Modified bismuth tungstate catalyst as well as preparation method and application thereof
The modified bismuth tungstate catalyst was prepared by doping bismuth, tungsten, sulfur and tin sources, which solved the problem of low photocatalytic activity of Bi2WO6, significantly improved the antibiotic removal efficiency and the stability of the catalyst, and achieved efficient antibiotic wastewater treatment.
Patent Information
- Application Number
- CN202410777667.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-01
AI Technical Summary
Bi2WO6 photocatalyst has low photocatalytic activity in antibiotic wastewater treatment, mainly due to its large spectrum width and easy recombination of photogenerated electrons and holes, resulting in low separation efficiency of photogenerated carriers, limiting its application effect.
By doping soluble bismuth salt, soluble tungstate, sulfur source and tin source, Sn-S-BWO modified bismuth tungstate catalyst is prepared, its morphology structure and electronic structure are adjusted, and the utilization rate of visible light and overall photocatalysis are improved. active.
The removal rates of ciprofloxacin and tetracycline are significantly improved, reaching 91.5% and 97.1%, and the stability and photocatalytic activity of the catalyst are improved. It is in line with the concept of green chemistry and is suitable for large-scale production.
Smart Images

Figure CN118719096A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of photocatalysis technology, and in particular to a modified bismuth tungstate catalyst, a preparation method and application thereof. Background Art
[0002] Ciprofloxacin (CIP) and tetracycline (TC) are widely used fluoroquinolone and tetracyclic antibiotics. Due to their high chemical stability, they cannot be effectively biodegraded. They are used and remain in the environment and eventually accumulate in the food chain, endangering human health. Therefore, there is an urgent need for an economical and effective technology to treat complex organic pollutants in water environments. Currently, relatively effective ways to remove antibiotics in water mainly include membrane filtration, adsorption and advanced oxidation methods. Among them, advanced oxidation technology (AOPS) is one of the treatment processes for efficiently treating refractory organic matter, and has attracted much attention due to its high reactivity and oxidative degradation ability.
[0003] As an important branch of advanced oxidation technology, photocatalytic oxidation converts solar energy into usable chemical energy by preparing suitable photocatalytic materials, thereby achieving efficient removal of organic pollutants. When the semiconductor material is irradiated with light energy (hv) greater than its forbidden band, the photogenerated charges with reducing effect jump from the valence band to the conduction band and react with dissolved oxygen in water to produce superoxide radicals (·O 2- ) leaving a valence band hole that will react with water or hydroxide (OH - ) reacts to generate hydroxyl radicals (·OH) with strong oxidizing effect. Both photogenerated charge-hole pairs and active free radicals can act as active substances in the photocatalytic reaction to participate in the removal of pollutants.
[0004] In recent years, visible light-driven semiconductor photocatalysts have attracted much attention. 2 WO 6 It has excellent stability, efficient electron transfer capability, and can be excited by visible light and ultraviolet light. It is a green catalytic material. 2 WO 6 Its unique layered structure enables it to effectively degrade organic pollutants such as antibiotics, and it is considered to be the most promising photocatalyst in antibiotic wastewater treatment.
[0005] However, 2 WO 6 The spectrum width of Bi is large (2.8eV), it can only absorb light less than 450nm, and its photogenerated electron-holes are easy to recombine, and the separation efficiency of photogenerated carriers is low. These problems lead to 2 WO 6 The photocatalytic activity of Bi 2 WO 6Application in antibiotic wastewater treatment. Therefore, the selection of semiconductor modified materials with appropriate energy band potential is crucial to achieve efficient degradation effect. Summary of the invention
[0006] The object of the present invention is to provide a modified bismuth tungstate catalyst, a preparation method and an application thereof, which improves the utilization rate of visible light and the overall photocatalytic activity, and can effectively and stably remove antibiotics, especially CIP and TC.
[0007] The embodiments of the present invention are implemented by the following technical solutions:
[0008] The first object of the present invention is to provide a modified bismuth tungstate catalyst, comprising a soluble bismuth salt, a soluble tungstate, a sulfur source and a tin source; the mass ratio of the soluble bismuth salt, the soluble tungstate, the sulfur source and the tin source is 15-25:5-10:2-5:1.
