis(oxalate)borate, and sodium hexafluorophosphate.
[0131] The preparation method of the sodium ion battery in the present invention comprises:
[0132] I. Assembling the positive electrode sheet, the negative electrode sheet, the electrolyte and the composite membrane to obtain the sodium ion battery; or
[0133] II. Compressing the positive electrode sheet, the negative electrode sheet and the electrolyte membrane to obtain the sodium ion battery.
[0134] Preferably, in the sodium ion battery, the thickness of the positive electrode sheet and the negative electrode sheet is 150-400 μm, and the thickness of the electrolyte membrane is in the range of 10-50 μm.
[0135] Specifically:
[0136] Prepare a positive electrode active slurry by using a formulated amount of a Prussian blue positive electrode material, a conductive agent and a binder;
[0137] The positive electrode active slurry is coated on at least one side of the current collector along the thickness direction, dried to obtain a positive electrode active layer, and pressed to obtain a positive electrode sheet;
[0138] The positive electrode sheet, electrolyte membrane and negative electrode sheet are stacked in order and pressed.
[0139] The positive electrode sheet of the present invention comprises a current collector and a positive electrode active layer arranged on at least one side of the current collector along the thickness direction, and the positive electrode active layer comprises a Prussian blue positive electrode material.
[0140] Preferably, the positive electrode active layer comprises the following components in mass percentage: 75-95% of Prussian blue positive electrode material, 5-15% of conductive agent and 5-15% of binder.
[0141] Preferably, the current collector is aluminum foil, or other materials that can be used as a current collector; preferably, the thickness of the current collector is in the range of 5-14 μm.
[0142] Preferably, the conductive agent used in the present invention is selected from one or more of conductive carbon black, conductive graphite, carbon nanotubes and graphene.
[0143] Preferably, the binder is a binder well known to those skilled in the art, without any particular limitation, such as chitosan, xanthan gum, gellan gum, gum arabic, polyacrylonitrile, polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose, lithium carboxymethyl cellulose, sodium carboxymethyl cellulose, polymethacryloyl, polyacrylic acid, lithium polyacrylate, sodium polyacrylate, polyacrylamide, styrene-butadiene rubber, sodium alginate, polyethylene glycol, guar gum, guar gum polymer and guar gum copolymer. In the embodiment of the present invention, PVDF is selected.
[0144] Preferably, the thickness of the positive electrode active layer is in the range of 100-300 μm, for example, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, 200 μm, 210 μm, 220 μm, 230 μm, 240 μm, 250 μm, etc., including but not limited to the thickness values listed above. Example 1
[0145] 1. Synthesis of raw materials
[0146] a) 4 g of sodium bicarbonate and 10 g of sodium tetraborate decahydrate were selected as buffers and dissolved in 100 ml of deionized water in a 200 ml round-bottom flask as a buffer with a pH value of 9.2. The solution was stirred for 10 minutes under an argon atmosphere, and then 10 g of dopamine hydrochloride was added to obtain solution A.
[0147] b) Methacrylic anhydride (4.7 ml) was mixed with tetrahydrofuran solvent (25 ml) (solvent B) and added dropwise to solution A. The mixture was stirred at room temperature under an argon atmosphere for 12 hours, the pH was adjusted to less than 2 by dropwise addition of hydrochloric acid, and then extracted three times with 50 ml of ethyl acetate extractant. The ethyl acetate layer was concentrated to about 30 ml by rotary evaporation. The product was then precipitated by adding 200 ml of hexane precipitant and stored at 4°C overnight. The product was recrystallized in hexane and dried under high vacuum to obtain a light gray solid (product A).
[0148] 2. Preparation of composite membrane
[0149] c) In the case of product A:hydroxyethyl methacrylate (HEMA) = 1:5, HEMA (5.5 g, 25 mmol), product A (1.1 g, 5 mmol) and AIBN initiator azobisisobutyronitrile (76 mg, 0.46 mmol) were stirred in 20 ml acetone, solvent in a 100 ml closed round bottom flask and purged with argon for 10 minutes. The solution was heated to 60°C and stirred for 12 hours. Subsequently, the reaction mixture was diluted by adding 20 ml methanol and then 200 ml diethyl ether to precipitate the polymer. The precipitation process was repeated two to three times to completely remove the unreacted raw materials and residual solvent. The polymer was then dried under high vacuum.
