Preparation method and application of P-Mo2N and preparation method and application of photocatalyst

By synthesizing P-Mo2N cocatalyst at a lower temperature and compounding it with Cd0.5Zn0.5S, the problem of excessive particle size and lack of active sites caused by the reaction of traditional MoxN catalyst at high temperature is solved, and the hydrogen evolution performance of the photocatalyst is significantly improved. Performance beyond Pt modification.

CN118719112APending Publication Date: 2024-10-01HEBEI UNIV OF SCI & TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410762099.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Traditional MoxN catalysts need to react at higher temperatures, resulting in thermal agglomeration to form large particles and a lack of surface active sites, affecting their catalytic performance.

Method used

Using PEG as an inducer, regular-shaped nanoflake precursors are synthesized at a lower temperature. Small-sized nanoparticle P-Mo2N cocatalysts are prepared through a one-step calcination method and compounded with Cd0.5Zn0.5S to construct Schottky interface to improve electron transfer efficiency.

Benefits of technology

Through the P-Mo2N@Cd0.5Zn0.5S composite catalyst, the electron utilization efficiency and hydrogen evolution performance of the photocatalyst are significantly improved, surpassing the performance of Pt modification and twice that of Pt-modified Cd0.5Zn0.5S.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118719112A_ABST
    Figure CN118719112A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method and application of P-Mo2N and a preparation method and application of a photocatalyst, the preparation method of the P-Mo2N comprises the following steps: S1, taking melamine, PEG and phosphomolybdic acid, dissolving in water, placing in a flask, heating, stirring, washing and drying to obtain a precursor; the mass ratio of the melamine to the PEG to the phosphomolybdic acid is (2-8): (0.2-2): 3; s2, the precursor and sodium hypophosphite are mixed and then calcined in inert gas, phosphorus-doped molybdenum nitride P-Mo2N is obtained, the mass ratio of the precursor to the sodium hypophosphite is (1.5-2.5): 3, PEG is adopted as an inducer, melamine and phosphomolybdic acid are induced at a low temperature to be synthesized into a nanosheet-shaped precursor with a regular shape, and the phosphorus-doped molybdenum nitride P-Mo2N is obtained. The small-size nano-particle P-Mo2N cocatalyst is prepared by a one-step calcination method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of inorganic synthesis, and in particular to a preparation method and application of P-Mo2N and a preparation method and application of a photocatalyst. Background Art

[0002] The excessive use of fossil fuels has led to energy crises and environmental pollution. There is an urgent need to explore clean, environmentally friendly and sustainable green energy. Hydrogen has high energy density and its combustion products are pollution-free. It is expected to become an ideal alternative energy source for fossil fuels. Photocatalytic water decomposition technology for hydrogen production has the characteristics of deep reaction at room temperature and pressure. It can maximize the use of solar energy to produce hydrogen and has become a green hydrogen production technology with important application prospects.

[0003] To date, a variety of semiconductor photocatalysts have been synthesized and applied to photocatalytic hydrogen production. However, the photocatalysts currently used generally have the problem of easy recombination of photogenerated carriers and slow reaction kinetics, which has become a bottleneck restricting the overall efficiency of the reaction. In recent years, the introduction of co-catalysts has been proven to be a successful strategy to improve the activity, stability and selectivity of semiconductor photocatalysts. In particular, the precious metal Pt has been proven to be a highly active co-catalyst for photocatalytic hydrogen production of various photocatalysts. However, the high cost and extreme scarcity of Pt have seriously hindered its large-scale application.

[0004] Among them, Mo x N-based catalysts are considered to be strong competitors to replace Pt catalysts due to their Pt-like electronic structure, high conductivity, stable physicochemical properties, wide pH applicability, and excellent HER performance. x The initial water dissociation process of H2O on the N surface to form adsorbed H* is very slow, which is contrary to the ideal HER catalyst that should have strong water dissociation ability and appropriate H* adsorption energy. x N catalysts often need to react at higher temperatures to be obtained, which makes them easily thermally agglomerated to form large particles, resulting in a lack of surface active sites. Summary of the invention

[0005] Therefore, the technical problem to be solved by the present invention is to overcome the traditional Mo x N catalysts often need to react at higher temperatures to be obtained, which makes them easily thermally agglomerated to form large particles, thereby causing defects such as lack of surface active sites. This paper provides a preparation method and application of P-Mo2N and P-Mo2N@Cd 0.5 Zn 0.5 Preparation method and application of S composite catalyst.