[0009] Furthermore, the soluble bismuth salt is bismuth nitrate, bismuth nitrate pentahydrate,
[0010] The soluble tungstate sodium tungstate, sodium tungstate dihydrate,
[0011] The sulfur source is cysteine or L-cysteine;
[0012] The tin source is tin tetrachloride or tin tetrachloride pentahydrate;
[0013] The second object of the present invention is to provide a method for preparing a modified bismuth tungstate catalyst, comprising the following steps:
[0014] S1, dissolving a soluble bismuth salt in an alcohol solvent to obtain a bismuth salt alcohol solution, dissolving a soluble tungstate in water to obtain a tungstate aqueous solution; dropping the tungstate aqueous solution into the bismuth salt alcohol solution and continuously stirring for a period of time to obtain a first mixed solution;
[0015] S2, adding a sulfur source and a tin source to the first mixed solution obtained in S1 in sequence, and stirring for a period of time to obtain a second mixed solution;
[0016] S3, heating, filtering, washing and drying the second mixed solution obtained in S2 to obtain a modified bismuth tungstate catalyst.
[0017] The third object of the present invention is to provide an application of the modified bismuth tungstate catalyst in the degradation of antibiotic-containing wastewater under visible light, especially in the catalytic degradation of a mixed solution of ciprofloxacin and tetracycline.
[0018] The technical solution of the embodiment of the present invention has at least the following advantages and beneficial effects:
[0019] 1. The Sn-S-BWO doped modified bismuth tungstate nanophotocatalyst prepared by the present invention has excellent catalytic degradation of antibiotic-containing wastewater under visible light, especially the degradation of ciprofloxacin and tetracycline. This is mainly due to the fact that the morphology and structure of the doped bismuth-based catalyst have changed, which greatly improves the adsorption capacity of antibiotics, especially ciprofloxacin and tetracycline, and significantly improves the catalytic stability of the catalyst. The synergistic effect of sulfur and tin significantly improves the utilization rate of visible light and the overall photocatalytic activity. The removal rates of CIP and TC can reach 91.5% and 97.1% respectively, which significantly improves the catalytic activity compared with the unmodified material.
[0020] 2. The raw materials used in the preparation method of the Sn-S-BWO doped modified bismuth tungstate nanophotocatalyst prepared by the present invention are non-toxic, simple to operate, and have mild reaction conditions. It conforms to the concept of green chemistry, has broad application prospects in solving water environmental pollution, and is suitable for mass production. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0022] Figure 1 The performance diagram of the catalyst provided in Example 1 of the present invention for catalytic degradation of CIP and TC at different dosages;
[0023] Figure 2 The catalytic degradation performance diagram of the catalyst provided in Example 1 of the present invention at different CIP and TC initial concentrations;
[0024] Figure 3 The cyclic performance curve diagram of the catalyst provided in Example 1 of the present invention;
[0025] Figure 4 (a) is a scanning electron microscope image of the catalyst of Comparative Example 1, Figure 4 (b) is a scanning electron microscope image of the catalyst of Comparative Example 2, Figure 4 (c) is a scanning electron microscope image of the catalyst of Example 1;
[0026] Figure 5 Transmission electron microscope (TEM) and scanning electron microscope-energy dispersive spectroscopy (SEM-EDS) images of the catalyst of Example 1 of the present invention;
[0027] Figure 6 The X-ray diffraction (XRD) diagrams of the catalysts of Example 1 and Comparative Examples 1-2 of the present invention;
[0028] Figure 7 It is the Fourier transform infrared spectrum (FT-IR) graph of the catalyst of Example 1 of the present invention and Comparative Examples 1-2;
[0029] Figure 8 The UV-visible diffuse reflectance spectra (UV-visDRS) of the catalysts of Example 1 and Comparative Examples 1-2 of the present invention are shown;
[0030] Fig. 9 The transient photocurrent (It) and steady-state photoluminescence (PL) spectra of the catalysts of Example 1 and Comparative Examples 1-2 of the present invention are shown. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0032] For example: The basic information of the instruments used is as follows: SEM photos and EDS spectra were taken using a JSM 7800F field emission scanning electron microscope from JEOL, Japan. TEM was taken on a FEI Tecnai G2 F20 projection electron microscope from the United States. XRD spectra were recorded on a MiniFlex 600 from Rigaku, Japan. FT-IR spectra were measured on a Spectrum Two spectrometer from PerkinElmer, USA, using KBr as a reference sample. UV-Vis DRS spectra were recorded by UH-4150 from Hitachi, Japan. PL steady-state and transient photoluminescence spectra were recorded on a FLS1000 steady-state transient fluorescence spectrometer from Edinburgh, UK. UV-Vis absorption spectra were performed by a USB 4000 spectrophotometer from Ocean Optics, Shanghai.