[0150] d) 6.6 g of the polymer obtained in the above step was dissolved in methanol at a concentration of 0.5 g / ml, and added to the filler trimethylsilyl isocyanate (0.01 g), mixed well and evacuated, and these steps were repeated several times to ensure that the materials were mixed completely. When the methanol was completely evaporated in the air, a composite film material was obtained. Among them, the proportion of the filler trimethylsilyl isocyanate was 0.15wt%.
[0151] e) The composite film material prepared in the above steps is coated on a metal base plate in a coating thickness of 50 μm, and heat-treated in an oven at 80° C. for 90 min to obtain a composite film.
[0152] 3. Preparation of electrolyte membrane
[0153] f) 6.6 g of the polymer obtained in the above step was dissolved in methanol at a concentration of 0.5 g / ml, and added to the filler trimethylsilyl isocyanate (0.01 g) and the electrolyte salt sodium hexafluorophosphate (0.2 g), mixed well and evacuated, and these steps were repeated several times to ensure that the materials were mixed completely. When the methanol was completely evaporated in the air, the electrolyte composite material was obtained. Among them, the filler trimethylsilyl isocyanate accounted for 0.15wt%.
[0154] g) The electrolyte composite material prepared in the above steps is coated on a metal substrate in a coating thickness of 50 μm, and heat-treated in an oven at 80° C. for 90 min to obtain an electrolyte membrane. Example 2
[0155] The ratio of product A:HEMA = 1:5 was replaced by product A:HEMA = 1:3, and the proportion of filler trimethylsilyl isocyanate was adjusted to 2 wt %, and the rest was the same as in Example 1. Example 3
[0156] The ratio of product A:HEMA = 1:5 was replaced by product A:HEMA = 1:1, and the proportion of filler trimethylsilyl isocyanate was adjusted to 1 wt %, and the rest was the same as in Example 1. Example 4
[0157] The filler trimethylsilyl isocyanate was replaced by 2-trifluoromethylnicotinate methyl ester, and the rest was the same as in Example 2. Example 5
[0158] The filler trimethylsilyl isocyanate was replaced with 2-trifluoromethylnicotinate methyl ester, and the proportion of the filler 2-trifluoromethylnicotinate methyl ester was adjusted to 1 wt %, and the rest was the same as in Example 2. Example 6
[0159] The composite membrane prepared in step (e) is used as a separator and a liquid electrolyte is added. The added liquid electrolyte is a carbonate solvent PC:EC=1:1, the electrolyte salt is sodium hexafluorophosphate, the concentration is 1 mol / L, and the rest is the same as in Example 2. Comparative Example 1
[0160] Purified hydroxyethyl methacrylate (6.6 g), filler (0.01 g trimethylsilyl isocyanate) and electrolyte salt (0.2 g sodium hexafluorophosphate) and AIBN (76 mg) were stirred in 20 ml anhydrous DMF in a 100 ml closed round bottom flask, and the mixture was degassed three times using a pump-freeze-thaw cycle and backfilled with argon. The solution was heated to 60°C and stirred for 12 hours for polymerization. Comparative Example 2
[0161] Purified hydroxyethyl methacrylate (6.6 g), electrolyte salt (0.2 g sodium hexafluorophosphate) and AIBN (76 mg) were stirred in 20 ml anhydrous DMF in a 100 ml closed round bottom flask, and the mixture was degassed three times using a pump-freeze-thaw cycle and backfilled with argon. The solution was heated to 60 ° C and stirred for 12 h to polymerize. Comparative Example 3
[0162] No filler trimethylsilyl isocyanate was added, and the remaining steps were the same as in Example 1. Comparative Example 4
[0163] The filler trimethylsilyl isocyanate was replaced with the commonly used water-absorbing desiccant calcium chloride, and the remaining steps were the same as in Example 1. Comparative Example 5
[0164] This comparative example does not use the above composite membrane, but uses a liquid electrolyte and a conventional separator, that is, a carbonate solvent PC:EC=1:1, an electrolyte salt is sodium hexafluorophosphate with a concentration of 1 mol / L, and a separator is polyethylene PE. Test Case
[0165] Adhesion strength and electrochemical performance test
