Secondary battery separator and secondary battery

By optimizing the distribution of inorganic particles and polymer particles in the cover layer of the secondary battery separator to form a loose porous structure, the unevenness problem after hot pressing of the traditional separator is solved, and the ion conduction performance and safety of the battery are improved.

CN118712658BActive Publication Date: 2024-11-29SINOMA LITHIUM BATTERY SEPARATOR (NANJING) CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411202292.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-29
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

Traditional diaphragms are difficult to maintain flatness after hot pressing, resulting in uneven ion distribution and battery safety risks, affecting performance stability.

Method used

Design a secondary battery separator, inorganic particles are continuously distributed in the cover layer, polymer particles are discretely distributed and protruded, and the crawling height and crawling degree are limited. By adjusting the slurry viscosity and particle distribution, a loose porous structure is formed to reduce Unevenness after hot pressing.

Benefits of technology

The film surface flatness after hot pressing is achieved, the ion conduction performance and adhesion force are improved, the powder drop rate is reduced, and the safety and performance stability of the battery are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118712658B_ABST
    Figure CN118712658B_ABST
Patent Text Reader

Abstract

The present invention discloses a secondary battery separator and a secondary battery, wherein the secondary battery separator comprises a substrate and a covering layer. The substrate comprises a polyolefin microporous membrane with polyolefin as the main component; the covering layer is arranged on at least one surface of the substrate; the covering layer comprises inorganic particles and polymer particles, wherein the inorganic particles are continuously distributed in the covering layer, the polymer particles are discretely distributed in the inorganic particles and protrude from the surface of the covering layer, and the inorganic particles are accumulated as little as possible in the direction of the polymer particles to form a slope, thereby reducing the problem of uneven membrane surface after hot pressing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of secondary battery separators, and in particular relates to a secondary battery separator and a secondary battery. Background Art

[0002] With the rapid development of energy technology, energy storage devices are playing an increasingly important role in many fields, especially in electric vehicles and renewable energy. As a key component in energy storage devices, diaphragms have an important impact on the performance and safety of batteries. In energy storage devices, the main function of diaphragms is to separate the positive and negative electrodes to prevent short circuits while allowing ions to pass through during charging and discharging.

[0003] Traditional diaphragm designs usually use a single polyolefin microporous membrane as a substrate, which has certain ion permeability and mechanical strength, but still needs to be improved in terms of improving adhesion and reducing thermal shrinkage. To solve these problems, researchers have tried to introduce a covering layer on the substrate of the diaphragm to improve its performance.

[0004] At present, in the prior art, the covering layer of the diaphragm is usually composed of inorganic fillers and particulate polymers. These inorganic fillers and particulate polymers not only improve the mechanical strength of the diaphragm, but also help to improve the transmission performance of ions in the diaphragm. Further, patent application CN116569294A discloses that the covering layer contains inorganic fillers and particulate polymers protruding from the covering layer, and the thickness of the particulate polymer is at least 0.1 times that of the inorganic filler part. The covering layer is formed in a manner inclined toward the protruding particulate polymer (climbing effect). Such a setting improves the adhesion of the particulate polymer and reduces thermal shrinkage.

[0005] Although the polymer particles in the covering layer are more prominent, the polymer particles partially melt and deform during the hot pressing of the diaphragm, which will not affect the flatness of the coating layer. However, during the hot pressing process of this mixed coating diaphragm with a climbing effect, due to the distribution characteristics of the particle polymer and inorganic filler and their interaction with the substrate, it is difficult for the diaphragm to maintain ideal flatness after hot pressing. The uneven diaphragm not only affects the uniform distribution and efficient transmission of ions inside the battery, but may also cause the risk of internal short circuits in the battery, thereby threatening the safety and performance stability of the battery. Summary of the invention

[0006] The purpose of the present invention is to design a granular polymer-inorganic particle mixed coating separator with good flatness after hot pressing and a secondary battery comprising the separator.