[0033] The following is a detailed description of a modified bismuth tungstate catalyst, a preparation method and an application thereof provided in an embodiment of the present invention.
[0034] The first object of the present invention is to provide a modified bismuth tungstate catalyst, comprising a soluble bismuth salt, a soluble tungstate, a sulfur source and a tin source; the mass ratio of the soluble bismuth salt, the soluble tungstate, the sulfur source and the tin source is 15-25:5-10:2-5:1. Preferably, the mass ratio is 18:6:2:1.
[0035] Further, the soluble bismuth salt includes but is not limited to bismuth nitrate and / or bismuth nitrate pentahydrate;
[0036] The soluble tungstate includes but is not limited to sodium tungstate and / or sodium tungstate dihydrate;
[0037] The sulfur source includes but is not limited to cysteine and / or L-cysteine;
[0038] The tin source includes but is not limited to tin tetrachloride and / or tin tetrachloride pentahydrate;
[0039] The second object of the present invention is to provide a method for preparing a modified bismuth tungstate catalyst, comprising the following steps: (1) reacting a soluble bismuth salt with a tungstate to generate a bismuth tungstate catalytic core; and (2) modifying the bismuth tungstate catalytic core by doping a sulfur source and a tin source to obtain a modified bismuth tungstate catalyst.
[0040] More specifically, the preparation method thereof comprises the following steps:
[0041] S1, dissolving a soluble bismuth salt in an alcohol solvent (such as ethylene glycol, methanol, ethanol, propanol, etc., preferably ethylene glycol) and stirring for 0.5 hours to obtain a bismuth salt alcohol solution, dissolving a soluble tungstate in water and stirring for 0.5 hours to obtain a tungstate aqueous solution; adding the tungstate aqueous solution dropwise to the bismuth salt alcohol solution and continuously stirring for 0.5-1 hours to obtain a first mixed solution;
[0042] S2. Add a sulfur source and a tin source to the first mixed solution obtained in S1 in sequence, and continue stirring for 2-3 hours to obtain a second mixed solution; finally, transfer the second mixed solution to an autoclave, and heat it at 150-200° C. for 20-30 hours; filter and wash the obtained product, dry it in an oven at 50-80° C. for 20-30 hours, and collect the product to obtain a modified bismuth tungstate catalyst Sn-S-BWO.
[0043] The third object of the present invention is to provide an application of the modified bismuth tungstate catalyst in the degradation of antibiotic-containing wastewater under visible light, especially in the catalytic degradation of a mixed solution of ciprofloxacin and tetracycline.
[0044] In the present invention, the inventors based on the existing Bi 2 WO 6 In the application, the photogenerated electron-hole is easy to recombine and the separation efficiency of the photogenerated carrier is low. The inventors considered that without affecting Bi 2 WO 6 On the basis of the overall structure, ions of different radii are doped into the lattice to induce internal strain and generate defects in the lattice to solve the above problems, so as to exert a more stable photocatalytic adsorption and degradation effect; specifically, the present invention is in Bi 2 WO 6L-cysteine was used as a sulfur doping source and tin tetrachloride was used as a tin doping source in the lattice to induce Bi 2 WO 6 L-cysteine is used as the sulfur doping source, on this basis, by forming Bi-S bonds, Bi 2 WO 6 The structure of the 3D structure changes to a 2D layered structure, which is mainly due to the S 2- (r=0.184nm) replaces Bi 2 WO 6 O in the lattice 2- (r = 0.140nm) caused by the change of the layered structure, the new lamellar structure formed after the change can enhance the scattering of visible light in it compared with the spherical structure, extend the refraction path of visible light in it, and enhance the photocatalytic activity. In addition, the generation of bi-s bonds on its surface and the introduction of active functional groups can also increase more adsorption sites for ciprofloxacin and tetracycline molecules, thereby improving the adsorption effect of ciprofloxacin and tetracycline.