[0166] (1) The shear adhesion strength test is to stretch the standard sample at a constant rate until it is completely torn, and record the shear force value when it is completely torn, which can describe the adhesion strength between the material and the electrode. The test is carried out using an Instron 5566 universal testing machine. The test sample is in the shape of a long strip, with a test length and width of 30 mm and 50 mm respectively. The electrolyte membrane is clamped between two Prussian blue electrodes (all electrodes used in shear adhesion strength tests are prepared from the same batch) and a pressure of 5 MPa is applied. After maintaining the pressure for 30 minutes, the electrodes on both sides are pulled by a tensile machine at a stretching rate of 5 mm / min. The shear force of desorption is measured, and the shear force divided by the contact area is the shear adhesion strength value. The test is completed at room temperature;
[0167] The conductivity of the electrolyte membrane is tested by electrochemical impedance spectroscopy (EIS). The EIS test is performed using stainless steel as a blocking electrode. The obtained bulk resistance can be used to calculate the ionic conductivity σ of the electrolyte membrane using the following formula.
[0168]
[0169] Where d is the thickness of the electrolyte membrane, S is the area of the blocking electrode, and Rb is the bulk resistance. The results are shown in Table 1.
[0170] (2) The negative electrode uses metal sodium sheet, and the positive electrode uses iron-manganese-based Prussian blue Na 1.87 Cu 0.25 Mn 0.5 Fe 0.25[Fe(CN)6]·3H2O, slurry is prepared in a ratio of active material: conductive carbon black: binder = 8:1:1, coated on aluminum foil, the wet coating thickness is 200 microns, dried and rolled, and then cut into corresponding shapes. The electrolyte membrane is used as a diaphragm for battery stacking assembly (at this time, no additional electrolyte is added to the battery system, and the embodiments and comparative examples using electrolyte and composite membrane / diaphragm can be assembled according to the traditional method), the battery is charged and discharged for 5 cycles at 0.1C, and charged and discharged for 5 times at 1C, 5C, 10C, and 20C, and the battery rate performance is tested (see Table 2), and then charged and discharged for 5000 times at 5C, and a long cycle test is performed to calculate the capacity retention rate. The capacity retention rate is the ratio of the discharge capacity at the 5000th week to the discharge capacity at the first week during the 5C cycle. After the cycle, the electrode was disassembled and the water content of the positive electrode, the adhesion strength of the electrolyte and the electrode were tested using a Karl Fischer titrator. The electrodes on both sides were pulled using a tensile machine at a stretching rate of 5 mm / min, and the desorption shear force was measured. The shear force divided by the contact area was the shear adhesion strength value (Table 1).
[0171] Among them, iron-manganese-based Prussian blue Na 1.87 Cu 0.25 Mn 0.5 Fe 0.25 The preparation method of [Fe(CN)6]·3H2O is as follows:
[0172] (1) Take 2.8 L of 0.5 mol / L sodium ferrocyanide solution as solution A;
[0173] (2) 1 L of 2 mol / L sodium citrate solution was mixed with 0.7 L of 1 mol / L manganese sulfate, 0.35 L of 1 mol / L copper sulfate, and 0.35 L of 1 mol / L ferrous sulfate solution to prepare solution B.
[0174] (3) Solution A was added dropwise to solution B at a rate of 100 mL / min to generate a precipitate. The precipitate was allowed to stand at 40 °C for 12 h. The solid-liquid mixed solution was filtered and the obtained solid was vacuum dried to obtain the product.
[0175] The results are as follows:
[0176] The actual picture of the electrolyte membrane prepared in Example 1 is as follows Figure 1 As shown, the battery charge and discharge performance test results obtained by the above-mentioned stacking method for the electrolyte membrane of Example 1 are shown in Figure 2 , it can be seen that the charge and discharge curve of the battery is normal, and the specific capacity of the material is 128mAh / g, which is basically the same as the capacity of conventional liquid electrolytes.
