Low-impedance NASICON type solid electrolyte membrane and preparation method thereof, and all-solid-state lithium battery and preparation method thereof
Through the combination of pre-annealing and nano-scale additives, the preparation technology of NASICON type solid electrolyte membrane is improved, solving the problems of ceramic membrane structural failure and high grain boundary impedance in fast Joule thermal technology, and improving the structural compactness of all-solid lithium batteries and cyclic stability.
Patent Information
- Application Number
- CN202411033839.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
The existing NASICON type solid electrolyte membrane has problems such as mechanical structure failure, many body phase defects and high grain boundary impedance in the rapid Joule thermal technology, which limits the safety and cycle life of all-solid-state lithium batteries.
Pre-annealing treatment is adopted to promote ceramic particles diffusion and structural recombination, combined with the design of nano-scale boron-based liquid sintering aids, ionic fillers and fiber reinforced materials, and low-impedance NASICON type solid electrolyte membranes are prepared through improved rapid Joule thermal technology. And a mixed ITO/LLZTO layer is introduced into all solid state lithium batteries to reduce interface impedance.
It significantly improves the density and mechanical strength of the NASICON type solid electrolyte membrane, reduces body phase defects and crystal interface pores, improves electrochemical performance and cycle stability, extends the cycle life of the battery and improves safety.
Smart Images

Figure CN118970152A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of solid-state batteries, and relates to a low-impedance NASICON solid-state electrolyte membrane and a preparation method thereof, and an all-solid-state lithium battery and a preparation method thereof. Background Art
[0002] Energy shortage and excessive carbon emission crisis have led to a new energy production and consumption pattern that has shifted from absolute dominance of fossil energy to low-carbon multi-energy integration. Innovation in electrochemical energy storage technology is a key way to implement the energy revolution. This technology can facilitate the storage / release of electric energy and meet the needs of different scale energy storage technologies on the power generation side, distribution side and user side. The ultimate goal is to solve major strategic issues such as large-scale access to renewable energy, complementary coupling utilization of multiple energies, deep electrification of terminal energy consumption, and construction of smart energy networks. Therefore, it has received close attention and research from emerging markets and scientific research fields. Liquid-based lithium-ion batteries are regarded as one of the most competitive mainstream electrochemical energy storage technologies due to their advantages such as light weight, high specific energy / specific power, and long cycle life. However, with the rapid development of modular energy storage technology, high-power electric vehicles, and microelectronic devices, existing liquid-based lithium-ion batteries cannot meet further development needs in terms of energy density / power density, charge and discharge rate, and working safety. Using solid electrolyte membranes with ion conductivity to replace unstable diaphragm / electrolyte systems and constructing high-voltage all-solid-state lithium batteries is an important way to achieve a breakthrough in battery energy density and safety of use.
[0003] As the most important component of lithium metal solid-state batteries, solid electrolyte membranes are difficult to synthesize and have high manufacturing costs. In the existing NASICON solid electrolyte membrane synthesis method, the traditional high-temperature solid-phase sintering process has high energy consumption and low production efficiency. The grain growth and grain boundary diffusion under high temperature conditions are uncontrollable, which easily forms uneven microstructures and undesirable ion migration paths. At the same time, the long sintering time will also cause the crystal state transformation, phase separation and active lithium volatilization of ceramic particles, affecting the lattice stability of the electrolyte and the final ionic conductivity. Emerging synthesis methods such as rapid Joule heating technology can quickly achieve the crystallization and densification process of the solid electrolyte embryo through "flash burning", reducing unnecessary lithium volatilization and production energy consumption, but there are also many problems that need to be solved, including: (1) Rapid Joule heating technology is prone to uneven heat distribution, and the ceramic particles in different regions of the material expand uncoordinatedly when heated. The irregular growth stress generated causes the mechanical properties of the ceramic membrane structure to decrease; (2) The drastic temperature change during the rapid Joule heating process hinders the sufficient diffusion and structural reorganization of ceramic particles, resulting in the generation of more bulk defects and the accumulation of impurities at the grain boundaries, increasing the electrochemical AC impedance of the solid electrolyte membrane bulk and crystal interface; (3) The increase in bulk defects may also cause grain boundary weakening and provide more deposition sites for poor lithium deposition, thereby reducing the overall structural density of the solid electrolyte membrane and increasing the risk of structural failure caused by dendrite penetration in the later stage. In addition, the high-valent metal cations in the commonly used NASICON solid electrolyte are prone to reduction side reactions at high reduction potentials, generating inert interlayers that hinder ion migration and diffusion, limiting the long cycle life of all-solid-state lithium batteries.
[0004] In summary, the current rapid Joule heating technology is prone to ceramic membrane mechanical structure failure (microcracks, voids), a large number of bulk defects and high grain boundary impedance in the process of preparing oxide solid electrolyte membranes, which in turn has an adverse effect on the density of the solid electrolyte membrane structure and limits the safety and cycle life of all-solid-state lithium batteries. Summary of the invention
[0005] The purpose of the present invention is to provide a low-impedance NASICON type solid electrolyte membrane and its preparation method and an all-solid-state lithium battery and its preparation method, so as to solve the technical problems of ceramic membrane mechanical structure failure, large number of bulk defects and high grain boundary impedance in the process of preparing oxide solid electrolyte membrane by rapid Joule heating technology in the prior art.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] In a first aspect, the present invention discloses a method for preparing a low-impedance NASICON solid electrolyte membrane, comprising the following steps:
[0008] The lithium source, aluminum source and phosphorus source are mixed, and then a titanium source or a germanium source is added and ball-milled; the ball-milled powder is sequentially dried and subjected to high-temperature solid-phase synthesis to obtain ceramic coarse particles; the ceramic coarse particles are sequentially ball-milled, dried and sieved to obtain NASICON type solid electrolyte powder;
[0009] Adding a nano-sized boron-based liquid-phase sintering aid, an ion filler and a fiber reinforcement material to NASICON solid electrolyte powder and mixing them uniformly to obtain a mixture, putting the mixture into a metal mold and pressing it into a ceramic green embryo, and placing the ceramic green embryo in a crucible for annealing treatment;
[0010] The annealed ceramic body is transferred to a Joule heating element of a Joule electric heating device, and sintered by rapid Joule heat treatment under a protective atmosphere. After the heat treatment, the ceramic body is cooled to room temperature to obtain a rough NASICON solid electrolyte membrane.
[0011] The rough NASICON solid electrolyte membrane is placed in a metallographic grinder and polished, and then the surface of the solid electrolyte membrane is treated with acid immersion, and then neutralized with an alkaline solution and fully rinsed with ethanol to prepare a low-impedance NASICON solid electrolyte membrane.
[0012] Furthermore, the NASICON solid electrolyte powder is lithium aluminum germanium phosphate or lithium aluminum titanium phosphate, and the chemical formula is Li 1+x Al x Ge 2-x (PO4)3 or Li 1+x Al x Ti 2-x (PO4)3, wherein 0≤x≤1; the lithium source is lithium carbonate or lithium hydroxide, the aluminum source is aluminum nitrate or aluminum oxide, the phosphorus source is diammonium phosphate or phosphoric acid, the titanium source is tetrabutyl titanate or titanium oxide, and the germanium source is germanium oxide; the ball milling medium used in the ball milling process is isopropanol or ethanol, and the ball mill speed is 90rpm~500rpm; the specific steps of the high-temperature solid phase synthesis are: heating at a heating rate of 4℃ / min~10℃ / min to a roasting temperature of 600℃~900℃ for high-temperature solid phase synthesis, the insulation time is 6h~8.5h, and then cooling to room temperature at a cooling rate of 8℃ / min~13℃ / min; the screening process uses a nylon mesh screen of 200 mesh~800 mesh for screening.
[0013] Furthermore, the added mass ratio of the boron-based liquid-phase sintering aid, the ion filler and the fiber reinforcement material is (1.5-3):1:(0.5-1); the total mass of the boron-based liquid-phase sintering aid, the ion filler and the fiber reinforcement material accounts for 1wt%-5wt% of the mass of the mixture; the boron-based liquid-phase sintering aid is a mixture of one or more of sodium aluminum borate, sodium borohydride, ammonium boron nitrate, aluminum triboride and boron oxide; the ion filler is a mixture of one or more of lithium tetrafluoroborate, lithium borate, lithium nitride and lithium titanate; the fiber reinforcement material is a mixture of one or more of single-walled carbon nanotubes, para-aramid nanofibers, polyimide fibers, boron carbide fibers and boron fibers; the pressure of the ceramic green body during the pressing process is 5MPa-15MPa; the temperature of the annealing treatment is (T c -200)℃~(T c -300)℃,T c The crystallization temperature is the crystallization temperature, the holding time is 2h to 3h, the heating rate is 4℃ / min to 10℃ / min, and the cooling rate is 8℃ / min to 13℃ / min.
[0014] Furthermore, the protective atmosphere is an inert gas; the voltage of the Joule heating during the rapid Joule heat treatment is 10V to 100V, the heating current is 10A to 60A, and the sintering temperature threshold is 800°C to 960°C; the temperature is lowered to room temperature after the heat treatment is completed by manually adjusting the current so that the temperature drops to room temperature at a uniform rate; the acid used for the acid leaching treatment is hydrochloric acid or dilute nitric acid; the alkaline solution is a dilute sodium hydroxide solution or a sodium bicarbonate solution.
[0015] In a second aspect, the present invention discloses a low-impedance NASICON-type solid electrolyte membrane, which is prepared by the above-mentioned method for preparing a low-impedance NASICON-type solid electrolyte membrane.
[0016] In a third aspect, the present invention discloses an all-solid-state lithium battery, comprising a positive electrode, a negative electrode and a solid electrolyte membrane; the solid electrolyte membrane is arranged between the positive electrode and the negative electrode; the solid electrolyte membrane is the above-mentioned low-impedance NASICON type solid electrolyte membrane.