[0007] In a first aspect, the present invention provides a secondary battery separator, comprising a substrate and a covering layer, wherein the substrate comprises a polyolefin microporous membrane having polyolefin as a main component, and the covering layer is disposed on at least one surface of the substrate, characterized in that the covering layer comprises inorganic particles and polymer particles, wherein the inorganic particles are continuously distributed in the covering layer, and the polymer particles are discretely distributed in the inorganic particles and protrude from the surface of the covering layer;

[0008] The maximum distance from the boundary line of the substrate-covering layer to the outline of the protruding polymer particles is measured in the cross section in the thickness direction of the diaphragm as L1, the maximum distance from the boundary line of the substrate-covering layer to the outer surface of the inorganic particles of the covering layer is L2, and the thickness of the inorganic particles in the covering layer is L0;

[0009] Climbing height of the covering layer , where H = L2-L0, 2R is the D50 of the polymer particles;

[0010] The degree of ball creep of the covering layer , where M<15%.

[0011] Preferably, the secondary battery separator satisfies . Further preferably, It is 0.5-1.5.

[0012] Preferably, the surface density per unit thickness of the covering layer is 0.8-2.0 g / (cm 2 ·μm).

[0013] Preferably, the covering layer contains 50-99 parts of inorganic particles and 1-50 parts of polymer particles based on 100 parts of the total mass of the inorganic particles and the polymer particles; further preferably, the mass ratio of the inorganic particles to the polymer particles is 1-20:1.

[0014] Preferably, the polymer particles have a D50 of 0.5-10 μm, a L0 of 0.1-5 μm, and a L1 of 0.5-10 μm.

[0015] Preferably, the polymer particles include one or more of polyimide water-soluble microspheres, styrene-butadiene rubber microspheres, polyacrylate modified microspheres, polyetherimide, aramid, aramid, polyvinylidene fluoride, poly(meth)acrylate polymer, polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride and polyvinylidene fluoride-hexafluoropropylene.

[0016] Preferably, the inorganic particles include first inorganic particles and second inorganic particles, and the mass ratio of the first inorganic particles to the second inorganic particles is (15~35):(1~30); the D50 diameter of the first inorganic particles is D, the D50 diameter of the second inorganic particles is d, D / d≥2, D is 0.3-0.9μm, and d is 0.05-0.5μm.

[0017] Preferably, the inorganic particles include third inorganic particles, and D50 / D10 of the third inorganic particles is ≥2.

[0018] Preferably, the inorganic particles include one or more of silicon dioxide, aluminum oxide, magnesium oxide, zirconium oxide, titanium oxide, calcium oxide, boehmite, aluminum nitride, boron nitride, barium sulfate, barium titanate, calcium fluoride and barium fluoride.

[0019] Preferably, the covering layer is formed by coating a slurry onto the substrate, the slurry comprising inorganic particles and polymer particles, the slurry having a viscosity of 100-260 mPa·S. Further preferably, the polymer particles in the slurry have a dry weight of 1%-50% and a wet weight of 0.3%-30%.

[0020] As a preference for the slurry, the slurry also includes one or more of carboxymethyl cellulose, a binder, a regulator, a wetting agent and a dispersant. Based on the total weight of the slurry as 100 parts by weight, the amount of carboxymethyl cellulose is 0-15 parts by weight, the amount of the binder is 0-6 parts by weight, the amount of the regulator is 0-5 parts by weight, the amount of the wetting agent is 0-1 part by weight, and the amount of the dispersant is 0-2 parts by weight. The amounts of the carboxymethyl cellulose, the binder, the regulator, the wetting agent and the dispersant are not 0 at the same time; the binder is one or more of styrene-butadiene rubber, acrylic resin, polyvinyl alcohol, polyacrylonitrile, polyvinylidene fluoride, polyethylene oxide, polytetrafluoroethylene, acrylic acid and its derivative copolymers, acrylamide and its derivative copolymers; the regulator is one or more of polyacrylic acid, polyvinyl alcohol, polyimide, and cellulose; the wetting agent is one or more of anionic surfactants, polyethylene surfactants, and polyol surfactants; the dispersant is one or more of polyvinyl pyrrolidone, polyacrylamide, and polyvinyl alcohol.