[0045] In addition, after metallic tin and non-metallic sulfur are doped into bismuth tungstate, an intermediate impurity level is generated. The quantum confinement effect further reduces the transition energy of photoexcited electrons, promotes the separation and transfer of photogenerated charges, greatly enhances the light absorption intensity, and produces more active free radicals, thereby enhancing the adsorption of ciprofloxacin and tetracycline. At the same time, its own photocatalytic activity is improved. The two jointly promote and achieve the effective and stable removal of ciprofloxacin and tetracycline.
[0046] Example 1
[0047] The preparation method of the modified bismuth tungstate catalyst in this embodiment comprises the following steps:
[0048] S1. Dissolve 0.330 g of sodium tungstate dihydrate in 40 mL of deionized water and stir for 0.5 h to obtain a tungstate aqueous solution; dissolve 0.970 g of bismuth nitrate pentahydrate in ethylene glycol and stir for 0.5 h to obtain a bismuth salt alcohol solution; add the tungstate aqueous solution dropwise to the bismuth salt alcohol solution and continue stirring for 1 h to obtain a first mixed solution;
[0049] S2, adding 0.1 g of L-cysteine and 0.045 g of tin tetrachloride pentahydrate to the first mixed solution obtained in S1, and stirring for 2 hours to obtain a second mixed solution;
[0050] S3. Finally, the second mixed solution was transferred to an autoclave and heated at 160°C for 24 hours. The obtained product was filtered, washed, and dried in an oven at 60°C for 24 hours. The product was collected to obtain a modified bismuth tungstate catalyst, named 0.045-Sn-S-BWO.
[0051] Example 2
[0052] The preparation method of the modified bismuth tungstate catalyst in this embodiment comprises the following steps:
[0053] S1. Dissolve 0.315 g of sodium tungstate dihydrate in 40 mL of deionized water and stir for 0.5 h to obtain a tungstate aqueous solution; dissolve 0.950 g of bismuth nitrate pentahydrate in ethylene glycol and stir for 0.5 h to obtain a bismuth salt alcohol solution; add the tungstate aqueous solution dropwise to the bismuth salt alcohol solution and continue stirring for 1 h to obtain a first mixed solution;
[0054] S2, adding 0.15 g of L-cysteine and 0.050 g of tin tetrachloride pentahydrate to the first mixed solution obtained in S1, and stirring for 2 hours to obtain a second mixed solution;
[0055] S3. Finally, the second mixed solution was transferred to an autoclave and heated at 180°C for 24 hours; the obtained product was filtered, washed, and dried in an oven at 70°C for 24 hours, and the product was collected to obtain a modified bismuth tungstate catalyst, named 0.050-Sn-S-BWO.
[0056] Example 3
[0057] The preparation method of the modified bismuth tungstate catalyst in this embodiment comprises the following steps:
[0058] S1. Dissolve 0.350 g of sodium tungstate dihydrate in 40 mL of deionized water and stir for 0.5 h to obtain a tungstate aqueous solution; dissolve 0.950 g of bismuth nitrate pentahydrate in ethylene glycol and stir for 0.5 h to obtain a bismuth salt alcohol solution; add the tungstate aqueous solution dropwise to the bismuth salt alcohol solution and continue stirring for 1 h to obtain a first mixed solution;
[0059] S2, adding 0.15 g of L-cysteine and 0.040 g of tin tetrachloride pentahydrate to the first mixed solution obtained in S1, and stirring for 2 hours to obtain a second mixed solution;
[0060] S3. Finally, the second mixed solution was transferred to an autoclave and heated at 180°C for 24 hours. The obtained product was filtered, washed, and dried in an oven at 60°C for 24 hours. The product was collected to obtain a modified bismuth tungstate catalyst, named 0.040-Sn-S-BWO.
[0061] Comparative Example 1
[0062] The preparation method of the bismuth tungstate catalyst in this comparative example is different from that in Example 1 in that step S2 is not included; and the obtained catalyst is named BWO.
[0063] Under visible light irradiation for 90 minutes, the photocatalytic degradation efficiencies of the samples for ciprofloxacin and tetracycline were 60.7% and 77.7%, respectively.
[0064] Comparative Example 2
[0065] The difference between the preparation method of the modified bismuth tungstate catalyst in this comparative example and that in Example 1 is that only L-cysteine is added to S2, and no tin tetrachloride pentahydrate is added; the obtained catalyst is named S-BWO.