[0017] In a fourth aspect, the present invention discloses a method for preparing the above-mentioned all-solid-state lithium battery, comprising the following steps:
[0018] Indium tin oxide, nano-scale lithium lanthanum zirconium tantalum oxide powder and polyvinylidene fluoride are mixed, and N-methylpyrrolidone is added to prepare a viscous dilute ceramic slurry using a stirring device; the dilute ceramic slurry is dripped onto the negative electrode side surface of the NASICON solid electrolyte membrane and vacuum dried;
[0019] The positive electrode active material, conductive carbon, nano-scale LATP powder and polyvinylidene fluoride are mixed and then N-methylpyrrolidone is added to prepare a viscous composite positive electrode slurry through high-energy ball milling. The positive electrode slurry is scraped on the positive electrode side surface of the NASICON type solid electrolyte membrane with dilute ceramic slurry and vacuum dried to obtain an ITO / LLZTO@NASICON type solid electrolyte membrane;
[0020] The ITO / LLZTO@NASICON solid electrolyte membrane was assembled into a button-type all-solid-state lithium battery in a glove box, and the assembled button-type all-solid-state lithium battery was transferred to the Joule heating element of the Joule electric heating device for thermal pulse-assisted in-situ alloying and interface thermal welding, and finally an all-solid-state lithium battery was prepared.
[0021] Furthermore, the added mass ratio of indium tin oxide, nano-scale lithium lanthanum zirconium tantalum oxide powder and polyvinylidene fluoride is (0.5-1):(1-3):(0.2-0.5); the solid content of the dilute ceramic slurry is 20wt%-35wt%; and the stirring device is a magnetic stirring device.
[0022] Furthermore, the positive electrode active material is lithium nickel cobalt manganese oxide, lithium iron phosphate, lithium manganese iron phosphate or lithium cobalt oxide; the added mass ratio of the positive electrode active material, conductive carbon, nano-scale LATP powder and polyvinylidene fluoride is 8:1:(4-6):(4-6); the rotation speed of the high-energy ball mill is 500rpm-1000rpm; the coating thickness of the positive electrode slurry is 80 microns-150 microns.
[0023] Furthermore, in the process of using the Joule electric heating device to perform heat pulse-assisted in-situ alloying and interface thermal welding, the voltage is 12V to 32V, the current is 6A to 15A, and the heat treatment time is 5min to 10min.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] The present invention discloses a low-impedance NASICON solid electrolyte membrane and a preparation method thereof. A pre-annealing treatment is performed before rapid Joule heat treatment, and ceramic particles are diffused and reorganized at a mild non-crystallization temperature. The growth internal stress generated by ceramic particles in the rapid Joule heat link during the intense thermal motion is greatly eliminated, so that the NASICON solid electrolyte membrane prepared based on UHS technology has a higher density and mechanical strength, and prevents the generation of micropores, microcracks, and defects. In addition, the present invention designs a mixed powder formula of NASICON solid electrolyte under rapid Joule heat, and the introduction of liquid-phase sintering aids, ion fillers, and fiber-reinforced materials greatly improves the electrochemical performance and metal dendrite suppression ability of the NASICON solid electrolyte membrane, and the bulk defects and crystal interface macropores of the solid electrolyte membrane are almost completely eliminated. Among them, the "concrete" design of the composite of liquid-phase sintering aids and fiber-reinforced materials makes the thermal diffusion process of ceramic particles smoother, the grain boundary distance between each ceramic grain is narrowed, and the puncture and tensile strength of the electrolyte membrane are greatly improved. The introduction of ion fillers reduces the early appearance of the discharge platform and the reduction of discharge capacity caused by concentration polarization during high-rate charge and discharge, while shortening the ion migration path and uniformly increasing the ion migration path. The NASICON solid electrolyte membrane prepared by the present invention based on the rapid Joule heating technology solves the problems of high energy consumption, low production efficiency and serious lithium volatilization of the traditional high-temperature solid-phase sintering process. The prepared solid electrolyte membrane has high structural density and ionic conductivity.
[0026] The present invention discloses an all-solid-state lithium battery and a preparation method thereof. An ITO / LLZTO mixed layer is added to the surface of a prepared NASICON-type membrane to prepare an ITO / LLZTO@NASICON-type solid electrolyte membrane. The introduction of the LLZTO-containing interface layer suppresses adverse interface side reactions (such as the reduction of tetravalent titanium ions) under high reduction potentials and enhances the interface stability of the cycle process. The addition of ITO homogenizes the current density on the surface of the solid electrolyte membrane. In the subsequent battery interface thermal welding process, ITO and Li undergo an in-situ alloying reaction to generate a lithium oxide, Li x In、Li x Sn alloy interlayer, which significantly reduces the interface resistance of solid-state batteries (887Ω / cm 2 -256Ω / cm 2 ), the solid-state lithium battery assembled by the present invention has low impedance, high safety and cycle life. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0028] Figure 1 This is a sintering system diagram of the LATP film and the thermal pulse welding solid-state battery interface prepared based on the improved UHS technology (NUHS) in the embodiment of the present invention, wherein Figure 1 a is the preheating annealing stage system of NUHS technology, Figure 1 b is the rapid hot forming stage system of NUHS technology, Figure 1 c is a thermal pulse welding system for improving the interface contact of solid-state batteries;
[0029] Figure 2 The morphology, structure, and crystallization of the LATP membranes prepared by different sintering methods in the embodiments of the present invention are shown in FIG. Figure 2 (a) Ordinary high temperature sintering, Figure 2 (b) Ordinary Joule heating sintering, Figure 2 (c) To improve the LATP membrane prepared by Joule heating sintering, Figure 2 (d) XRD diffraction patterns of LATP films prepared by three sintering methods. Figure 2 (e) The crystallinity of LATP films prepared by three sintering methods. Figure 2 (f) The average particle size of three LATP films and LATP particles;
[0030] Figure 3 The cross section and surface crystal shape changes of the LATP film during the preparation of the LATP film based on the improved UHS technology (NUHS) according to the embodiment of the present invention;
[0031] Figure 4 The thermal, mechanical strength and roughness tests of LATP films prepared by different sintering methods in the embodiments of the present invention are as follows: Figure 4 (a) is the thermal imaging test image of LATP film prepared by ordinary high-temperature sintering. Figure 4 (b) is the thermal imaging test image of the LATP film prepared by ordinary Joule heating sintering. Figure 4 (c) Thermal imaging test image of LATP film prepared by improved Joule heating sintering. Figure 4 (d) is the puncture test of three membranes. Figure 4 (e) is the Young's modulus test of the three films. Figure 4 (f) Roughness test of three films;
[0032] Figure 5The present invention tests the electrochemical window, electrochemical AC impedance and battery rate of different LATP membranes, wherein Figure 5 (a) The electrochemical windows of three LATP membranes. Figure 5 (b) is the electrochemical impedance curve of three LATP membranes. Figure 5 (c) is the electrochemical impedance of the solid-state battery before and after thermal welding. Figure 5 (d) The capacity level of solid-state batteries made from three types of LATP at a charge and discharge rate of 0.05-0.5C;
[0033] Figure 6 In the present invention, the LATP membranes prepared by different sintering methods were subjected to long cycle tests at a rate of 0.2C, wherein Figure 6 a is the long cycle curve of all-solid-state NCM811 battery equipped with LATP membranes prepared by different sintering methods at 0.2C rate, Figure 6 b is Figure 6 a The first cycle charge and discharge curves of the three all-solid-state batteries in the test. Figure 6 C is the capacity-voltage curve of the all-solid-state NCM811 battery equipped with LATP membrane prepared by improved Joule heating technology at the 1st, 10th, 50th and 100th cycles. Figure 6 d is the long cycle curve of all-solid-state LFP batteries equipped with LATP membranes prepared by different sintering methods at a rate of 0.2C. Figure 6 e is Figure 6 d The first cycle charge and discharge curves of the three all-solid-state batteries in the test. Figure 6 f is the capacity-voltage curve of the all-solid-state LFP battery equipped with LATP membrane prepared by improved Joule heating technology at the 1st, 10th, 50th and 100th cycles. DETAILED DESCRIPTION
[0034] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0035] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0036] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0037] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0038] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0039] The present invention is further described in detail below in conjunction with the accompanying drawings:
[0040] The embodiment of the present invention discloses a low-impedance NASICON solid electrolyte membrane based on improved rapid Joule heating technology (UHS) and a preparation method thereof, wherein the preparation method comprises the following steps:
[0041] S1, mixing a lithium source, an aluminum source and a phosphorus source, adding a titanium source or a germanium source and ball milling; drying and high-temperature solid-phase synthesis of the ball-milled powder in turn to obtain ceramic coarse particles; ball milling, drying and sieving the ceramic coarse particles in turn to obtain NASICON type solid electrolyte powder;
[0042] In this step, the NASICON solid electrolyte powder is lithium aluminum germanium phosphate (Li 1+x Al x Ge 2-x (PO4)3, 0≤x≤1), lithium aluminum titanium phosphate (Li 1+x Al x Ti 2-x(PO4)3,0≤x≤1), wherein the lithium source is lithium carbonate or lithium hydroxide, the aluminum source is aluminum nitrate or aluminum oxide, the phosphorus source is ammonium dihydrogen phosphate or phosphoric acid, the titanium source is tetrabutyl titanate or titanium oxide, and the germanium source is germanium oxide; the addition ratio of each raw material component follows the molar ratio of each element in the chemical formula; the ball milling medium used in the ball milling process is isopropanol or ethanol, and the ball mill speed is 90rpm~500rpm; the specific steps of the high temperature solid phase synthesis are: heating at a heating rate of 4℃ / min~10℃ / min to a roasting temperature of 600℃~900℃ for high temperature solid phase synthesis, the heat preservation time is 6h~8.5h, and then cooling to room temperature at a cooling rate of 8℃ / min~13℃ / min; the screening process uses a nylon mesh screen of 200 mesh~800 mesh for screening.