[0177] Table 1 Adhesion performance and water content results before and after cycling
[0178]
[0179] Note: The conductivity of Comparative Example 5 was measured by a conductivity meter.
[0180] Table 2 Rate performance test results
[0181]
[0182] From Table 1 we can see that:
[0183] Due to the addition of product A, the pre-cycle adhesion shear strength of the electrolyte membrane of the present invention is increased by nearly 3 times (compared with Example 1 and Comparative Example 1). This is mainly due to the good water-resistant bonding performance brought by the dopamine functional group. As the proportion of product A increases, the adhesion shear strength tends to increase. Considering the processing characteristics, the proportion of product A is optimal at 15%-50%. At the same time, since product A has a multi-element multi-level cross-linked network and abundant hydrogen bonds, the conductivity of the electrolyte membrane is also improved. When the mass fraction of the filler trimethylsilyl isocyanate is 0.15%, the conductivity of Comparative Example 1 is 2.87×10 -3 S / cm. When about 17% of product A was added, the conductivity of Example 1 was as high as 4.51×10 -3 S / cm, increased by 57%;
[0184] By comparing Example 1 with Comparative Example 1, it can be seen that due to the presence of Product A, since it does not undergo coordination reaction with the Prussian analogue and does not dissolve the Prussian analogue, it stabilizes the Prussian blue positive electrode material;
[0185] By comparing Example 2 and Example 3, it can be seen that the selectivity of the filler and the water molecules gives the gel electrolyte an excellent crystallization water response characteristic, which can play a role in crystallization water balance. When the crystallization water content of the Prussian blue material and the crystallization water content of the gel electrolyte reach a balance, the Prussian blue material no longer has a crystallization water release reaction, and the electrochemical system enters a stable state.
[0186] Combining Comparative Examples 1 and 2, it can be seen that the filler can balance the crystallization water to a certain extent. In the absence of Product A, the Prussian blue material positive electrode material will continue to release crystallization water. This is mainly because when the crystallization water is released, the Prussian blue skeleton collapses. The bonding strength between the hydroxyethyl methacrylate and the Prussian blue electrode in the comparative example is not high. As the crystallization water is released, the contact force between the electrolyte membrane and the electrode is reduced again, resulting in an increase in the interface impedance. When Product A is added, the multi-layer cross-linked network of Product A will "coat" the hydroxyethyl methacrylate, and the strong adhesion of dopamine can maintain the stability of the interface impedance, thereby maintaining the stability of the battery cycle.
[0187] Under the dual effects of the addition of product A and the corresponding characteristics of the crystallization water of the filler, the capacity retention rates of Examples 1 and 2 are above 90%. Although the rate performance of Comparative Example 5 is very good, the precipitation of interstitial water in the Prussian blue active material during the cycle causes the material structure to collapse, and the capacity retention rate is only 10%. After disassembly, the moisture content in the electrolyte is as high as 4500ppm.
[0188] From Table 2 we can see that:
[0189] Since the electrolyte membrane has good adhesion properties, the contact resistance between the electrolyte and the electrode can be greatly reduced, so the rate performance is greatly improved. The capacity retention rate of 20C is more than 56% of that of 1C, which is basically close to the liquid electrolyte of Comparative Example 5. The capacity of the comparative example is not much different at 0.1C and 1C, but the capacity shows a sharp decline at high rates (5C, 10C, 20C), mainly because the conventional electrolyte membrane has insufficient adhesion to the pole piece, resulting in a large interface impedance between the electrolyte and the pole piece, which greatly affects the rate performance of the battery. In addition, by comparing Example 6 and Example 2, it can be seen that the rate performance of the two is basically close, which shows that the conductivity of the liquid electrolyte and the conductivity of the electrolyte membrane are close, and the cycle stability of Example 2 (5000-week capacity retention rate 94%) is higher than that of Example 6 (5000-week capacity retention rate 83%), which is mainly due to the good contact performance of the electrolyte membrane and the electrode, which delays the increase in interface impedance caused by expansion and contraction during the cycle.
[0190] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.