[0006] In order to solve the above technical problems, the invention provides a method for preparing P-Mo2N, comprising the following steps:

[0007] S1, taking melamine, PEG and phosphomolybdic acid, dissolving them in water and placing them in a flask, heating, stirring, washing and drying to obtain a precursor; the mass ratio of melamine, PEG and phosphomolybdic acid is (2-8): (0.2-2): 3;

[0008] S2, after mixing the above-mentioned precursor and sodium hypophosphite, calcining them under inert gas to obtain phosphorus-doped molybdenum nitride P-Mo2N, the mass ratio of the precursor and sodium hypophosphite is (1.5-2.5):3.

[0009] As a preferred embodiment, in step S1, the heating temperature is 60-70°C and the stirring time is 0.5-1.5 hours.

[0010] As a preferred embodiment, in step S1, the PEG is one of PEG-2000, PEG-4000 and PEG-6000.

[0011] As a preferred embodiment, in step S2, sodium hypophosphite is first placed at the bottom of the container, a layer of carbon cloth is covered on the surface of the sodium hypophosphite, the prepared precursor is spread on the carbon cloth, and the container is placed in a tubular furnace filled with argon for calcination.

[0012] As a preferred solution, in step S2, during the calcination process, the heating rate is 3-6°C / min, the calcination temperature is 500-700°C, and the calcination time is 4-6 hours.

[0013] The present invention also provides a use of the P-Mo2N described in any one of the above items in a photocatalytic hydrogen evolution reaction.

[0014] The present invention also provides a method for preparing a photocatalyst, comprising the following steps:

[0015] S1, weighing cadmium acetate and zinc acetate and dissolving them in water to obtain a clear solution; the molar ratio of cadmium acetate to zinc acetate is 1:1;

[0016] S2, adding the P-Mo2N prepared in any one of claims 1 to 4 to the above clear solution, adjusting the pH value to between 7 and 7.5, stirring, washing, and drying to prepare P-Mo2N@Cd 0.5 Zn 0.5 S composite catalyst;

[0017] The mass ratio of the P-Mo2N to zinc acetate is (0.05-0.2):1.

[0018] As a preferred solution, the pH is adjusted using sodium hydroxide at a concentration of 0.2 mol / L.

[0019] The present invention also provides application of the photocatalyst prepared by the above preparation method in photocatalytic hydrogen production.

[0020] The technical solution of the present invention has the following advantages:

[0021] 1. The present invention provides a method for preparing P-Mo2N, which uses PEG as an inducing agent to induce melamine and phosphomolybdic acid to synthesize a nano-flake precursor with a regular shape at a relatively low temperature, and prepares a small-sized nano-particle P-Mo2N co-catalyst by a one-step calcination method.

[0022] 2. The present invention provides a P-Mo2N@Cd 0.5 Zn 0.5 Preparation method of S composite catalyst, using P-Mo2N as a co-catalyst to modify the relatively stable ternary Cd 0.5 Zn 0.5 S, to construct Schottky interface. P-Mo2N as co-catalyst and Cd 0.5 Zn 0.5 After S is combined, it has a lower Mott-Schottky barrier, thus enhancing the electron transfer in the semiconductor photocatalyst Cd 0.5 Zn 0.5 The transmission between S and P-Mo2N improves the utilization efficiency of photocatalyst electrons, thereby greatly improving the hydrogen evolution performance of the photocatalyst. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0024] Figure 1 is the XRD pattern of the P-Mo2N co-catalyst prepared in Example 1 of the present invention;

[0025] Figure 2 This is the XPS full spectrum scan of the P-Mo2N co-catalyst prepared in Example 1 of the present invention;

[0026] Figure 3 is a SEM image of the precursor prepared in Example 1 of the present invention;

[0027] Figure 4 is a SEM image of the P-Mo2N co-catalyst prepared in Example 1 of the present invention;

[0028] Figure 5 are XRD diffraction patterns of P-Mo2N prepared in Example 1 of the present invention, ZCS prepared in Example 7, ZCS / Mo2N-10 prepared in Example 4, and ZCS / Mo2N-5 prepared in Example 5;

[0029] Figure 6 This is the XPS full spectrum scan of ZCS / Mo2N-10 prepared in Example 4 of the present invention;

[0030] Figure 7 1 is a hydrogen production performance diagram in Experimental Example 1, Experimental Example 2 and Experimental Example 3 of the present invention;

[0031] Figure 8 It is the DRS spectrum of P-Mo2N prepared in Example 1 of the present invention, ZCS prepared in Example 7, ZCS / Mo2N-10 prepared in Example 4 and ZCS / Mo2N-5 prepared in Example 5. DETAILED DESCRIPTION

[0032] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0033] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0034] Example 1

[0035] Melamine, PEG-4000 and phosphomolybdic acid were dissolved in water in a mass ratio of 5:1:3, placed in a round-bottom flask, stirred at 65°C for 1 hour, washed with distilled water and dried to obtain a precursor;

[0036] Take sodium hypophosphite and put it at the bottom of the porcelain boat, cover the surface of the sodium hypophosphite with a layer of carbon cloth, and evenly spread the prepared precursor on the carbon cloth. The mass ratio of the precursor to the sodium hypophosphite is 2:3. Put the above porcelain boat into a tubular furnace with argon gas, the heating rate is 5℃ / min, the calcination temperature is 600℃, and the calcination time is 5 hours, and the P-Mo2N co-catalyst can be prepared.