[0043] S2, adding nano-boron-based liquid phase sintering aid, ion filler and fiber reinforcement material to NASICON solid electrolyte powder and mixing them evenly to obtain a mixture, putting the mixture into a metal mold and pressing it into a ceramic embryo, placing the ceramic embryo in a crucible for annealing treatment, and the annealing heat treatment system is as follows Figure 1 a;
[0044] In this step, the added mass ratio of the boron-based liquid phase sintering aid, the ion filler and the fiber reinforcement material is (1.5-3):1:(0.5-1); the total mass of the boron-based liquid phase sintering aid, the ion filler and the fiber reinforcement material accounts for 1wt%-5wt% of the mass of the mixture; the boron-based liquid phase sintering aid is a mixture of one or more of sodium aluminum borate (Na2B4O7·10H2O), sodium borohydride (NaBH4), ammonium borate nitrate (NH4H2BO3), aluminum triboride (AlB2), and boron oxide (B2O3); the ion filler is lithium tetrafluoroborate (LiBF4), lithium borate (LiB(C2O4)2), lithium nitride (Li3N), lithium titanate (Li4Ti5O 12 ), the fiber reinforcement material is a mixture of one or more of single-walled carbon nanotubes, para-aramid nanofibers, polyimide fibers, boron carbide fibers, and boron fibers; the pressure of the ceramic embryo during the pressing process is 5MPa to 15MPa; the temperature of the annealing treatment is (T c -200)℃~(T c -300)℃,T c The crystallization temperature is the crystallization temperature, the holding time is 2h to 3h, the heating rate is 4℃ / min to 10℃ / min, and the cooling rate is 8℃ / min to 13℃ / min.
[0045] S3, transferring the annealed ceramic body to the Joule heating element of the electric heating device, sintering by rapid Joule heat treatment under a protective atmosphere, cooling to room temperature after the heat treatment to obtain a rough NASICON solid electrolyte membrane, the rapid Joule heat sintering system Figure 1 b.
[0046] In this step, the protective atmosphere is a mixture of one or more of nitrogen, argon or other inert gases; the voltage of Joule heating during the rapid Joule heat treatment is 10V~100V, the heating current is 10A~60A, and the sintering temperature threshold is 800℃~960℃; after the heat treatment, the current is manually adjusted to make the temperature drop slowly and evenly to room temperature to prevent sudden cooling from causing quenching and cracking of the ceramic membrane.
[0047] S4, placing the rough NASICON type solid electrolyte membrane in a metallographic grinding and polishing machine for grinding and polishing, then performing acid immersion treatment on the surface of the solid electrolyte membrane, and then neutralizing it with an alkaline solution and fully rinsing it with ethanol to prepare a low-impedance NASICON type solid electrolyte membrane.
[0048] In this step, the acid used for acid leaching is hydrochloric acid or dilute nitric acid; the alkaline solution used for alkali neutralization is dilute sodium hydroxide solution or sodium bicarbonate solution.
[0049] The embodiment of the present invention discloses an all-solid-state lithium battery and a preparation method thereof. The preparation method of the all-solid-state lithium battery comprises the following steps:
[0050] S1, mixing indium tin oxide (ITO), nano-scale lithium lanthanum zirconium tantalum oxide powder (LLZTO), and polyvinylidene fluoride (PVDF), adding a small amount of N-methylpyrrolidone (NMP), and using a stirring device to prepare a viscous dilute ceramic slurry; dropping the dilute ceramic slurry onto the negative electrode side surface of the NASICON solid electrolyte membrane and vacuum drying;
[0051] In this step, the added mass ratio of indium tin oxide, nano-scale lithium lanthanum zirconium tantalum oxide powder and polyvinylidene fluoride is (0.5-1):(1-3):(0.2-0.5); the solid content of the dilute ceramic slurry is 20wt%-35wt%; and the stirring device is a magnetic stirring device.
[0052] S2, after mixing the positive electrode active material, conductive carbon, nano-LATP powder and polyvinylidene fluoride, adding a small amount of N-methylpyrrolidone (NMP), configuring it into a viscous composite positive electrode slurry through high-energy ball milling, and applying the positive electrode slurry on the positive electrode side surface of the NASICON type solid electrolyte membrane with dilute ceramic slurry prepared in S1 and vacuum drying it to obtain an ITO / LLZTO@NASICON type solid electrolyte membrane;
[0053] In this step, the positive electrode active material is lithium nickel cobalt manganese oxide, lithium iron phosphate, lithium iron manganese phosphate or lithium cobalt oxide; the added mass ratio of the positive electrode active material, conductive carbon, nano-scale LATP powder and polyvinylidene fluoride is 8:1:(4-6):(4-6); the rotation speed of the high-energy ball mill is 500rpm-1000rpm; the coating thickness of the positive electrode slurry is 80 microns-150 microns;
[0054] S3, assemble the ITO / LLZTO@NASICON type solid electrolyte membrane into a button-type all-solid-state lithium battery in a glove box, transfer the assembled button-type all-solid-state lithium battery to the Joule heating element of the Joule electric heating device for heat pulse-assisted in-situ alloying and interface thermal welding, and finally prepare an all-solid-state lithium battery. The interface thermal welding system is shown in Figure 1 c.
[0055] In this step, the voltage of the rapid Joule heat treatment process is 12V to 32V, the current is 6A to 15A, and the heat treatment time is 5min to 10min.
[0056] The present invention provides a method for preparing a NASICON solid electrolyte membrane and an all-solid-state lithium battery based on rapid Joule heating technology, which solves the drawbacks of traditional high-temperature solid-phase sintering process and conventional rapid Joule heat treatment for preparing solid electrolyte membranes. The prepared solid electrolyte membrane and all-solid-state battery have excellent performance. The method has important scientific research value and commercial significance for the promotion of Joule heating technology and the mass production of all-solid-state lithium batteries.
[0057] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0058] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0059] Example 1
[0060] A method for preparing a high-density NASICON solid electrolyte membrane based on improved rapid Joule heating technology (UHS), comprising the following steps:
[0061] Step 1: Take an appropriate amount of lithium aluminum germanium phosphate (Li 1+x Al x Ge 2-x (PO4)3, x = 0) required raw materials, put into a grinding jar and add a number of zirconia balls of different sizes, then put into a ball mill and add isopropanol as a ball milling medium, set the ball milling speed to 100rpm, grind for 13h, after grinding, dry the powder and set the final target roasting temperature of 700℃, the heating rate is 4℃ / min, and perform high temperature solid phase synthesis. After reaching 700℃, keep warm, and set the holding time to 6h. Then gradually cool down, the cooling rate is 8℃ / min, and after cooling, ball mill, dry and screen with a 500-mesh nylon mesh.
[0062] Step 2: Take the NASICON solid electrolyte powder with suitable particle size and high purity obtained in step 1, add nano-boron-based liquid phase sintering aids: sodium aluminum borate (Na2B4O7·10H2O), sodium borohydride (NaBH4), add ion filler: lithium tetrafluoroborate (LiBF4), and add fiber reinforcement material: para-aramid nanofiber, and mix them evenly. The addition ratio of liquid phase sintering aid, ion filler, and fiber reinforcement material is 1.5:1:0.5, and the total mass of the three additives accounts for 2wt% of the mass ratio of the mixture.
[0063] Step 3, taking the mixture mixed evenly in step 2 and putting it into a metal mold, using a hydraulic press with a pressure of 10 MPa to press the powder into a ceramic green body.
[0064] Step 4, placing the ceramic green body obtained in step 3 into a crucible, and heating the green body at (T c The pre-annealing treatment was carried out at -200)℃, the heating rate was 4℃ / min, and after reaching the predetermined temperature, it was kept warm for 2h, and then gradually cooled down at a cooling rate of 8℃ / min.
[0065] Step 5, transfer the ceramic body prepared in step 4 to the Joule heating element of the Joule electric heating device, the Joule heating voltage is set to 60V, and the heating current is 20A. Rapid Joule heat treatment is performed in a neon atmosphere, and the sintering temperature threshold is set to 800°C. After the heat treatment is completed, the current is manually adjusted to slowly cool down to room temperature.
[0066] Step 6, placing the NASICON solid electrolyte membrane obtained in step 5 in a metallographic grinder and polisher for fine grinding and polishing, using hydrochloric acid to acid-immerse the surface of the polished electrolyte membrane to remove carbonate impurities, neutralizing it with sodium bicarbonate solution and rinsing it with ethanol to eliminate moisture and static electricity, and the cleaned electrolyte membrane needs to be vacuum-sealed in a plastic bag using a vacuum heat sealer for protection and storage.
[0067] Step 7, indium tin oxide (ITO), nano-scale lithium lanthanum zirconium tantalum oxide powder (LLZTO), and polyvinylidene fluoride (PVDF) are mixed in a ratio of 0.5:1:0.2, and a small amount of N-methylpyrrolidone (NMP) is added, and a magnetic stirring device is used to prepare a viscous dilute ceramic slurry, the solid content of the dilute ceramic slurry is 20wt%, and the ceramic slurry is dripped onto the negative electrode side surface of the NASICON solid electrolyte membrane and vacuum dried;
[0068] Step 8, lithium nickel cobalt manganese oxide, conductive carbon, nano-scale LATP powder, and polyvinylidene fluoride are mixed in a ratio of 8:1:4:4, and a small amount of N-methylpyrrolidone (NMP) is added, and the mixture is configured into a viscous composite positive electrode slurry by high-energy ball milling. The high-energy ball milling speed is 500 rpm. The modified NASICON solid electrolyte membrane prepared in step 7 is taken, and the positive electrode slurry is scraped on the positive electrode side surface of the NASICON solid electrolyte membrane and vacuum dried. The thickness of the positive electrode slurry scraped is 80 microns, and finally an ITO / LLZTO@NASICON solid electrolyte membrane is prepared;
[0069] Step 9, take the solid electrolyte membrane prepared in step 8 and assemble it into a button-type all-solid-state lithium battery in a glove box, transfer the assembled button-type all-solid-state lithium battery to the Joule heating element of the Joule electric heating device, use 12V voltage / 6A current to perform thermal pulse-assisted in-situ alloying and interface thermal welding, the heat treatment time is 5 minutes, and an all-solid-state lithium battery with low interface and bulk impedance is obtained.