[0066] Experimental Example 1
[0067] The catalyst samples obtained in each embodiment and comparative example were subjected to photocatalytic degradation experiments under visible light for 90 minutes, and then the photocatalytic degradation efficiency of ciprofloxacin and tetracycline was measured. The results are shown in Table 1.
[0068] It should be noted that the photocatalytic degradation experiment was carried out in the xenon light source system of CEL-LAX500, simulating sunlight and filtering out ultraviolet light with a filter (λ>420nm). All experiments were carried out in a 50mL photochemical reaction tube containing 40mL CIP and 10mg / L TC solution (25℃). Unless otherwise specified, the pH of the solution is the initial value by default. First, add an appropriate amount of catalyst under continuous stirring conditions to make the reaction system reach adsorption-desorption equilibrium and turn on the light source to start further reaction. Unless otherwise specified, the amount of catalyst is 0.5g / L. At regular reaction times, 1mL of the reaction solution was drawn with a syringe equipped with a 0.22μm polyethersulfone syringe filter, and UV-Vis spectral analysis was performed at 271nm (CIP) and 357nm (TC) by a UV spectrophotometer. All experiments were performed 3 times, and the data were averaged. According to the absorbance before and after illumination, the degradation rate of organic pollutants is calculated as η = (C0-Ct) / C0×100%, where C0 is the absorbance of the sample at the beginning of illumination and Ct is the absorbance of the sample after illumination. The degradation rate constant graph is calculated by the pseudo-first-order kinetic model.
[0069] Table 1 - Photocatalytic degradation efficiency of ciprofloxacin and tetracycline
[0070] Ciprofloxacin / % tetracycline / % Example 1 91.5 97.1 Example 2 91.3 97.0 Example 3 91.4 97.2 Comparative Example 1 60.7 77.7 Comparative Example 2 79.1 80.1
[0071] The results in Table 1 show that the modified catalyst prepared in the embodiment of the present invention has excellent photocatalytic degradation efficiency for ciprofloxacin and tetracycline under visible light, which is mainly due to the synergistic effect of the sulfur source and the tin source. 2 WO 6 After being added to the nanosheets, regulating the electronic structure can significantly enhance the catalytic degradation activity of the material, greatly improving the utilization rate of visible light and the overall photocatalytic activity.
[0072] Experimental Example 2
[0073] The catalyst obtained in Example 1 was subjected to a catalytic performance test, as follows:
[0074] The performance of the catalyst obtained in Example 1 in catalytic degradation of CIP and TC at different dosages is shown in Figure 1 ;Depend on Figure 1 The results show that as the catalyst dosage increases from 0.25 g / L to 0.75 g / L, the CIP removal rate of the catalyst in Example 3 increases from 67.2% to 91.5%, and the TC removal rate increases from 74.4% to 97.1%. After the catalyst dosage continues to increase to 0.75 g / L, the CIP removal rate and TC removal rate do not increase significantly over time. Considering that the relatively high catalyst dosage may lead to a light scattering screen, which limits the use of light and the generation of charge carriers to a certain extent, thereby reducing the removal efficiency of organic matter, the appropriate catalyst dosage is determined to be 0.50 g / L.
[0075] The catalyst obtained in Example 1 was tested for its catalytic degradation performance at different initial CIP and TC concentrations at a dosage of 0.5 g / L. The results are shown in Figure 2 ; Figure 2 The effect of initial concentrations of CIP and TC on the removal efficiency when 0.5 g / L of the catalyst obtained in Example 1 is added.
[0076] Depend on Figure 2 The results show that as the concentration increases from 5 mg / L to 20 mg / L, the degradation rates of CIP and TC by the catalyst obtained in Example 1 decrease from 96.3% and 99.6% to 77.3% and 85.5%, respectively. The main reasons for this result are: on the one hand, as the initial concentration increases, the degradation of organic matter requires more active free radicals; on the other hand, as the initial concentration increases, the removal process will produce more degradation intermediates, which will compete with the initial substrate for active free radicals and catalyst surface active sites; at higher concentrations, insufficient free radical production will lead to a decrease in removal efficiency.