[0037] Example 2

[0038] Melamine, PEG-2000 and phosphomolybdic acid were dissolved in water in a mass ratio of 2:0.2:3, placed in a round-bottom flask, stirred at 60°C for 0.5 hours, washed with distilled water and dried to obtain a precursor;

[0039] Sodium hypophosphite is placed at the bottom of a porcelain boat, a layer of carbon cloth is placed on the surface of the sodium hypophosphite, and the prepared precursor is evenly spread on the carbon cloth. The mass ratio of the precursor to the sodium hypophosphite is 1.5:3. The porcelain boat is placed in a tubular furnace filled with argon gas. The heating rate is 3°C / min, the calcination temperature is 500°C, and the calcination time is 6 hours. P-Mo2N co-catalyst can be prepared.

[0040] Example 3

[0041] Melamine, PEG-6000 and phosphomolybdic acid were dissolved in water in a mass ratio of 8:2:3, placed in a round-bottom flask, stirred at 70°C for 1.5 hours, washed with distilled water and dried to obtain a precursor;

[0042] Take sodium hypophosphite and put it at the bottom of the porcelain boat, cover the surface of the sodium hypophosphite with a layer of carbon cloth, and evenly spread the prepared precursor on the carbon cloth. The mass ratio of the precursor to the sodium hypophosphite is 2.5:3. Put the above porcelain boat into a tubular furnace with argon gas, the heating rate is 6°C / min, the calcination temperature is 700°C, and the calcination time is 4 hours, and the P-Mo2N co-catalyst can be prepared.

[0043] Figure 1 The XRD diagram of the P-Mo2N co-catalyst prepared in Example 1 shows that the main diffraction peaks of the obtained P-Mo2N are in the same position as the standard card peaks of Mo2N (PDF#25-1366), and the diffraction peaks at 37.4°, 43.4°, 63.2°, and 75.6° can be well matched with the (110), (200), (220), and (311) crystal planes of Mo2N on the standard card. It can be seen that the black sample calcined at 600°C is the P-Mo2N nanoparticles.

[0044] Figure 2 This is the XPS full spectrum scan of the P-Mo2N co-catalyst prepared in Example 1. It can be seen from the figure that the P-Mo2N sample mainly contains N, O, Mo, P, and C elements. This proves that P is successfully doped into Mo2N.

[0045] Figure 3 This is a SEM image of the precursor prepared in Example 1. The long-chain PEG-4000 can regulate the assembly process of melamine and molybdenum phosphate, inducing the precursor to form uniform nanosheets as shown in the figure, which plays an important role in the subsequent calcination to form a P-Mo2N co-catalyst with uniform structure and morphology.

[0046] Figure 4 This is a SEM image of the P-Mo2N co-catalyst prepared in Example 1. It can be seen from the figure that P-Mo2N is nanoparticles with uniform morphology.

[0047] Example 4

[0048] 0.399 g of cadmium acetate and 0.329 g of zinc acetate were weighed and put into 25 ml of distilled water to obtain a clear solution. Then 0.0399 g of the P-Mo2N cocatalyst prepared in Example 1 was weighed, and the pH was adjusted to 7.3 with 0.2 mol / L sodium hydroxide. The mixture was stirred at room temperature for 18 hours, washed, and dried to obtain P-Mo2N@Cd 0.5 Zn 0.5 S composite photocatalyst, denoted as ZCS / Mo2N-10.

[0049] Example 5

[0050] 0.399 g of cadmium acetate and 0.329 g of zinc acetate were weighed and put into 25 ml of distilled water to obtain a clear solution. Then 0.0181 g of the P-Mo2N cocatalyst prepared in Example 1 was weighed, and the pH was adjusted to 7.3 with 0.2 mol / L sodium hydroxide. The mixture was stirred at room temperature for 18 hours, washed, and dried to obtain P-Mo2N@Cd 0.5 Zn 0.5 S composite photocatalyst, denoted as ZCS / Mo2N-5.