[0070] Example 2
[0071] Step 1: Take an appropriate amount of lithium aluminum titanium phosphate (Li 1+x Al x Ti 2-x (PO4)3, x = 0.5) the required raw materials, put into the grinding jar and add a number of zirconia balls of different sizes, then put into the ball mill and add isopropanol as the ball milling medium, the ball milling speed is set to 300rpm, grind for 10h, after grinding, dry the powder and set the final target roasting temperature of 800℃, the heating rate is 6℃ / min, and high temperature solid phase synthesis is carried out. After reaching 800℃, keep warm, and the holding time is set to 7h. Then gradually cool down, the cooling rate is 9℃ / min, and after cooling, ball mill, dry and screen with a 600 mesh nylon sieve.
[0072] Step 2, take the NASICON solid electrolyte powder with suitable particle size and high purity obtained in step 1, add nano-level boron-based liquid phase sintering aids: ammonium boron nitrate (NH4H2BO3), aluminum triboride (AlB2), add ion fillers: lithium tetrafluoroborate (LiBF4), lithium borate (LiB(C2O4)2), and add fiber reinforcement materials: single-walled carbon nanotubes, and mix them evenly. The addition ratio of liquid phase sintering aid, ion filler, and fiber reinforcement material is 2:1:0.5, and the total mass of the three additives accounts for 2wt% of the mass ratio of the mixture.
[0073] Step 3, taking the mixture mixed evenly in step 2 and putting it into a metal mold, using a hydraulic press at a pressure of 9 MPa to press the powder into a ceramic green body.
[0074] Step 4, placing the ceramic green body obtained in step 3 into a crucible, and heating the green body at (T c The pre-annealing treatment was carried out at -250)℃, the heating rate was 6℃ / min, and after reaching the predetermined temperature, it was kept warm for 2.5h, and then gradually cooled down at a cooling rate of 9℃ / min.
[0075] Step 5, transfer the ceramic body prepared in step 4 to the Joule heating element of the Joule electric heating device, the Joule heating voltage is set to 80V, and the heating current is 20A. Rapid Joule heat treatment is performed in a nitrogen atmosphere, and the sintering temperature threshold is set to 900°C. After the heat treatment is completed, the current is manually adjusted to slowly cool down to room temperature.
[0076] Step 6, placing the NASICON solid electrolyte membrane obtained in step 5 in a metallographic grinding and polishing machine for fine grinding and polishing, using dilute nitric acid to acid-immerse the polished electrolyte membrane surface to remove carbonate impurities, using dilute sodium hydroxide solution to neutralize and rinse with ethanol to eliminate moisture and static electricity, and the cleaned electrolyte membrane needs to be vacuum-sealed in a plastic bag using a vacuum heat sealer for protection and storage.
[0077] Step 7, indium tin oxide (ITO), nano-scale lithium lanthanum zirconium tantalum oxide powder (LLZTO), and polyvinylidene fluoride (PVDF) are mixed in a ratio of 0.571:1.286:0.243, and a small amount of N-methylpyrrolidone (NMP) is added, and a magnetic stirring device is used to prepare a viscous dilute ceramic slurry, the solid content of the dilute ceramic slurry is 22.4wt%, and the ceramic slurry is dripped onto the negative electrode side surface of the NASICON solid electrolyte membrane and vacuum dried;
[0078] Step 8, lithium iron phosphate, conductive carbon, nano-scale LATP powder, and polyvinylidene fluoride are mixed in a ratio of 8:1:4.286:4.286, and a small amount of N-methylpyrrolidone (NMP) is added, and the mixture is configured into a viscous composite positive electrode slurry by high-energy ball milling. The high-energy ball milling speed is 572 rpm. The modified NASICON solid electrolyte membrane prepared in step 7 is taken, and the positive electrode slurry is scraped on the positive electrode side surface of the NASICON solid electrolyte membrane and vacuum dried. The thickness of the positive electrode slurry scraped is 90 microns, and finally an ITO / LLZTO@NASICON solid electrolyte membrane is prepared;
[0079] Step 9, take the solid electrolyte membrane prepared in step 8 and assemble it into a button-type all-solid-state lithium battery in a glove box, transfer the assembled button-type all-solid-state lithium battery to the Joule heating element of the Joule electric heating device, control the voltage of 14.8V / the current of 7.2A to perform thermal pulse-assisted in-situ alloying and interface thermal welding, the heat treatment time is 5.7min, and an all-solid-state lithium battery with low interface and bulk impedance is obtained.
[0080] Example 3
[0081] Step 1: Take an appropriate amount of lithium aluminum titanium phosphate (Li 1+x Al x Ti 2-x (PO4)3, x = 0.3) The required raw materials are placed in a grinding jar and a number of zirconia balls of varying sizes are added. Then, they are placed in a ball mill and isopropanol is added as a ball milling medium. The ball milling speed is set to 400rpm and the grinding is performed for 10 hours. After grinding, the powder is dried and the final target roasting temperature of 800°C is set. The heating rate is 8°C / min for high-temperature solid phase synthesis. After reaching 900°C, the temperature is kept at 7.5h. Then the temperature is gradually lowered at a cooling rate of 10°C / min. After cooling, the powder is ball milled, dried, and sieved using a 700-mesh nylon sieve.
[0082] Step 2: Take the NASICON solid electrolyte powder with suitable particle size and high purity obtained in step 1, add nano-boron-based liquid phase sintering aids: sodium aluminum borate (Na2B4O7·10H2O), boron oxide (B2O3), and add ion fillers: lithium nitride (Li3N), lithium titanate (Li4Ti5O 12 ), and fiber reinforcement materials: single-walled carbon nanotubes and polyimide fibers are added and mixed evenly. The addition ratio of liquid phase sintering aid, ion filler and fiber reinforcement material is 3:1:1, and the total mass of the three additives accounts for 3wt% of the mass ratio of the mixture.
[0083] Step 3, taking the mixture mixed evenly in step 2 and putting it into a metal mold, using a hydraulic press at a pressure of 13 MPa to press the powder into a ceramic green body.
[0084] Step 4, placing the ceramic green body obtained in step 3 into a crucible, and heating the green body at (T c The pre-annealing treatment was carried out at -300)℃, the heating rate was 8℃ / min, and after reaching the predetermined temperature, it was kept warm for 3h, and then gradually cooled down at a cooling rate of 10℃ / min.
[0085] Step 5: transfer the ceramic body prepared in step 4 to the Joule heating element of the Joule electric heating device, and set the Joule heating voltage to 80V and the heating current to 40A. Perform rapid Joule heat treatment in a nitrogen atmosphere, and set the sintering temperature threshold to 910°C. After the heat treatment, manually adjust the current to slowly cool down to room temperature.
[0086] Step 6, placing the NASICON solid electrolyte membrane obtained in step 5 in a metallographic grinding and polishing machine for fine grinding and polishing, using dilute nitric acid to acid-immerse the polished electrolyte membrane surface to remove carbonate impurities, using dilute sodium hydroxide solution to neutralize and rinse with ethanol to eliminate moisture and static electricity, and the cleaned electrolyte membrane needs to be vacuum-sealed in a plastic bag using a vacuum heat sealer for protection and storage.
[0087] Step 7, indium tin oxide (ITO), nano-scale lithium lanthanum zirconium tantalum oxide powder (LLZTO), and polyvinylidene fluoride (PVDF) are mixed in a ratio of 0.642:1.572:0.286, and a small amount of N-methylpyrrolidone (NMP) is added, and a magnetic stirring device is used to prepare a viscous dilute ceramic slurry, the solid content of the dilute ceramic slurry is 24.28wt%, and the ceramic slurry is dripped onto the negative electrode side surface of the NASICON solid electrolyte membrane and vacuum dried;
[0088] Step 8, lithium iron manganese phosphate, conductive carbon, nano-scale LATP powder, and polyvinylidene fluoride are mixed in a ratio of 8:1:4.572:4.572, and a small amount of N-methylpyrrolidone (NMP) is added, and a viscous composite positive electrode slurry is prepared by high-energy ball milling. The high-energy ball milling speed is 640 rpm. The modified NASICON solid electrolyte membrane prepared in step 7 is taken, and the positive electrode slurry is scraped on the positive electrode side surface of the NASICON solid electrolyte membrane and vacuum dried. The positive electrode slurry is scraped to a thickness of 100 microns, and finally an ITO / LLZTO@NASICON solid electrolyte membrane is prepared;
[0089] Step 9, take the solid electrolyte membrane prepared in step 8 and assemble it into a button-type all-solid-state lithium battery in a glove box, transfer the assembled button-type all-solid-state lithium battery to the Joule heating element of the Joule electric heating device, control the voltage of 17.7V / 8.5A current to perform thermal pulse-assisted in-situ alloying and interface thermal welding, the heat treatment time is 6.4min, and an all-solid-state lithium battery with low interface and bulk impedance is obtained.
[0090] Example 4
[0091] Step 1: Take an appropriate amount of lithium aluminum germanium phosphate (Li 1+x Al x Ge 2-x (PO4)3, x = 0.7) the required raw materials, put into a grinding jar and add a number of zirconia balls of different sizes, then put into a ball mill and add isopropanol as a ball milling medium, set the ball milling speed to 500rpm, grind for 10h, after grinding, dry the powder and set the final target roasting temperature of 800℃, the heating rate is 9℃ / min, and perform high temperature solid phase synthesis. After reaching 900℃, keep warm, and set the holding time to 8h. Then gradually cool down, the cooling rate is 12℃ / min, and after cooling, ball mill, dry and screen with 800 mesh nylon sieve.
[0092] Step 2, take the NASICON solid electrolyte powder with suitable particle size and high purity obtained in step 1, add nano-scale boron-based liquid phase sintering aids: ammonium boron nitrate (NH4H2BO3), aluminum triboride (AlB2), boron oxide (B2O3), add ion fillers: lithium tetrafluoroborate (LiBF4), lithium borate (LiB(C2O4)2), lithium nitride (Li3N), and add fiber reinforcement materials: polyimide fiber, boron carbide fiber, and mix them evenly. The addition ratio of liquid phase sintering aid, ion filler, and fiber reinforcement material is 2:1:1, and the total mass of the three additives accounts for 4wt% of the mass ratio of the mixture.