[0021] In a second aspect, the present invention provides a secondary battery comprising the secondary battery separator described above.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The secondary battery separator of the present invention has a small climbing height of inorganic particles on the surface of polymer particles and a low climbing degree. The inorganic particles are accumulated as little as possible toward the polymer particles to form a slope, thereby reducing the problem of uneven membrane surface after hot pressing. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a schematic diagram of the cross section of a battery separator;

[0025] Figure 2 This is a SEM image (5k magnification) of a diaphragm prepared using the finished slurry obtained in Example 1;

[0026] Figure 3 and Figure 4 This is a SEM image of a diaphragm prepared from the finished slurry obtained in Example 1 after vertical cutting, wherein: Figure 3 The magnification is 10k. Figure 4 The magnification is 5k;

[0027] Figure 5 This is a partial enlarged SEM image of a diaphragm prepared using the finished slurry obtained in Comparative Example 1 after vertical cutting (photographed at 5K magnification, partial enlargement). DETAILED DESCRIPTION

[0028] The present invention is described in detail below by way of examples. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art in this field can make some non-essential improvements and adjustments to the present invention based on the above content of the present invention.

[0029] The present invention provides a secondary battery separator, comprising a substrate and a covering layer, wherein the substrate comprises a polyolefin microporous membrane having polyolefin as a main component, and the covering layer is disposed on at least one surface of the substrate, characterized in that the covering layer comprises inorganic particles and polymer particles, wherein the inorganic particles are continuously distributed in the covering layer, and the polymer particles are discretely distributed in the inorganic particles and protrude from the surface of the covering layer;

[0030] The maximum distance from the boundary line of the substrate-covering layer to the outline of the protruding polymer particles is measured in the cross section in the thickness direction of the diaphragm as L1, the maximum distance from the boundary line of the substrate-covering layer to the outer surface of the inorganic particles of the covering layer is L2, and the thickness of the inorganic particles in the covering layer is L0;

[0031] Climbing height of the covering layer , where H = L2-L0, 2R is the D50 of the polymer particles;

[0032] The degree of ball creep of the covering layer , M<15%, such as M can specifically be 0, 3%, 5%, 7%, 9%, 11% and 13%.

[0033] The battery separator of the present invention has limited climbing height and climbing degree, and can achieve the effect of no unevenness during the hot pressing process. A specific manifestation is that the extreme difference of hot pressing thickness is less than 0.3 μm.

[0034] In the present invention, ,specific It can be 0.3, 0.5, 0.7, 0.9, 1.1, 1.3, 1.5 and 1.7. Within this range, the coating layer achieves a balance between adhesion and anti-powdering performance, and a specific performance is: adhesion> 0.8N / m, and powdering rate is less than 5%. It is 0.5-1.5. If it is greater than 1.5, it indicates that the depth of the polymer particles embedded in the covering layer is too small, which will increase the risk of powder falling. If it is less than 0.5, it indicates that the depth of the polymer particles embedded in the covering layer is too large, which will result in low bonding force.

[0035] In a preferred embodiment, L0 is between 0.1-5μm, specifically 0.1μm, 0.5μm, 1μm, 1.5μm, 2μm, 2.5μm, 3μm, 3.5μm, 4μm, 4.5μm and 5μm, and L1 is between 0.5-10μm, specifically 0.5μm, 1μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm and 10μm.

[0036] The particle sizes of various organic and inorganic substances described in the present invention all refer to volume particle sizes, for example, D50 all refers to Dv50.

[0037] In the present invention, the D50 of the polymer particles is 0.5-10 μm, specifically 0.5 μm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm and 10 μm. The D50 of the polymer particles depends on the selection of the polymer raw materials. In particular, the value of D50 can be determined by the raw materials, or by electron microscopic photography, taking 5 samples of the polymer particles at random, measuring their diameters, and taking the average value as the value of D50.

[0038] It should be noted that when substituting into the relational expression, the unit calculation should not be brought in. The relational expression and range proposed in the present invention are designed based on the numerical relationship of these parameters and are not affected by whether the dimensions are equal.