[0077] Experimental Example 3
[0078] The catalyst obtained in Example 1 was tested for its recycling performance. The test results are shown in Figure 3 ;Depend on Figure 3It can be seen that the excellent performance stability and structural stability of the catalyst obtained in Example 1 were demonstrated through four consecutive degradation tests. After the cyclic degradation experiment, the removal rate of CIP and TC by the catalyst obtained in Example 1 only decreased by 7.6% (from 91.5% to 83.9%) and 11.4% (from 97.1% to 85.7%). The above results show that the built-in electric field constructed by doping lattice compressive strain electron spin polarization is conducive to maintaining good reusability and structural stability. It can promote the stable and rapid separation of photogenerated charge carriers. Thereby achieving a faster reaction rate and a stable removal effect.
[0079] Experimental Example 4
[0080] The microstructure of the catalysts obtained in Example 1 and Comparative Examples 1-2 was tested, and the scanning electron microscope (SEM) images thereof are shown in FIG. Figure 4 ;Depend on Figure 4 It can be seen that:
[0081] Figure 4 (a) shows that the catalyst obtained in Comparative Example 1 exhibits a closely packed nanosphere structure, while Figure 4 (b) shows that the catalyst structure of the catalyst obtained in Comparative Example 2 shows obvious layered changes after L-cysteine sulfur doping; Figure 4 It can be seen in (c) that when tin doping is added, due to the generation of compressive strain, the microstructure of the catalyst of Example 1 of the present invention is between the two forms. The nanosheets and spheres are intertwined to form a slightly wrinkled irregular shape, which is also conducive to the adsorption of target molecules, enhances the dispersion of incident light on the surface of the material, and enhances the catalytic activity.
[0082] Experimental Example 5
[0083] The microstructure of the catalyst obtained in Example 1 was further observed. Specifically, the transmission electron microscope (TEM) and scanning electron microscope-energy dispersive spectrometer (SEM-EDS) images are shown in FIG. Figure 5 ;Depend on Figure 5 It can be seen that the lattice distances observed by high-resolution transmission electron microscopy are 0.271 and 0.374 nm, respectively, belonging to the (200) and (113) planes of Comparative Example 1, which are consistent with the XRD results. The evolution of the nanostructure to defects and compressed states promotes the movement of electrons between the built-in electric field and enhances the catalytic activity. In addition, TEM-EDS mapping shows the uniform distribution of all elements (Sn, S, Bi, W and O) in the composite material.
[0084] Experimental Example 6
[0085] The phase structure and crystallization of the catalyst samples obtained in Example 1 and Comparative Examples 1-2 were further analyzed, and the X-ray diffraction (XRD) patterns of the obtained catalysts are shown in Figure 6 ,Depend on Figure 6 It can be seen that:
[0086] The phase structure and crystallinity of the synthesized photocatalysts were analyzed by XRD. The diffraction peaks of all examples correspond to Bi 2 WO 6 The XRD patterns of the differently doped BWO samples still retain the prominent diffraction peaks of the BWO (113), (200) and (220) crystal planes, indicating that the doped catalysts do not significantly change the overall structure of the original BWO.
[0087] Experimental Example 7
[0088] The chemical bonds of the catalyst samples obtained in Example 1 and Comparative Examples 1-2 were further analyzed, and the obtained Fourier transform infrared spectra (FT-IR) were shown in FIG. Figure 7 ,Depend on Figure 7 It can be seen that:
[0089] In the picture 577cm -1 and 735cm -1 The vibration at 1426 cm-1 is attributed to the stretching vibration of the Bi-O and WO bonds in the BWO obtained in Comparative Example 1. The peak vibration of the Bi-O bond increases after doping, and the decrease in the WO peak intensity indicates a decrease in the vibration group. The carboxyl group of L-cysteine (-COO-, 1426 cm-1 -1 and 1665cm -1 ) and Bi-S bonds (603cm -1 ) shows that O 2- The lattice doping part is S 2- Substitution, -OH at 990cm -1 The tensile vibration at the point is significantly reduced, indicating that the amount of water absorbed by the material surface is reduced.