[0093] Step 3, taking the mixture mixed evenly in step 2 and putting it into a metal mold, using a hydraulic press to press the mixture into a ceramic green body, and the pressure during the pressing process of the ceramic green body is 15 MPa.
[0094] Step 4, placing the ceramic green body obtained in step 3 into a crucible, pre-annealing the green body at (Tc-200)°C, heating rate of 9°C / min, keeping the temperature for 3h after reaching the predetermined temperature, and then gradually cooling at a cooling rate of 12°C / min.
[0095] Step 5, transfer the ceramic body prepared in step 4 to the Joule heating element of the Joule electric heating device, the Joule heating voltage is set to 100V, and the heating current is 50A. Rapid Joule heat treatment is performed in an argon atmosphere, and the sintering temperature threshold is set to 960°C. After the heat treatment is completed, the current is manually adjusted to slowly cool down to room temperature.
[0096] Step 6, placing the NASICON solid electrolyte membrane obtained in step 5 in a metallographic grinding and polishing machine for fine grinding and polishing, using hydrochloric acid to acid-immerse the surface of the polished electrolyte membrane to remove carbonate impurities, using a dilute sodium hydroxide solution to neutralize and rinse with ethanol to eliminate moisture and static electricity, and the cleaned electrolyte membrane needs to be vacuum-sealed in a plastic bag using a vacuum heat sealer for protection and storage.
[0097] Step 7, indium tin oxide (ITO), nano-scale lithium lanthanum zirconium tantalum oxide powder (LLZTO), and polyvinylidene fluoride (PVDF) are mixed in a ratio of 0.713:1.858:0.329, and a small amount of N-methylpyrrolidone (NMP) is added, and a magnetic stirring device is used to prepare a viscous dilute ceramic slurry, the solid content of the dilute ceramic slurry is 26.42wt%, and the ceramic slurry is dripped onto the negative electrode side surface of the NASICON solid electrolyte membrane and vacuum dried;
[0098] Step 8, lithium cobalt oxide, conductive carbon, nano-scale LATP powder, and polyvinylidene fluoride are mixed in a ratio of 8:1:4.858:4.858, and a small amount of N-methylpyrrolidone (NMP) is added, and the mixture is configured into a viscous composite positive electrode slurry by high-energy ball milling. The high-energy ball milling speed is 714 rpm. The modified NASICON solid electrolyte membrane prepared in step 7 is taken, and the positive electrode slurry is scraped on the positive electrode side surface of the NASICON solid electrolyte membrane and vacuum dried. The thickness of the positive electrode slurry scraped is 110 microns, and finally an ITO / LLZTO@NASICON solid electrolyte membrane is prepared;
[0099] Step 9, take the solid electrolyte membrane prepared in step 8 and assemble it into a button-type all-solid-state lithium battery in a glove box, transfer the assembled button-type all-solid-state lithium battery to the Joule heating element of the Joule electric heating device, control the voltage of 20.5V / 9.8A current to perform thermal pulse-assisted in-situ alloying and interface thermal welding, the heat treatment time is 7.1min, and an all-solid-state lithium battery with low interface and bulk impedance is obtained.
[0100] Example 5
[0101] Step 1: Take an appropriate amount of lithium aluminum germanium phosphate (Li 1+x Al x Ge 2-x(PO4)3, x = 0.9) The required raw materials are placed in a grinding jar and several zirconia balls of different sizes are added. Then the mixture is placed in a ball mill and ethanol is added as a ball milling medium. The ball milling speed is set to 500rpm and the powder is ground for 10 hours. After grinding, the powder is dried. The target calcination temperature is set to 900°C and the heating rate is 10°C / min for high-temperature solid-phase synthesis. After reaching 900°C, the temperature is kept at 7h. Then the temperature is gradually lowered at a cooling rate of 13°C / min. After cooling, the mixture is ball milled, dried and sieved using an 800-mesh nylon mesh.
[0102] Step 2: Take the high-purity, nano-scale NASICON solid electrolyte powder obtained in step 1, add nano-scale boron-based liquid phase sintering aids: ammonium borate nitrate (NH4H2BO3), aluminum triboride (AlB2), boron oxide (B2O3), add ion fillers: lithium nitride (Li3N), lithium titanate (Li4Ti5O 12 ), and fiber reinforcement materials: single-walled carbon nanotubes and para-aramid nanofibers are added and mixed evenly. The addition ratio of liquid phase sintering aid, ion filler and fiber reinforcement material is 1.5:1:0.5, and the total mass of the three additives accounts for 4wt% of the mass ratio of the mixture.
[0103] Step 3, taking the mixture mixed evenly in step 2 and putting it into a metal mold, using a hydraulic press to press the mixture into a ceramic green body, and the pressure during the pressing process of the ceramic green body is 15 MPa.
[0104] Step 4, placing the ceramic green body obtained in step 3 in a crucible, pre-annealing the green body at (Tc-200)°C, heating rate of 8°C / min, keeping the temperature for 3h after reaching the predetermined temperature, and then gradually cooling at a cooling rate of 11°C / min.
[0105] Step 5, transfer the ceramic body prepared in step 4 to the Joule heating element of the Joule electric heating device, the Joule heating voltage is set to 100V, and the heating current is 60A. Rapid Joule heat treatment is performed in an argon atmosphere, and the sintering temperature threshold is set to 960°C. After the heat treatment is completed, the current is manually adjusted to slowly cool down to room temperature.
[0106] Step 6, placing the NASICON solid electrolyte membrane obtained in step 5 in a metallographic grinding and polishing machine for fine grinding and polishing, using hydrochloric acid to acid-immerse the surface of the polished electrolyte membrane to remove carbonate impurities, neutralizing it with sodium bicarbonate solution and rinsing it with ethanol to eliminate moisture and static electricity, and the cleaned electrolyte membrane needs to be vacuum-sealed in a plastic bag using a vacuum heat sealer for protection and storage.
[0107] Step 7, indium tin oxide (ITO), nano-scale lithium lanthanum zirconium tantalum oxide powder (LLZTO), and polyvinylidene fluoride (PVDF) are mixed in a ratio of 0.784:2.144:0.372, and a small amount of N-methylpyrrolidone (NMP) is added, and a magnetic stirring device is used to prepare a viscous dilute ceramic slurry, the solid content of the dilute ceramic slurry is 28.56wt%, and the ceramic slurry is dripped onto the negative electrode side surface of the NASICON solid electrolyte membrane and vacuum dried;
[0108] Step 8, lithium nickel cobalt manganese oxide, conductive carbon, nano-scale LATP powder, and polyvinylidene fluoride are mixed in a ratio of 8:1:5.144:5.144, and a small amount of N-methylpyrrolidone (NMP) is added, and a viscous composite positive electrode slurry is prepared by high-energy ball milling. The high-energy ball milling speed is 786 rpm. The modified NASICON solid electrolyte membrane prepared in step 7 is taken, and the positive electrode slurry is scraped on the positive electrode side surface of the NASICON solid electrolyte membrane and vacuum dried. The thickness of the positive electrode slurry scraped is 120 microns, and finally an ITO / LLZTO@NASICON solid electrolyte membrane is prepared;
[0109] Step 9, take the solid electrolyte membrane prepared in step 8 and assemble it into a button-type all-solid-state lithium battery in a glove box, transfer the assembled button-type all-solid-state lithium battery to the Joule heating element of the Joule electric heating device, control the voltage of 23.4V / 11.1A current to perform thermal pulse-assisted in-situ alloying and interface thermal welding, the heat treatment time is 7.8min, and an all-solid-state lithium battery with low interface and bulk impedance is obtained.
[0110] Example 6
[0111] Step 1: Take an appropriate amount of lithium aluminum germanium phosphate (Li 1+x Al x Ge 2-x (PO4)3, x = 0.5) the required raw materials, put into the grinding jar and add a number of zirconia balls of different sizes, then put into the ball mill and add isopropanol as the ball milling medium, the ball milling speed is set to 500rpm, grind for 10h, after grinding, dry the powder and set the final target roasting temperature of 800℃, the heating rate is 9℃ / min, and high temperature solid phase synthesis is carried out. After reaching 900℃, keep warm, and the holding time is set to 8h. Then gradually cool down, the cooling rate is 12℃ / min, and after cooling, ball mill, dry and screen with 800 mesh nylon sieve.
[0112] Step 2, take the NASICON solid electrolyte powder with suitable particle size and high purity obtained in step 1, add nano-scale boron-based liquid phase sintering aids: ammonium boron nitrate (NH4H2BO3), aluminum triboride (AlB2), boron oxide (B2O3), add ion fillers: lithium tetrafluoroborate (LiBF4), lithium borate (LiB(C2O4)2), lithium nitride (Li3N), and add fiber reinforcement materials: polyimide fiber, boron carbide fiber, and mix them evenly. The addition ratio of liquid phase sintering aid, ion filler, and fiber reinforcement material is 2:1:1, and the total mass of the three additives accounts for 4wt% of the mass ratio of the mixture.
[0113] Step 3, taking the mixture mixed evenly in step 2 and putting it into a metal mold, using a hydraulic press to press the mixture into a ceramic green body, and the pressure during the pressing process of the ceramic green body is 15 MPa.
[0114] Step 4, placing the ceramic green body obtained in step 3 into a crucible, and heating the green body at (T c The pre-annealing treatment was carried out at -200)℃, the heating rate was 9℃ / min, and after reaching the predetermined temperature, it was kept warm for 3h, and then gradually cooled down at a cooling rate of 12℃ / min.
[0115] Step 5, transfer the ceramic body prepared in step 4 to the Joule heating element of the Joule electric heating device, the Joule heating voltage is set to 100V, and the heating current is 50A. Rapid Joule heat treatment is performed in an argon atmosphere, and the sintering temperature threshold is set to 960°C. After the heat treatment is completed, the current is manually adjusted to slowly cool down to room temperature.