[0039] In the present invention, the surface density per unit thickness of the covering layer is 0.8-2.0 g / (cm 2 ·μm), specifically 0.8g / (cm 2 ·μm)、1.1g / (cm 2 ·μm)、1.2g / (cm 2 ·μm)、1.4g / (cm 2·μm)、1.6g / (cm 2 ·μm)、1.8g / (cm 2 ·μm) and 2.0g / (cm 2 ·μm). Control the unit thickness density of the covering layer to be 0.8-2.0g / (cm 2 ·μm), the cover layer has good liquid absorption and retention performance and ion conductivity, and maintains good thermal shrinkage performance. Specifically, it can be shown that the liquid absorption rate is greater than 80%, the thermal shrinkage rate is less than 3%, and the air permeability value-added rate is less than 20%. In the present invention, the inorganic particles can be a mixture of first inorganic particles and second inorganic particles, the mass ratio of the first inorganic particles to the second inorganic particles is (15~35):(1~30), the D50 diameter of the first inorganic particle size particles is D, the D50 diameter of the second inorganic particle size particles is d, D / d≥2, preferably D / d is 2-5, specifically 2, 2.1, 2.3, 2.5, 3, 3.2, 3.5, 3.8, 4, 4.5 and 5; the D50 diameter of the first inorganic particles is 0.3-0.9μm, specifically 0.3μm, 0.5μm, 0.7μm and 0.9μm; the D50 diameter of the second inorganic particles is 0.05-0.5μm, specifically 0.05μm, 0.1μm, 0.15μm, 0.2μm, 0.3μm, 0.4μm and 0.5μm. In the present invention, the inorganic particles may also be third inorganic particles having a certain particle size distribution, in which D50 / D10 is ≥2, preferably 2-10, specifically 2, 3, 4, 5, 6, 7, 8, 9 and 10.

[0040] When two or more inorganic particles with large particle size differences or inorganic particles with a certain particle size distribution are selected, the relatively small-sized inorganic particles themselves have a higher specific surface area, and the relatively small-sized inorganic particles will adhere to the surface of the large-sized inorganic particles to form a relatively dense inorganic particle group similar to a flower bud. Because the size of the flower buds will be randomly generated within a range, a loose and porous stacking morphology is formed. The van der Waals force between these inorganic particle groups is much greater than the surface tension generated on the surface of the polymer particles. As the slurry is deposited and dried, the inorganic particle groups tend to settle evenly near the polymer particles, reducing the climbing effect during the slurry deposition process, thereby reducing the unevenness of the diaphragm after hot pressing.

[0041] The present invention has no particular restrictions on the substrate. The polyolefin microporous membrane containing polyolefin as the main component can be selected with reference to the existing lithium-ion battery separator. Generally, the substrate can be a polyolefin-based membrane, such as a polypropylene-based membrane, a polyethylene-based membrane, etc. As a preferred embodiment, the base membrane is a polyethylene-based membrane. The thickness of the base membrane can be 5-12 μm.

[0042] In the present invention, the covering layer is formed by coating a slurry onto a substrate, the slurry includes inorganic particles and polymer particles, and may also include one or more of CMC, a binder, a regulator, a wetting agent and a dispersant, and the slurry viscosity is controlled at 100-260 mPa·S. In the present invention, the climbing effect of the diaphragm is further improved by adjusting the slurry viscosity within a specific range. When the slurry viscosity is appropriate, inorganic particle groups similar to flower buds are more easily formed. Adjusting the slurry viscosity can be achieved by adjusting the mass fractions of the regulator, the binder and the CMC. Those skilled in the art can obtain the required slurry viscosity through a limited number of experiments.

[0043] The inorganic particles, polymer particles, CMC (carboxymethyl cellulose), binder, regulator, wetting agent and dispersant in the present invention are commonly used in the art, and the present invention does not specifically limit them. For example, the inorganic particles can be silicon dioxide (SiO 2 )、Alumina(Al 2 O 3 )、MgO、ZrO 2 ), titanium oxide (TiO 2 ), calcium oxide (CaO) and other oxide particles, boehmite (ALOOH), aluminum nitride (AlN), boron nitride (BN) and other nitride particles, barium sulfate (BaSO 4 ), barium titanate (BaTiO 3 ), calcium fluoride (CaF 2 ) and barium fluoride (BaF 2 ) and other insoluble ionic crystalline particles; when the inorganic particles are a mixture of multiple substances, the dosage of the different substances can be any ratio, as long as the total amount meets the inorganic particle dosage limit. Preferably, the inorganic particles are boehmite.