[0051] Example 6

[0052] 0.399 g of cadmium acetate and 0.329 g of zinc acetate were weighed and put into 25 ml of distilled water to obtain a clear solution. Then 0.0726 g of the P-Mo2N cocatalyst prepared in Example 1 was weighed, and the pH was adjusted to 7.3 with 0.2 mol / L sodium hydroxide. The mixture was stirred at room temperature for 18 hours, washed, and dried to obtain P-Mo2N@Cd 0.5 Zn 0.5 S composite photocatalyst, denoted as ZCS / Mo2N-5.

[0053] Example 7

[0054] Weigh 0.399g of cadmium acetate and 0.329g of zinc acetate into 25ml of distilled water to obtain a clear solution, adjust the pH to 7.3 with 0.2mol / L sodium hydroxide, stir at room temperature for 18 hours, wash, and dry to obtain Cd 0.5 Zn 0.5 S photocatalyst, denoted as ZCS.

[0055] Figure 5 The XRD diffraction patterns of P-Mo2N prepared in Example 1, ZCS prepared in Example 7, ZCS / Mo2N-10 prepared in Example 4, and ZCS / Mo2N-5 prepared in Example 5 are shown in order. 0.5 Zn 0.5 The role of S is to serve as a control. As can be seen from the figure, in Cd 0.5 Zn 0.5 After adding different mass ratios of P-Mo2N samples to S, the XRD diffraction peaks did not change much, and no diffraction peaks of P-Mo2N were shown. 0.5 Zn 0.5 The mass of P-Mo2N added to the S complex is very small, so P-Mo2N / Cd 0.5 Zn 0.5 No diffraction peak of P-Mo2N can be detected in the XRD diffraction pattern of the S composite.

[0056] Figure 6 P-Mo2N@Cd prepared in Example 4 0.5 Zn 0.5 XPS full spectrum scanning diagram of S composite photocatalyst. It can be seen from the figure that P-Mo2N@Cd 0.5 Zn 0.5 The S composite photocatalyst mainly contains N, Mo, P, C, Cd, Zn and S elements.

[0057] Experimental Example 1

[0058] Take 10 mg of P-Mo2N@Cd prepared in Example 4 0.5 Zn 0.5 The S composite photocatalyst and 30 ml of lactic acid aqueous solution were placed in a quartz reactor and continuously stirred. At the same time, the temperature in the reactor was stabilized at 15°C. A xenon lamp was used as the light source for irradiation (300w, Perfect Light, with a 400nm cutoff filter), Ar was used as the carrier gas, and the hydrogen production performance was analyzed every 1 hour by a gas chromatograph (Techcomp GC7900, thermal conductivity detector).

[0059] Experimental Example 2

[0060] Take 10 mg of Cd prepared in Example 7 0.5 Zn 0.5S photocatalyst and 30 ml of lactic acid aqueous solution were placed in a quartz reactor and continuously stirred. At the same time, the temperature in the reactor was stabilized at 15°C. A xenon lamp was used as the light source for irradiation (300w, Perfect Light, with a 400nm cutoff filter), Ar was used as the carrier gas, and the hydrogen production performance was analyzed every 1 hour by a gas chromatograph (Techcomp GC7900, thermal conductivity detector).

[0061] Experimental Example 3

[0062] Take 10 mg of Cd prepared in Example 6 0.5 Zn 0.5 S photocatalyst, 0.5 ml chloroplatinic acid and 30 ml lactic acid aqueous solution were placed in a quartz reactor and stirred continuously. At the same time, the temperature in the reactor was stabilized at 15 ° C. A xenon lamp was used as a light source (300 w, Perfect Light, with a 400 nm cutoff filter) to pre-illuminate the quartz reactor for 30 min. 0.5 Zn 0.5 Precious metal Pt was deposited on the surface of the S photocatalyst. After exhaust, the quartz reactor was illuminated with a xenon lamp as the light source (300w, Perfect Light, with a 400nm cutoff filter). Ar was used as the carrier gas and the hydrogen production performance was analyzed every 1 hour by a gas chromatograph (Techcomp GC7900, thermal conductivity detector).

[0063] Figure 7 The hydrogen production performance diagrams in Experimental Examples 1, 2 and 3 show that the introduction of the promoter P-Mo2N significantly improves the Cd 0.5 Zn 0.5 The photocatalytic hydrogen evolution activity of S is Pt modified Cd 0.5 Zn 0.5 Twice as S.