[0116] Step 6, placing the NASICON solid electrolyte membrane obtained in step 5 in a metallographic grinding and polishing machine for fine grinding and polishing, using hydrochloric acid to acid-immerse the surface of the polished electrolyte membrane to remove carbonate impurities, using a dilute sodium hydroxide solution to neutralize and rinse with ethanol to eliminate moisture and static electricity, and the cleaned electrolyte membrane needs to be vacuum-sealed in a plastic bag using a vacuum heat sealer for protection and storage.
[0117] Step 7, indium tin oxide (ITO), nano-scale lithium lanthanum zirconium tantalum oxide powder (LLZTO), and polyvinylidene fluoride (PVDF) are mixed in a ratio of 0.855:2.43:0.415, and a small amount of N-methylpyrrolidone (NMP) is added, and a magnetic stirring device is used to prepare a viscous dilute ceramic slurry, the solid content of the dilute ceramic slurry is 30.7wt%, and the ceramic slurry is dripped onto the negative electrode side surface of the NASICON solid electrolyte membrane and vacuum dried;
[0118] Step 8, lithium iron phosphate, conductive carbon, nano-scale LATP powder, and polyvinylidene fluoride are mixed in a ratio of 8:1:5.43:5.43, and a small amount of N-methylpyrrolidone (NMP) is added, and the mixture is configured into a viscous composite positive electrode slurry by high-energy ball milling. The high-energy ball milling speed is 857 rpm. The modified NASICON solid electrolyte membrane prepared in step 7 is taken, and the positive electrode slurry is scraped on the positive electrode side surface of the NASICON solid electrolyte membrane and vacuum dried. The thickness of the positive electrode slurry scraped is 130 microns, and finally an ITO / LLZTO@NASICON solid electrolyte membrane is prepared;
[0119] Step 9, take the solid electrolyte membrane prepared in step 8 and assemble it into a button-type all-solid-state lithium battery in a glove box, transfer the assembled button-type all-solid-state lithium battery to the Joule heating element of the Joule electric heating device, control the voltage of 26.2V / 12.4A current to perform thermal pulse-assisted in-situ alloying and interface thermal welding, the heat treatment time is 8.5min, and an all-solid-state lithium battery with low interface and bulk impedance is obtained.
[0120] Example 7
[0121] Step 1: Take an appropriate amount of lithium aluminum titanium phosphate (Li 1+x Al x Ti 2-x (PO4)3, x=1) The required raw materials are placed in a grinding jar and several zirconia balls of different sizes are added. Then, they are placed in a ball mill and isopropanol is added as a ball milling medium. The ball milling speed is set to 400rpm and the grinding is performed for 10 hours. After grinding, the powder is dried and the final target roasting temperature of 800℃ is set. The heating rate is 8℃ / min for high-temperature solid phase synthesis. After reaching 900℃, the temperature is kept at 7.5h. Then the temperature is gradually lowered at a cooling rate of 10℃ / min. After cooling, the powder is ball milled, dried and sieved using a 700-mesh nylon sieve.
[0122] Step 2: Take the NASICON solid electrolyte powder with suitable particle size and high purity obtained in step 1, add nano-boron-based liquid phase sintering aid: sodium aluminum borate (Na2B4O7·10H2O), add ion fillers: lithium nitride (Li3N), lithium titanate (Li4Ti5O 12 ), and fiber reinforcement materials: single-walled carbon nanotubes and polyimide fibers are added and mixed evenly. The addition ratio of liquid phase sintering aid, ion filler and fiber reinforcement material is 3:1:1, and the total mass of the three additives accounts for 3wt% of the mass ratio of the mixture.
[0123] Step 3, taking the mixture mixed evenly in step 2 and putting it into a metal mold, using a hydraulic press at a pressure of 13 MPa to press the powder into a ceramic green body.
[0124] Step 4, placing the ceramic green body obtained in step 3 into a crucible, pre-annealing the green body at (Tc-300)°C, heating rate of 8°C / min, keeping the temperature for 3h after reaching the predetermined temperature, and then gradually cooling at a cooling rate of 10°C / min.
[0125] Step 5: transfer the ceramic body prepared in step 4 to the Joule heating element of the Joule electric heating device, and set the Joule heating voltage to 80V and the heating current to 40A. Perform rapid Joule heat treatment in a nitrogen atmosphere, and set the sintering temperature threshold to 910°C. After the heat treatment, manually adjust the current to slowly cool down to room temperature.
[0126] Step 6, placing the NASICON solid electrolyte membrane obtained in step 5 in a metallographic grinding and polishing machine for fine grinding and polishing, using dilute nitric acid to acid-immerse the polished electrolyte membrane surface to remove carbonate impurities, using dilute sodium hydroxide solution to neutralize and rinse with ethanol to eliminate moisture and static electricity, and the cleaned electrolyte membrane needs to be vacuum-sealed in a plastic bag using a vacuum heat sealer for protection and storage.
[0127] Step 7, indium tin oxide (ITO), nano-scale lithium lanthanum zirconium tantalum oxide powder (LLZTO), and polyvinylidene fluoride (PVDF) are mixed in a ratio of 0.926:2.716:0.458, and a small amount of N-methylpyrrolidone (NMP) is added, and a magnetic stirring device is used to prepare a viscous dilute ceramic slurry, the solid content of the dilute ceramic slurry is 32.84wt%, and the ceramic slurry is dripped onto the negative electrode side surface of the NASICON solid electrolyte membrane and vacuum dried;
[0128] Step 8, lithium manganese iron phosphate, conductive carbon, nano-scale LATP powder, and polyvinylidene fluoride are mixed in a ratio of 8:1:5.716:5.716, and a small amount of N-methylpyrrolidone (NMP) is added, and the mixture is configured into a viscous composite positive electrode slurry by high-energy ball milling. The high-energy ball milling speed is 929 rpm. The modified NASICON solid electrolyte membrane obtained in step 7 is taken, and the positive electrode slurry is scraped on the positive electrode side surface of the NASICON solid electrolyte membrane and vacuum dried. The thickness of the positive electrode slurry scraped is 140 microns, and finally an ITO / LLZTO@NASICON solid electrolyte membrane is obtained;
[0129] Step 9, take the solid electrolyte membrane prepared in step 8 and assemble it into a button-type all-solid-state lithium battery in a glove box, transfer the assembled button-type all-solid-state lithium battery to the Joule heating element of the Joule electric heating device, control the voltage of 29.1V / the current of 13.7A to perform thermal pulse-assisted in-situ alloying and interface thermal welding, the heat treatment time is 9.2min, and an all-solid-state lithium battery with low interface and bulk impedance is obtained.
[0130] Example 8
[0131] Step 1: Take an appropriate amount of lithium aluminum germanium phosphate (Li 1+x Al x Ge 2-x (PO4) 3, x=0.4) required raw materials, put them into a grinding jar and add several zirconia balls of different sizes, then put the mixture into a ball mill and add ethanol as a ball milling medium, set the ball milling speed to 500rpm, grind for 10h, and after grinding, dry the powder. Set the target roasting temperature to 900℃, the heating rate to 10℃ / min, and perform high-temperature solid phase synthesis. After reaching 900℃, keep warm, and set the holding time to 7h. Then gradually cool down, the cooling rate is 13℃ / min, and after cooling, ball mill, dry and sieve with an 800-mesh nylon mesh.
[0132] Step 2: Take the high-purity, nano-scale NASICON solid electrolyte powder obtained in step 1, add nano-scale boron-based liquid phase sintering aids: ammonium borate nitrate (NH4H2BO3), aluminum triboride (AlB2), and add ion fillers: lithium nitride (Li3N), lithium titanate (Li4Ti5O 12 ), and fiber reinforcement materials: single-walled carbon nanotubes and para-aramid nanofibers are added and mixed evenly. The addition ratio of liquid phase sintering aid, ion filler and fiber reinforcement material is 1.5:1:0.5, and the total mass of the three additives accounts for 4wt% of the mass ratio of the mixture.
[0133] Step 3, taking the mixture mixed evenly in step 2 and putting it into a metal mold, using a hydraulic press to press the mixture into a ceramic green body, and the pressure during the pressing process of the ceramic green body is 15 MPa.
[0134] Step 4, placing the ceramic green body obtained in step 3 in a crucible, pre-annealing the green body at (Tc-200)°C, heating rate of 8°C / min, keeping the temperature for 3h after reaching the predetermined temperature, and then gradually cooling at a cooling rate of 11°C / min.
[0135] Step 5, transfer the ceramic body prepared in step 4 to the Joule heating element of the Joule electric heating device, the Joule heating voltage is set to 100V, and the heating current is 60A. Rapid Joule heat treatment is performed in an argon atmosphere, and the sintering temperature threshold is set to 960°C. After the heat treatment is completed, the current is manually adjusted to slowly cool down to room temperature.
[0136] Step 6, placing the NASICON solid electrolyte membrane obtained in step 5 in a metallographic grinding and polishing machine for fine grinding and polishing, using hydrochloric acid to acid-immerse the surface of the polished electrolyte membrane to remove carbonate impurities, neutralizing it with sodium bicarbonate solution and rinsing it with ethanol to eliminate moisture and static electricity, and the cleaned electrolyte membrane needs to be vacuum-sealed in a plastic bag using a vacuum heat sealer for protection and storage.