[0044] The polymer particles may be one or more of PI (polyimide) water-soluble microspheres, SBR (styrene-butadiene rubber) microspheres, PAA (polyacrylate) modified microspheres, polyetherimide, aramid, aramid, polyvinylidene fluoride, poly(meth)acrylate polymer, polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene; preferably at least one of poly(meth)acrylate polymer, SBR (styrene-butadiene rubber) microspheres, PI (polyimide) water-soluble microspheres, and PAA (polyacrylate) modified microspheres. One-shot poly(meth)acrylate polymers are particularly preferred.

[0045] The binder can be one or more of styrene-butadiene rubber, acrylic resin, polyvinyl alcohol, polyacrylonitrile, polyvinylidene fluoride, polyethylene oxide, polytetrafluoroethylene, copolymers of acrylic acid and its derivatives, copolymers of acrylamide and its derivatives; the regulator can be one or more of polyacrylic acid, PVA, polyimide, and cellulose; the wetting agent can be one or more of anionic surfactants, polyethylene surfactants, and polyol surfactants; the dispersant can be one or more of polyvinyl pyrrolidone (PVP), polyacrylamide (PAM), and polyvinyl alcohol (PVA). The amount of each raw material can be conventionally adjusted according to actual needs, and the present invention does not make specific limitations. For example, the amount of CMC can be 0-15 parts by weight, the amount of the binder can be 0-6 parts by weight, the amount of the regulator can be 0-5 parts by weight, the amount of the wetting agent can be 0-1 part by weight, and the amount of the dispersant can be 0-2 parts by weight.

[0046] The various raw materials used above can be obtained by commercial purchase or homemade, and no special specification is made.

[0047] In the present invention, the dry weight of the polymer particles in the slurry is 1%-50%, specifically 1%, 5%, 10%, 15%, 20%, 30%, 40% and 50%, and the wet weight is 0.3%-30%, specifically 0.3%, 1%, 5%, 10%, 15%, 20% and 30%.

[0048] In the present invention, based on the total mass of the inorganic particles and the polymer particles in the covering layer as 100 parts, the covering layer contains 50-99 parts of inorganic particles, specifically 50 parts, 60 parts, 70 parts, 80 parts, 90 parts and 99 parts, and 1-50 parts of polymer particles, specifically 1 part, 10 parts, 20 parts, 30 parts, 40 parts and 50 parts. The mass ratio of the inorganic particles to the polymer particles is 1-20:1, specifically 1:1, 5:1, 10:1, 15:1 and 20:1.

[0049] Hereinafter, the present application will be described in detail by way of specific examples. In the following examples and comparative examples, unless otherwise specified, parts are by weight.

[0050] Embodiment 1:

[0051] 7.66 parts of boehmite B (small particle size), 0.3 parts of dispersant polyvinyl pyrrolidone and 54.61 parts of ultrapure water were dispersed at a speed of 1300 rpm for 40 minutes to form a uniform slurry, 17.88 parts of boehmite A (large particle size) were added and dispersed at 1300 rpm for 20 minutes, 6 parts of CMC solution were added and dispersed at 1000 rpm for 20 minutes, and then ground with a grinder at a speed of 1000 rpm for 20 minutes (1 time) to form a boehmite slurry, 9.6 parts of polymer microspheres (PMMA emulsion) were added to the slurry and dispersed at a speed of 40 rpm for 20 minutes, 3.33 parts of binder styrene-butadiene rubber were added to the slurry and dispersed at a speed of 40 rpm for 20 minutes, 0.57 parts of regulator polyacrylic acid were added to the slurry and dispersed for 20 minutes, and 0.05 parts of wetting agent alkylphenol polyoxyethylene ether were added to the slurry and dispersed for 10 minutes to form a finished slurry.

[0052] Embodiment 2, 3:

[0053] 25.54 parts of boehmite C, 0.3 parts of dispersant polyvinyl pyrrolidone and 54.61 parts of ultrapure water were dispersed at a speed of 1300 rpm for 40 minutes to form a uniform slurry, and then 6 parts of CMC solution were added and dispersed at 1000 rpm for 20 minutes, and then ground with a grinder at a speed of 1000 rpm for 20 minutes (1 time) to form a boehmite slurry, 9.6 parts of polymer microspheres (PMMA emulsion) were added to the slurry and dispersed at 40 rpm for 20 minutes, 3.33 parts of binder styrene-butadiene rubber were added to the slurry and dispersed at 40 rpm for 20 minutes, 0.57 parts of regulator polyacrylic acid were added to the slurry and dispersed for 20 minutes, and 0.05 parts of wetting agent alkylphenol polyoxyethylene ether were added to the slurry and dispersed for 10 minutes to form a finished slurry.