[0090] Experimental Example 8
[0091] The light absorption capacity of the catalyst samples obtained in Example 1 and Comparative Examples 1-2 was evaluated by UV-vis DRS spectroscopy. The UV-visible diffuse reflectance spectra (UV-vis DRS) of the obtained catalysts are shown in FIG. Figure 8 ;like Figure 8 As shown, the BWO material obtained in Comparative Example 1 exhibits a sharp absorption edge in the ultraviolet region of about 380 nm, while the S-BWO material obtained in Comparative Example 2 exhibits higher light absorption efficiency in the visible light region. After tin doping, the 0.045-Sn-S-BWO material obtained in Example 1 generates an intermediate impurity level, and the quantum confinement effect further reduces the transition energy of photoexcited electrons. The light absorption range is slightly red-shifted, and the light absorption intensity of all doped materials is higher than that of the BWO obtained in Comparative Example 1.
[0092] Experimental Example 9
[0093] The PL spectroscopy method was used to evaluate the separation efficiency of photogenerated carriers for the catalyst samples obtained in Example 1 and Comparative Examples 1-2. Fig. 9 Transient photocurrent (It) and steady-state photoluminescence (PL) spectra of the catalyst. Fig. 9 As shown, in the transient photocurrent results, the 0.045-Sn-S-BWO obtained in Example 1 has the highest photocurrent, indicating that the electron-hole separation and light utilization efficiency are the highest. And the 0.045-Sn-S-BWO obtained in Example 1 shows the lowest fluorescence intensity on multiple characteristic peaks, indicating that the less the recombination of photogenerated carriers, the higher the electron separation efficiency.
[0094] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A modified bismuth tungstate catalyst, characterized in that: It includes a soluble bismuth salt, a soluble tungstate, a sulfur source and a tin source.
2. The modified bismuth tungstate catalyst according to claim 1, characterized in that The mass ratio of the soluble bismuth salt, the soluble tungstate, the sulfur source and the tin source is 15-25:5-10:2-5:
1.
3. The modified bismuth tungstate catalyst according to claim 1 or 2, characterized in that: The soluble bismuth salt is bismuth nitrate and / or bismuth nitrate pentahydrate.
4. The modified bismuth tungstate catalyst according to claim 1 or 2, characterized in that: The soluble tungstate is sodium tungstate and / or sodium tungstate dihydrate.
5. The modified bismuth tungstate catalyst according to claim 1 or 2, characterized in that: The sulfur source is cysteine and / or L-cysteine.
6. The modified bismuth tungstate catalyst according to claim 1 or 2, characterized in that: The tin source is tin tetrachloride and / or tin tetrachloride pentahydrate.
7. A method for preparing a modified bismuth tungstate catalyst according to any one of claims 1 to 6, characterized in that: The method comprises the following steps: (1) reacting a soluble bismuth salt with a tungstate to generate a bismuth tungstate catalyst core; and (2) modifying the bismuth tungstate catalyst core by doping a sulfur source and a tin source to obtain a modified bismuth tungstate catalyst.
8. The method for preparing the modified bismuth tungstate catalyst according to claim 7, characterized in that: The following steps are involved: S1, dissolving a soluble bismuth salt in an alcohol solvent to obtain a bismuth salt alcohol solution, dissolving a soluble tungstate in water to obtain a tungstate aqueous solution; dropping the tungstate aqueous solution into the bismuth salt alcohol solution and continuously stirring for a period of time to obtain a first mixed solution, i.e., a bismuth tungstate catalytic core; S2, adding a sulfur source and a tin source to the first mixed solution obtained in S1 in sequence, and stirring for a period of time to obtain a second mixed solution; S3, heating, filtering, washing and drying the second mixed solution obtained in S2 to obtain a modified bismuth tungstate catalyst.
9. The method for preparing the modified bismuth tungstate catalyst according to claim 8, characterized in that: In S3, the second mixed solution is heated at 150-200° C. for 20-30 hours; then the obtained product is filtered, washed, and dried in an oven at 50-80° C. for 20-30 hours.
10. Use of the modified bismuth tungstate catalyst according to any one of claims 1 to 6 or the modified bismuth tungstate catalyst prepared by the preparation method according to any one of claims 8 to 9 in degradation of antibiotic-containing wastewater under visible light.
Citation Information
Patent Citations
Preparation method for synthesizing photocatalyst SnS2 / Bi2WO6 nanosheets with visible-light response
CN107754819A
Tin sulfide-bismuth tungstate composite micron flower-shaped spheres as well as preparation method and application thereof
CN108355678A
Catalytic bed comprising a particular photocatalytic catalyst
WO2022078856A1