[0137] Step 7, indium tin oxide (ITO), nano-scale lithium lanthanum zirconium tantalum oxide powder (LLZTO), and polyvinylidene fluoride (PVDF) are mixed in a ratio of 1:3:0.5, and a small amount of N-methylpyrrolidone (NMP) is added, and a magnetic stirring device is used to prepare a viscous dilute ceramic slurry with a solid content of 35wt%, and the ceramic slurry is dripped onto the negative electrode side surface of the NASICON solid electrolyte membrane and vacuum dried;
[0138] Step 8, lithium cobalt oxide, conductive carbon, nano-scale LATP powder, and polyvinylidene fluoride are mixed in a ratio of 8:1:6:6, and a small amount of N-methylpyrrolidone (NMP) is added, and the mixture is configured into a viscous composite positive electrode slurry by high-energy ball milling, and the high-energy ball milling speed is 1000 rpm. The modified NASICON solid electrolyte membrane obtained in step 7 is taken, and the positive electrode slurry is scraped on the positive electrode side surface of the NASICON solid electrolyte membrane and vacuum dried. The thickness of the positive electrode slurry scraped is 150 microns, and finally an ITO / LLZTO@NASICON solid electrolyte membrane is obtained;
[0139] Step 9, take the solid electrolyte membrane prepared in step 8 and assemble it into a button-type all-solid-state lithium battery in a glove box, transfer the assembled button-type all-solid-state lithium battery to the Joule heating element of the Joule electric heating device, control the voltage of 32V / the current of 15A to perform thermal pulse-assisted in-situ alloying and interface thermal welding, the heat treatment time is 10 minutes, and an all-solid-state lithium battery with low interface and bulk impedance is obtained.
[0140] Example 9
[0141] The difference from Example 8 is that the NASICON solid electrolyte is lithium aluminum germanium phosphate (Li 1+x Al x Ge 2-x (PO4)3, x=0.6), and lithium tetrafluoroborate (LiBF4) is used as the ion filler.
[0142] Example 10
[0143] The difference from Example 9 is that the nano-boron-based liquid phase sintering aid is sodium aluminum borate (Na2B4O7·10H2O), and the ion filler is lithium titanate (Li4Ti5O 12 ).
[0144] Embodiment 11
[0145] The difference from Example 10 is that the voltage of Joule heating is 70V, the heating current is 50A, and the sintering temperature threshold is 880°C.
[0146] Example 12
[0147] The difference from Example 11 is that the positive electrode active material used in step 8 is lithium nickel cobalt manganese oxide.
[0148] Embodiment 13
[0149] The difference from Example 12 is that the high-energy ball milling speed in step 8 is 800 rpm.
[0150] Embodiment 14
[0151] The difference from Example 13 is that the voltage used in the heat treatment process in step 9 is 20V, the current used is 10A, and the treatment time is 8 minutes.
[0152] Through the above steps, NASICON solid electrolyte membrane with high structural density and high ionic conductivity and all-solid-state lithium battery with high energy density, good safety performance and long cycle life can be obtained. This battery has important scientific research value and good market application potential, and can effectively meet the development needs of various fields.
[0153] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
[0154] Comparative Example 1
[0155] The LATP membrane is prepared by ordinary high-temperature sintering method. The specific steps are as follows:
[0156] Step 1: Take an appropriate amount of lithium aluminum titanium phosphate (Li 1+x Al x Ti 2-x (PO4)3, x = 0.5) the required raw materials, put into a grinding jar and add a number of zirconia balls of different sizes, then put into a ball mill and add isopropanol as a ball milling medium, set the ball milling speed to 300rpm, and grind for 10h. After grinding, the powder is dried. Set the final target roasting temperature of 800℃, the heating rate is 6℃ / min, and high-temperature solid phase synthesis is carried out. After reaching 800℃, keep warm, and the insulation time is set to 7h. Then gradually cool down, the cooling rate is 9℃ / min, and after cooling, it is ball milled, dried and sieved with a 600-mesh nylon mesh.
[0157] Step 2: Take an appropriate amount of the NASICON solid electrolyte powder with suitable particle size and high purity obtained in step 1, put it into a metal mold, and use a hydraulic press to press the ceramic powder into a ceramic green body at a pressure of 10 MPa.
[0158] Step 3: Put the ceramic green body obtained in step 2 into a crucible, cover the surface with a layer of NASICON powder obtained in step 1, place the ceramic green body in a muffle furnace and heat the temperature from 20°C to 950°C at a rate of 5°C / min, keep it at this temperature for 6 hours, and then reduce the temperature to room temperature at a rate of 4°C / min.
[0159] Step 4: Place the NASICON solid electrolyte membrane obtained in step 3 in a metallographic grinder and polisher for fine grinding and polishing. Use dilute hydrochloric acid to acid-immerse the polished electrolyte membrane surface to remove carbonate impurities. Use dilute sodium hydroxide solution to neutralize and rinse with ethanol to eliminate moisture and static electricity. The cleaned electrolyte membrane needs to be vacuum-sealed in a plastic bag using a vacuum heat sealer for protection and storage.
[0160] Comparative Example 2
[0161] The LATP membrane was prepared by ordinary Joule heating sintering method. The specific steps are as follows:
[0162] Step 1: Take an appropriate amount of lithium aluminum titanium phosphate (Li 1+x Al x Ti 2-x (PO4)3, x = 0.5) the required raw materials, put into a grinding jar and add a number of zirconia balls of different sizes, then put into a ball mill and add isopropanol as a ball milling medium, set the ball milling speed to 300rpm, and grind for 10h. After grinding, the powder is dried. Set the final target roasting temperature of 800℃, the heating rate is 6℃ / min, and high-temperature solid phase synthesis is carried out. After reaching 800℃, keep warm, and the insulation time is set to 7h. Then gradually cool down, the cooling rate is 9℃ / min, and after cooling, it is ball milled, dried and sieved with a 600-mesh nylon mesh.
[0163] Step 2: Take an appropriate amount of the NASICON solid electrolyte powder with suitable particle size and high purity obtained in step 1, put it into a metal mold, and use a hydraulic press to press the ceramic powder into a ceramic green body at a pressure of 10 MPa.
[0164] Step 3: The ceramic green body prepared in step 2 is transferred to the Joule heating element of the Joule electric heating device. The Joule heating voltage is set to 80V and the heating current is 20A. Rapid Joule heat treatment is performed in a nitrogen atmosphere. The sintering temperature threshold is set to 920°C. After the heat treatment is completed, the current is manually adjusted to slowly cool down to room temperature.
[0165] Step 4: Place the NASICON solid electrolyte membrane obtained in step 3 in a metallographic grinder and polisher for fine grinding and polishing. Use dilute hydrochloric acid to acid-immerse the polished electrolyte membrane surface to remove carbonate impurities. Use dilute sodium hydroxide solution to neutralize and rinse with ethanol to eliminate moisture and static electricity. The cleaned electrolyte membrane needs to be vacuum-sealed in a plastic bag using a vacuum heat sealer for protection and storage.
[0166] The microscopic morphologies of the LATP membranes prepared in Comparative Example 1, Comparative Example 2 and Example 2 are as follows: Figure 2 As shown in a, b, and c, the LATP membrane (LATP-CHST) prepared based on high temperature sintering technology produces heterogeneous decomposition products during long sintering time, which are wrapped on the surface of LATP ceramic particles ( Figure 2 a). The LATP membrane (LATP-CUHS) prepared based on conventional rapid Joule heating technology has a regular ceramic particle structure and a relatively uniform arrangement, but there are large intercrystalline gaps between the LATP particles, which may lead to higher intercrystalline electrochemical impedance, which is not conducive to rapid lithium ion migration and diffusion ( Figure 2 b). Compared with the LATP membranes prepared by the first two methods, the LATP membrane (LATP-NUHS) prepared by the improved rapid Joule heating technology has a dense and uniform surface structure, the ceramic particles are in close contact, and there is no accumulation of decomposition products on the surface. X-ray diffraction tests were performed on the three samples to analyze the crystal structure, such as Figure 2 As shown in Figure d, the test found that the peak shapes of the two LATP films prepared based on the rapid Joule heating technology are basically consistent with the LATP standard spectrum (#35-0574), which indicates that the rapid Joule heating technology will not cause changes in the crystal phase structure. Among them, the peak shape of LATP-NUHS at the 104 / 113 / 024 crystal plane is slender, indicating good crystallinity and high LATP phase content. In contrast, LATP-CHST has more impurity peaks in the XRD spectrum, confirming Figure 2 The substance wrapped on the membrane surface in a is the product of heterogeneous decomposition. The XRD pattern is fitted and analyzed, as shown in Figure 2 e. Figure 2 As shown in figure f, the average grain sizes of LATP-CUHS, LATP-CHST and LATP-NUHS in each crystal plane direction are 51.62nm, 60.69nm and 51.38nm, respectively, and the corresponding crystallinity / LATP phase content are 94.97% / 83.69, 98.59 / 94.73 and 98.99% / 96.26%, respectively. The results show that the LATP membrane prepared based on the improved UHS technology has high crystallinity, high phase content and smaller grain size. Although the LATP membrane prepared using traditional high-temperature sintering technology has a compact structure, it contains more impurities and a larger grain size, which leads to low crystallinity and effective phase content.
[0167] The sintering process of the LATP film prepared based on the improved UHS technology in Example 2 was analyzed at a microscopic level. The cross-section and surface of the LATP film at sintering times of 1 s, 15 s, and 30 s were observed under a field emission scanning electron microscope. The results are as follows: Figure 3 As shown in the figure, at the beginning of sintering, there are large pores between the ceramic particles on the surface of the LATP membrane, and the structural density is insufficient. However, since the melting temperature of the liquid-phase sintering aid is reached, the boron oxide and lithium tetrafluoroborate around the ceramic particles melt and promote the directional growth of the LATP grains. After 15 seconds, the crystals inside the LATP membrane show a directional growth morphology, and the short rod-shaped crystals are tightly attached together, with a tendency to form crystal clusters, and the density of the membrane structure is significantly improved. After 30 seconds, the internal structure of the LATP membrane is compact, and the sintering aid and ion filler after melting and cooling tightly connect the crystals together. The resulting LATP membrane has a smooth and uniform surface and a dense internal structure.