[0054] The difference between Example 2 and Example 3 is that the boehmite particle sizes used are different, see Table 1 for details.

[0055] Example 4: The preparation method of Example 4 is the same as that of Example 1, except that the particle size of the boehmite used is different, see Table 1 for details.

[0056] Example 5 and Comparative Examples 1-3: The preparation methods of Example 5 and Comparative Examples 1-3 are the same as those of Examples 2-3, except that the boehmite particle sizes used are different, see Table 1 for details, wherein the slurry viscosity in Comparative Examples 2 and 3 is lower.

[0057] Example 6: The preparation method of Example 6 is the same as that of Example 1, except that the type of polymer used is different and the particle size of boehmite is different. For details, see Table 1.

[0058] Example 7: The preparation method of Example 7 is the same as that of Example 1, except that the type of polymer used is different, see Table 1 for details.

[0059] Example 8: The preparation method of Example 8 is the same as that of Example 2, except that the boehmite particle size, polymer D50 and coating thickness used are different, see Table 1 for details.

[0060] Example 9: The preparation method of Example 9 is the same as that of Example 2, except that the boehmite particle size and polymer D50 used are different, see Table 1 for details.

[0061] Comparative Example 4: The preparation method of Comparative Example 4 is the same as that of Example 1, except that the small particle size boehmite D50 and polymer D50 are different, see Table 1 for details.

[0062] Coating process: The finished slurry of the embodiment and the comparative example is coated on both sides of a 7 μm thick base film using a gravure roller or a wire rod. After the finished slurry is coated on the surface of the base film, it is dried in an oven (drying temperature is 75°C, time is 10s) to obtain a battery separator with a coated film.

[0063] Figure 2 This is a planar SEM image of a diaphragm prepared from the finished slurry obtained in Example 1; Figure 3-Figure 4 The SEM images of the diaphragm prepared from the finished slurry obtained in Example 1 at different magnifications after vertical cutting show that there is no obvious climbing effect. Figure 5 The SEM picture of the diaphragm prepared from the finished slurry of Comparative Example 1 after vertical cutting shows that the small inorganic particles tend to tilt around the polymer particles.

[0064]

Test method

[0065] Testing methods for L0, L1, L2:

[0066] Figure 1 Schematic diagram of the cross section of the diaphragm, through which L0, L1, L2 defined in the present invention can be intuitively understood. Reference numeral ① represents polymer particles, and reference numeral ② represents inorganic particles.

[0067] The cross-sectional samples of the battery separator were prepared at 21±4°C and humidity ≤65%RH, and the cross-sectional electron microscope images were obtained by photographing them using a Zeiss SIGMA 300 electron microscope. Five random positions were measured on the 5K electron microscope image and the average value was taken.

[0068] L0: The distance from the boundary line between the substrate and the covering layer to the outer surface of the covering layer. It should be noted that the "inorganic particle part" does not include the part within 1.5 times the D50 of the polymer particle (or 3 times R) from the center line of the protruding polymer particle.

[0069] L2: The maximum distance from the boundary line between the substrate and the covering layer to the outer surface of the inorganic particles in the covering layer.

[0070] L1: The maximum distance from the boundary line between the substrate and the cover layer to the outline of the protruding polymer particles.

[0071] The D50 of the polymer particles can also be measured using the method described above.

[0072] The test methods of various properties and physicochemical parameters involved in the present invention include:

[0073] 1. Weight measurement method:

[0074] (1) Take the base film, cut it into 10 cm × 10 cm pieces using a 10 cm × 10 cm mold, and place it on an electronic balance to weigh m0;

[0075] (2) Take the finished coated film, cut it into pieces using a 10 cm × 10 cm abrasive tool, and place it on an electronic balance to weigh m1;

[0076] (3) .