Claims
1. A composite film, characterized in that The composite membrane contains a polymer and a filler loaded in the polymer; The filler is selected from trimethylsilyl isocyanate and / or 2-trifluoromethylnicotinate; The preparation method of the polymer comprises the following steps: S1. Mixing the first solution and the second solution to obtain product A; wherein the solute of the first solution is selected from one or more of dopamine salt, hydroxydopamine salt, methyldopamine salt, and methoxydopamine salt, and the solute of the second solution is methacrylic anhydride; S2, heating the product A of S1 and hydroxyethyl methacrylate in the presence of an initiator to obtain the polymer; The molar ratio of the product A to hydroxyethyl methacrylate is 1:(1-5); and the filler accounts for 0.1wt%-5wt% of the total mass of the polymer.
2. The composite membrane according to claim 1, characterized in that The preparation method of the polymer comprises: mixing product A, hydroxyethyl methacrylate and an initiator in an organic solvent, and reacting at 40-100° C. to obtain the polymer.
3. A method for preparing a composite film, characterized in that: The following steps are involved: (1) mixing a first solution and a second solution to obtain a product A; wherein the solute of the first solution is selected from one or more of dopamine salts, hydroxydopamine salts, methyldopamine salts, and methoxydopamine salts, and the solute of the second solution is methacrylic anhydride; (2) heating the product A and hydroxyethyl methacrylate in the presence of an initiator to obtain a polymer; (3) mixing the polymer and the filler to form a film to obtain the composite film; The filler is selected from trimethylsilyl isocyanate and / or 2-trifluoromethylnicotinate; The molar ratio of the product A to hydroxyethyl methacrylate is 1:(1-5); The filler accounts for 0.1wt%-5wt% of the total mass of the polymer.
4. An electrolyte membrane, characterized in that The electrolyte membrane comprises: the composite membrane according to claim 1 or 2 or the composite membrane prepared by the preparation method according to claim 3, and an electrolyte salt supported in the polymer.
5. The electrolyte membrane according to claim 4, characterized in that The electrolyte salt includes at least one of sodium hexafluorophosphate, sodium bis(fluorosulfonyl)imide, sodium tetrafluoroborate, sodium perchlorate, and sodium difluorophosphate.
6. A method for preparing an electrolyte membrane, characterized in that: The following steps are involved: (01) mixing a first solution and a second solution to obtain a product A; wherein the solute of the first solution is selected from one or more of dopamine salts, hydroxydopamine salts, methyldopamine salts, and methoxydopamine salts, and the solute of the second solution is methacrylic anhydride; (02) heating the product A and hydroxyethyl methacrylate in the presence of an initiator to obtain a polymer; (03) mixing the polymer with a filler and an electrolyte salt to form a film, thereby obtaining the electrolyte membrane; The filler is selected from trimethylsilyl isocyanate and / or 2-trifluoromethylnicotinate; The molar ratio of the product A to hydroxyethyl methacrylate is 1:(1-5); The filler accounts for 0.1wt%-5wt% of the total mass of the polymer.
7. A battery separator, characterized in that: The battery separator contains the composite membrane according to claim 1 or 2, the composite membrane obtained by the preparation method according to claim 3, the electrolyte membrane according to claim 4 or 5, or the electrolyte membrane obtained by the preparation method according to claim 6.
8. A sodium ion battery, characterized in that: The sodium ion battery contains: I. A positive electrode sheet, a negative electrode sheet, an electrolyte, and a composite film according to claim 1 or 2 or a composite film prepared by the preparation method according to claim 3 containing a Prussian blue positive electrode material; or II. A positive electrode sheet and a negative electrode sheet containing a Prussian blue positive electrode material and an electrolyte membrane according to claim 4 or 5 or an electrolyte membrane obtained by the preparation method according to claim 6.
9. The sodium ion battery according to claim 8, characterized in that: When the sodium ion battery contains a positive electrode sheet, a negative electrode sheet and an electrolyte membrane, the sodium ion battery includes: an electrolyte membrane, a positive electrode sheet arranged on one side of the electrolyte membrane along the thickness direction, and a negative electrode sheet arranged on one side of the electrolyte membrane along the thickness direction away from the positive electrode sheet.