[0168] The thermal and mechanical properties of the LATP films prepared in Comparative Example 1, Comparative Example 2 and Example 2 were tested. The three LATP films were heated to a stable temperature at 100 and 200°C using a heating table and thermal imaging was performed. The results showed that LATP-CHST( Figure 4 b) and LATP-CUHS( Figure 4 c) There are "hot spots" of different sizes on the surface. Among them, LATP-CUHS has a large area of uneven heat area in the thermal imaging image. The existence of "hot spots" not only indicates the defects of the surface microstructure, which may provide sites for poor lithium deposition, but also may cause abnormal distribution of lithium ions due to the poor thermal environment, accelerating the growth and penetration of dendrites, while LATP-NUHS ( Figure 4 a) It has better thermal conductivity and fewer "hot spots", and better overall thermal stability. The three films were tested for puncture strength ( Figure 4 d) Young's modulus ( Figure 4 e) Roughness test ( Figure 4 f), the test found that LATP-NUHS has higher mechanical strength and a smoother surface, while LATP-CUHS has lower overall mechanical strength and an insufficiently smooth surface due to its poor structural density and surface defects. The reason for this phenomenon may be that the rapid temperature change causes violent thermal movement of ceramic particles, resulting in greater internal stress and unstable internal structure.
[0169] The impedance and charge-discharge rate tests were performed on the LATP membranes prepared in Comparative Example 1, Comparative Example 2 and Example 2. Figure 5 b. Figure 5d, the test found that LATP-NUHS has a lower electrochemical AC impedance, and the assembled battery can still operate stably at a higher rate of 0.5C, while the battery capacity of LATP-CUHS decays sharply at high charge and discharge rates. The electrochemical window test was performed on the LATP membranes prepared in Comparative Example 1, Comparative Example 2 and Example 2. Figure 5 As shown in a, the test current of LATP-CUHS changes significantly at 3.59V-3.75V, while that of LATP-CHST and LATP-NUHS is basically stable within 6V. After thermal welding, the interface impedance of the all-solid-state battery decreases significantly, as shown in Figure 5 c, which demonstrates the effectiveness of the thermal welding interface technology.
[0170] See also Figure 6 The LATP membranes prepared in Comparative Example 1, Comparative Example 2 and Example 2 were respectively assembled with NCM811 and LFP batteries for long cycle tests, and the all-solid-state NCM811 battery assembled with LATP-NUHS was subjected to interface thermal welding, as shown in FIG. Figure 6 As shown in a, the cycle stability and capacity retention rate of this battery are better than those of other batteries, and it has a higher first cycle capacity ( Figure 6 b), and the voltage polarization and capacity decay during the cycle are small ( Figure 6 c), for LFP batteries, LATP-NUHS batteries also showed good results, such as Figure 6 As shown in Figure d, the all-solid-state battery equipped with LATP-CUHS has a serious capacity decay, while the all-solid-state LFP battery equipped with LATP-NUHS has stable performance and a higher first cycle capacity ( Figure 6 b), and less voltage polarization and capacity decay during the cycle ( Figure 6 c).
[0171] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a low-impedance NASICON solid electrolyte membrane, characterized in that: The following steps are involved: The lithium source, aluminum source and phosphorus source are mixed, and then a titanium source or a germanium source is added and ball-milled; the ball-milled powder is sequentially dried and subjected to high-temperature solid-phase synthesis to obtain ceramic coarse particles; the ceramic coarse particles are sequentially ball-milled, dried and sieved to obtain NASICON type solid electrolyte powder; Adding a nano-sized boron-based liquid-phase sintering aid, an ion filler and a fiber reinforcement material to NASICON solid electrolyte powder and mixing them uniformly to obtain a mixture, putting the mixture into a metal mold and pressing it into a ceramic green embryo, and placing the ceramic green embryo in a crucible for annealing treatment; The annealed ceramic body is transferred to a Joule heating element of a Joule electric heating device, and sintered by rapid Joule heat treatment under a protective atmosphere. After the heat treatment, the ceramic body is cooled to room temperature to obtain a rough NASICON solid electrolyte membrane. The rough NASICON solid electrolyte membrane is placed in a metallographic grinder and polished, and then the surface of the solid electrolyte membrane is treated with acid immersion, and then neutralized with an alkaline solution and fully rinsed with ethanol to prepare a low-impedance NASICON solid electrolyte membrane.
2. The method for preparing a low-impedance NASICON solid electrolyte membrane according to claim 1, characterized in that: The NASICON solid electrolyte powder is lithium aluminum germanium phosphate or lithium aluminum titanium phosphate, and the chemical formula is Li 1+x Al x Ge 2-x (PO4)3 or Li 1+x Al x Ti 2-x (PO4)3, wherein 0≤x≤1; the lithium source is lithium carbonate or lithium hydroxide, the aluminum source is aluminum nitrate or aluminum oxide, the phosphorus source is diammonium phosphate or phosphoric acid, the titanium source is tetrabutyl titanate or titanium oxide, and the germanium source is germanium oxide; the ball milling medium used in the ball milling process is isopropanol or ethanol, and the ball mill speed is 90rpm~500rpm; the specific steps of the high-temperature solid phase synthesis are: heating at a heating rate of 4℃ / min~10℃ / min to a roasting temperature of 600℃~900℃ for high-temperature solid phase synthesis, the insulation time is 6h~8.5h, and then cooling to room temperature at a cooling rate of 8℃ / min~13℃ / min; the screening process uses a nylon mesh screen of 200 mesh~800 mesh for screening.
3. The method for preparing a low-impedance NASICON solid electrolyte membrane according to claim 1, characterized in that: The added mass ratio of the boron-based liquid-phase sintering aid, the ion filler and the fiber reinforcement material is (1.5-3):1:(0.5-1); the total mass of the boron-based liquid-phase sintering aid, the ion filler and the fiber reinforcement material accounts for 1wt%-5wt% of the mass of the mixture; the boron-based liquid-phase sintering aid is a mixture of one or more of sodium aluminum borate, sodium borohydride, ammonium boron nitrate, aluminum triboride and boron oxide; the ion filler is a mixture of one or more of lithium tetrafluoroborate, lithium borate, lithium nitride and lithium titanate; the fiber reinforcement material is a mixture of one or more of single-walled carbon nanotubes, para-aramid nanofibers, polyimide fibers, boron carbide fibers and boron fibers; the pressure of the ceramic green body during the pressing process is 5MPa-15MPa; the temperature of the annealing treatment is (T c -200)℃~(T c -300)℃,T c The crystallization temperature is the crystallization temperature, the holding time is 2h to 3h, the heating rate is 4℃ / min to 10℃ / min, and the cooling rate is 8℃ / min to 13℃ / min.
4. The method for preparing a low-impedance NASICON solid electrolyte membrane according to claim 1, characterized in that: The protective atmosphere is an inert gas; the voltage of the Joule heating during the rapid Joule heat treatment is 10V to 100V, the heating current is 10A to 60A, and the sintering temperature threshold is 800°C to 960°C; the temperature is lowered to room temperature after the heat treatment is completed by manually adjusting the current so that the temperature drops to room temperature at a uniform rate; the acid used for the acid leaching treatment is hydrochloric acid or dilute nitric acid; the alkaline solution is a dilute sodium hydroxide solution or a sodium bicarbonate solution.
5. A low-impedance NASICON solid electrolyte membrane, characterized in that: The invention is prepared by the method for preparing a low-impedance NASICON solid electrolyte membrane according to any one of claims 1 to 4.
6. An all-solid-state lithium battery, characterized in that: It comprises a positive electrode, a negative electrode and a solid electrolyte membrane; the solid electrolyte membrane is arranged between the positive electrode and the negative electrode; the solid electrolyte membrane is the low-impedance NASICON type solid electrolyte membrane as described in claim 5.
7. A method for preparing the all-solid-state lithium battery according to claim 6, characterized in that: The following steps are involved: Indium tin oxide, nano-scale lithium lanthanum zirconium tantalum oxide powder and polyvinylidene fluoride are mixed, and N-methylpyrrolidone is added to prepare a viscous dilute ceramic slurry using a stirring device; the dilute ceramic slurry is dripped onto the negative electrode side surface of the NASICON solid electrolyte membrane and vacuum dried; The positive electrode active material, conductive carbon, nano-scale LATP powder and polyvinylidene fluoride are mixed and then N-methylpyrrolidone is added to prepare a viscous composite positive electrode slurry through high-energy ball milling. The positive electrode slurry is scraped on the positive electrode side surface of the NASICON type solid electrolyte membrane with dilute ceramic slurry and vacuum dried to obtain an ITO / LLZTO@NASICON type solid electrolyte membrane; The ITO / LLZTO@NASICON solid electrolyte membrane was assembled into a button-type all-solid-state lithium battery in a glove box, and the assembled button-type all-solid-state lithium battery was transferred to the Joule heating element of the Joule electric heating device for thermal pulse-assisted in-situ alloying and interface thermal welding, and finally an all-solid-state lithium battery was prepared.
8. The method for preparing a low-impedance NASICON solid electrolyte membrane according to claim 7, characterized in that: The added mass ratio of indium tin oxide, nano-scale lithium lanthanum zirconium tantalum oxide powder and polyvinylidene fluoride is (0.5-1):(1-3):(0.2-0.5); the solid content of the dilute ceramic slurry is 20wt%-35wt%; and the stirring device is a magnetic stirring device.
9. The method for preparing a low-impedance NASICON solid electrolyte membrane according to claim 7, characterized in that: The positive electrode active material is lithium nickel cobalt manganese oxide, lithium iron phosphate, lithium iron manganese phosphate or lithium cobalt oxide; the added mass ratio of the positive electrode active material, conductive carbon, nano-scale LATP powder and polyvinylidene fluoride is 8:1:(4-6):(4-6); the rotation speed of the high-energy ball mill is 500rpm-1000rpm; the coating thickness of the positive electrode slurry is 80 microns-150 microns.
10. The method for preparing a low-impedance NASICON solid electrolyte membrane according to claim 7, characterized in that: In the process of using the Joule electric heating device to perform heat pulse-assisted in-situ alloying and interface thermal welding, the voltage is 12V to 32V, the current is 6A to 15A, and the heat treatment time is 5min to 10min.
Citation Information
Cited By
Core-shell structure composite solid electrolyte tolerant to lithium negative electrode as well as preparation method and application of core-shell structure composite solid electrolyte
CN120590158A
A core-shell structure composite solid electrolyte resistant to lithium negative electrode, a preparation method and application thereof
CN120590158B