[0077] 2. Unit area density measurement method:

[0078] Single layer density = coating weight / coating thickness

[0079] 3. Adhesion: The adhesion referred to in the invention refers to the degree of tightness and uniformity of the adhesion between the battery separator and the battery pole piece when the battery cell is assembled. In particular, the adhesion is evaluated according to the following method: Test with reference to the requirements of GB / T 2792.

[0080] (1) stacking A4 paper and a separator in the order of A4 paper / separator / separator / A4 paper, with the separator coatings facing each other;

[0081] (2) The stacked A4 paper and separator are subjected to thermoplastic treatment at a temperature of 100°C;

[0082] (3) Cut the thermoplasticized diaphragm into strips with a length of 200 mm and a width of 25 mm. The distance between the fixtures is (100 ± 5) mm and the test speed is (50 ± 10) mm / min.

[0083] 4. Heat resistance:

[0084] That is, the heat shrinkage rate is tested according to the method specified in GB / T12027-2004. The average value of the heat shrinkage rate in the TD direction and the heat shrinkage rate in the MD direction is taken.

[0085] 5. Breathability value-added rate:

[0086] Place the sample in a Wangyan air permeability tester and test the time required for 100 mL of air to pass through a 1 square inch membrane at a pressure of 1.22 kPa. This is the membrane air permeability value. The base membrane air permeability measurement value is A1, and the coating membrane air permeability measurement value is A2. .

[0087] 6. Slurry viscosity measurement method

[0088] The test was performed using a Brookfield DV2T viscometer, using a 2# rotor and 60 rpm.

[0089] 7. Hot pressing thickness measurement method

[0090] (1) Sample preparation: PET & diaphragm 25×150 mm, A4+PET+diaphragm+PET+A4

[0091] (2) Test method: Use pressure 1000kgf, temperature 60℃, time 1s, use PET clamp hot press

[0092] (3) After hot pressing, the thickness is measured at 10 points using a micrometer. The maximum value minus the minimum value of the data at these 10 points is the value of As a basis for judgment.

[0093] 8. Liquid absorption rate

[0094] Take a 25mm×50mm coating film sample, weigh it and record it as W1, soak it in the electrolyte for 2 hours, take it out and wipe off the electrolyte on the sample surface, weigh it and record it as W2, then .

[0095] 9. Fan drop rate

[0096] After the finished battery separator passes through a 90-degree angle roller 20 times, random samples are taken and 1K-fold electron microscope pictures (500-5K times) are taken to count the probability of polymer particles falling off (number of polymer particles falling off / total number of polymer particles). Repeat 5 times and calculate the average value as the powder loss rate.

[0097] The parameters and indicators of the above embodiments and comparative examples are listed as follows:

[0098] Table 1

[0099]

[0100] Table 1 (continued)

[0101]

[0102] It can be seen from the above table that Examples 1 to 9 meet the requirements of the climbing ball height and climbing ball degree specified in the present invention, and the extreme difference in hot pressing thickness is small after hot pressing (all <0.3μm), and a battery separator with a smooth membrane surface can be obtained; while the climbing ball height or climbing ball degree in Comparative Examples 1 to 4 does not meet the requirements of the present application, and the extreme difference in hot pressing thickness is significantly increased after hot pressing.

[0103] The battery separator provided by the present invention is not limited to being prepared by the preparation method provided by the present invention, and the battery separators in accordance with the present invention obtained by other methods should all fall within the protection scope of the claims of the present invention.

[0104] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the claims of the present invention.

Claims

1. A secondary battery separator, comprising a substrate and a covering layer, wherein the substrate comprises a polyolefin microporous membrane having polyolefin as a main component, and the covering layer is disposed on at least one surface of the substrate, characterized in that: The covering layer comprises inorganic particles and polymer particles, wherein the inorganic particles are continuously distributed in the covering layer, and the polymer particles are discretely distributed in the inorganic particles and protrude from the surface of the covering layer; measured by the cross section in the thickness direction of the diaphragm, the maximum distance from the boundary line of the substrate-covering layer to the outline of the protruding polymer particles is set to L1, the maximum distance from the boundary line of the substrate-covering layer to the outer surface of the inorganic particles of the covering layer is set to L2, and the thickness of the inorganic particle part in the covering layer is set to L0, and the inorganic particle part does not include the part within the range of 1.5 times D50 of the polymer particles or 3 times R from the center line of the protruding polymer particles; Climbing height of the covering layer , where H = L2-L0, 2R is the D50 of the polymer particles; The degree of ball creep of the covering layer , M<15%.