[0064] Figure 8 The DRS spectra of P-Mo2N prepared in Example 1, ZCS prepared in Example 7, ZCS / Mo2N-10 prepared in Example 4, and ZCS / Mo2N-5 prepared in Example 5 are shown in the figure. It can be seen that in the wavelength range of 600-800nm, the P-Mo2N@Cd prepared in Example 4 and Example 5 0.5 Zn 0.5 The absorption intensity of the S composite photocatalyst is significantly higher than that of the Cd prepared in Example 7. 0.5 Zn 0.5 The photocatalyst of S.

[0065] In summary, the present invention is based on the fact that heteroatom doping of transition metal carbides is one of the effective ways to adjust their electronic structure, promote charge transfer, and enhance the efficiency of the catalyst hydrogen evolution reaction. x The metallic properties and excellent hydrogen evolution kinetics of N are achieved by introducing P elements with lone pairs of electrons and high electronegativity. x On the basis of improving the kinetics of hydrogen evolution by N, Mo x Regulation of N Fermi level.

[0066] The present invention uses PEG as an inducing agent to induce melamine and phosphomolybdic acid to synthesize a nano-sheet precursor with a regular shape, and then prepares a small-sized nano-sheet P-Mo2N co-catalyst by a one-step calcination method at a relatively low temperature, and then reacts with cadmium acetate and zinc acetate at room temperature to prepare a highly active P-Mo2N@Cd 0.5 Zn 0.5 S composite catalyst. The introduction of the promoter P-Mo2N greatly increased the 0.5 Zn 0.5 The photocatalytic hydrogen evolution activity of S is Pt modified Cd 0.5 Zn 0.5 The method of the invention has mild experimental conditions, a simple preparation system, easy operation, easily controllable conditions, and stable quality and excellent performance of the obtained product.

[0067] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A kind of P-Mo 2 Preparation method of N, It is characterized in that The following steps are involved: S1, taking melamine, PEG and phosphomolybdic acid, dissolving them in water and placing them in a flask, heating, stirring, washing and drying to obtain a precursor; the mass ratio of melamine, PEG and phosphomolybdic acid is (2-8): (0.2-2): 3; S2, after mixing the above precursor and sodium hypophosphite, calcining under inert gas to obtain phosphorus-doped molybdenum nitride P-Mo 2 N, the mass ratio of the precursor to sodium hypophosphite is (1.5-2.5):

3.

2. The P-Mo according to claim 1 2 Preparation method of N, It is characterized in that In step S1, the heating temperature is 60-70°C and the stirring time is 0.5-1.5 hours.

3. The P-Mo according to claim 1 2 Preparation method of N, It is characterized in that In step S1, the PEG is one of PEG-2000, PEG-4000 and PEG-6000.

4. The P-Mo according to claim 1 2 Preparation method of N, It is characterized in that In step S2, sodium hypophosphite is first placed at the bottom of a container, a layer of carbon cloth is placed on the surface of the sodium hypophosphite, the prepared precursor is spread on the carbon cloth, and the container is placed in a tubular furnace filled with argon for calcination.

5. The P-Mo according to claim 4 2 Preparation method of N, It is characterized in that In step S2, during the calcination process, the heating rate is 3-6°C / min, the calcination temperature is 500-700°C, and the calcination time is 4-6 hours.

6. The P-Mo according to any one of claims 1 to 4 2 Application of N in photocatalytic hydrogen evolution reaction.

7. A method for preparing a photocatalyst, It is characterized in that The following steps are involved: S1, weighing cadmium acetate and zinc acetate and dissolving them in water to obtain a clear solution; the molar ratio of cadmium acetate to zinc acetate is 1:1; S2, adding the P-Mo prepared in any one of claims 1 to 4 to the above clear solution 2 N, adjust the pH value to between 7 and 7.5, stir, wash and dry to prepare P-Mo 2 N@C 0.5 Zn 0.5 S photocatalyst; The P-Mo 2 The mass ratio of N to zinc acetate is (0.05-0.2):

1.

8. The method for preparing a photocatalyst according to claim 6, It is characterized in that The pH was adjusted with 0.2 mol / L sodium hydroxide.

9. Use of the photocatalyst prepared by the preparation method of claim 7 or 8 in photocatalytic hydrogen production.

Citation Information

Patent Citations

  • Hexagonal-rod-shaped Mo2N, preparation thereof and application

    CN106006582A

  • Mo2N / MoO3 / C compound lithium ion battery negative material and preparation method thereof

    CN109841815A

  • MoP / Mo2N composite material as well as preparation method and application thereof

    CN113942982A

  • Molybdenum carbide particle size dependent nitrogen-doped carbon material catalyst as well as preparation method and application thereof

    CN115106111A

  • Molybdenum ceramic-based nanocomposite sorbent for removal of organic pollutants from water

    US20240024843A1