2. The secondary battery separator according to claim 1, characterized in that: The following relations are satisfied: 。 3. The secondary battery separator according to claim 1, characterized in that: The unit thickness surface density of the covering layer is 0.8-2.0 g / (cm 2 ·μm).

4. The secondary battery separator according to claim 1, characterized in that: The polymer particles have a D50 of 0.5-10 μm, a L0 of 0.1-5 μm, and a L1 of 0.5-10 μm.

5. The secondary battery separator according to claim 2, characterized in that: It is 0.5-1.

5.

6. The secondary battery separator according to claim 1, characterized in that: The inorganic particles include first inorganic particles and second inorganic particles, and the mass ratio of the first inorganic particles to the second inorganic particles is (15~35):(1~30); the D50 diameter of the first inorganic particles is D, the D50 diameter of the second inorganic particles is d, D / d≥2, D is 0.3-0.9μm, and d is 0.05-0.5μm.

7. The secondary battery separator according to claim 1, characterized in that: The inorganic particles include third inorganic particles, and D50 / D10 of the third inorganic particles is ≥2.

8. The secondary battery separator according to claim 1, characterized in that: The covering layer is formed by coating a slurry onto a substrate, wherein the slurry includes inorganic particles and polymer particles, and the slurry has a viscosity of 100-260 mPa·S.

9. The secondary battery separator according to claim 8, characterized in that: The polymer particles in the slurry have a dry weight of 1% to 50% and a wet weight of 0.3% to 30%.

10. The secondary battery separator according to claim 1, characterized in that: Based on 100 parts of the total weight of the inorganic particles and the polymer particles in the covering layer, the covering layer contains 50-99 parts of inorganic particles and 1-50 parts of polymer particles.

11. The secondary battery separator according to claim 10, characterized in that: The mass ratio of the inorganic particles to the polymer particles is 1-20:

1.

12. The secondary battery separator according to claim 1, characterized in that: The polymer particles include one or more of polyimide water-soluble microspheres, styrene-butadiene rubber microspheres, polyacrylate modified microspheres, polyetherimide, aramid, aramid sulfone, polyvinylidene fluoride, poly(meth)acrylate polymer, polyethylene oxide, polyacrylonitrile and polyvinylidene fluoride-hexafluoropropylene; The inorganic particles include one or more of silicon dioxide, aluminum oxide, magnesium oxide, zirconium oxide, titanium oxide, calcium oxide, boehmite, aluminum nitride, boron nitride, barium sulfate, barium titanate, calcium fluoride and barium fluoride.

13. The secondary battery separator according to claim 8, characterized in that: The slurry further comprises one or more of carboxymethyl cellulose, a binder, a regulator, a wetting agent and a dispersant. Based on the total weight of the slurry being 100 parts by weight, the amount of the carboxymethyl cellulose is 0-15 parts by weight, the amount of the binder is 0-6 parts by weight, the amount of the regulator is 0-5 parts by weight, the amount of the wetting agent is 0-1 part by weight, the amount of the dispersant is 0-2 parts by weight, and the amounts of the carboxymethyl cellulose, the binder, the regulator, the wetting agent and the dispersant are not all 0 at the same time; The binder is one or more of styrene-butadiene rubber, acrylic resin, polyvinyl alcohol, polyacrylonitrile, polyvinylidene fluoride, polyethylene oxide, polytetrafluoroethylene, copolymers of acrylic acid and its derivatives, and copolymers of acrylamide and its derivatives; The regulator is one or more of polyacrylic acid, polyvinyl alcohol, polyimide, and cellulose; The wetting agent is one or more of anionic surfactants, polyethylene surfactants, and polyol surfactants; The dispersant is one or more of polyvinyl pyrrolidone, polyacrylamide and polyvinyl alcohol.

14. A secondary battery, characterized in that: A secondary battery separator comprising the separator according to any one of claims 1 to 13.

Citation Information

Patent Citations

  • Separator for electrochemical cell and method for its manufacture

    CN101828283A

  • Separator for power storage device and power storage device comprising same

    CN116569294A