A catalyst for preparing chlorine from hydrogen chloride and its preparation method and application
By supporting copper, alkali metal, rare earth and tripolyphosphate on the activated alumina support, the corrosion-resistant catalyst is formed, and the problem of existing catalysts being deactivated under a fluorine-containing atmosphere is solved, achieving efficient, stable and environmentally friendly HCl Catalytic oxidation process for Cl2 is suitable for industrial applications.
Patent Information
- Application Number
- CN202411231556.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-09-04
AI Technical Summary
Existing catalysts are prone to inactivation in an environment containing trace amounts of HF and cannot effectively treat HCl gases containing a variety of gaseous fluorides, resulting in low utilization of chlorine resources and risk of environmental pollution.
Using activated alumina as a support, copper salt, alkali metal salt, rare earth metal salt and tripolyphosphate are supported, and the stability and activity of the catalyst are improved by forming coordination bonds, and a catalyst that is resistant to corrosion of fluorine-containing gas is prepared.
In an HCl atmosphere containing 1200 ppm fluoride, the catalyst maintains high catalytic activity and stability, has a low reaction temperature, high conversion rate, long service life, low cost, is suitable for industrial production, does not contain toxic components, and is environmentally friendly.
Smart Images

Figure CN118719141B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalysts, in particular to a catalyst for preparing chlorine from hydrogen chloride and a preparation method and application thereof. Background Art
[0002] In recent years, the fluorine chemical industry has developed rapidly, and most product grades have been continuously increased, forming a fluorine chemical product system. Usually, in the chlorine fluorination production process, the atomic utilization rate of chlorine resources is low, and the maximum does not exceed 50%. The remaining chlorine produces a large amount of hydrogen chloride as a by-product. Most of the impurity gases can be separated out of the by-product HCl gas during the distillation process, but there will still be about 10-5000ppm of fluorine-containing gases (such as hydrogen fluoride, hydrofluorocarbons, chlorofluorocarbons, etc.) in the HCl gas. Therefore, how to deal with this type of fluorine-containing HCl is an important issue in the fluorine chemical industry.
[0003] The production of chlorine from byproduct HCl has great economic value and environmental benefits. At present, electrolysis, direct oxidation and catalytic oxidation are commonly used to achieve the conversion of HCl to chlorine. Among them, the catalytic oxidation method has the advantages of low energy consumption and simple operation, and has become the most economical method for treating byproduct HCl to realize chlorine resource utilization. Currently, the ruthenium-based catalysts commonly used in industry, such as RuO2-SiO2 or RuO2-Al2O3, have high reaction activity, but in the presence of trace HF (>10 ppm), SiF4 and AlF3 will be generated, causing the catalyst to be deactivated. Therefore, in view of the industrial status quo that byproduct HCl contains a variety of gaseous fluorides, considering the influence of fluorine-containing gases on the activity of catalysts, it is of great significance to develop HCl oxidation catalysts that are resistant to fluorine-containing gas corrosion.
[0004] In addition to traditional copper-based catalysts, highly active chromium-based (CN114558581A), ruthenium-based (CN116078379A) and alloy-based catalysts (CN115814815A) have developed rapidly in recent years. Although these catalysts show high activity and certain application effects in the catalytic oxidation of HCl to produce Cl2, there are few reports on the application of HCl catalytic oxidation to prepare Cl2 in a fluorine-containing atmosphere. Patent document CN109607478A discloses a process for the one-step oxidation of HCl and HF mixed gas to produce Cl2, which uses a chromium-ruthenium-based catalyst resistant to HF corrosion, but the chromium-based catalyst has high biological toxicity and is prone to environmental pollution, which is not suitable for industrial production. Patent document CN101722019A discloses a catalyst loaded with RuO2 on a MgF2 carrier. Although it realizes the catalytic oxidation of HCl at low temperature, the catalytic oxidation rate of HCl is less than 10%, which cannot really meet the needs of industrial applications. Therefore, in the catalytic oxidation of by-product HCl to Cl2 in an atmosphere containing a variety of gaseous fluorides, there is an urgent need for a catalyst that can be used stably and continuously to meet the needs of industrial production. Summary of the invention
[0005] The purpose of the present invention is to overcome the above-mentioned deficiencies of the prior art and provide a catalyst for preparing chlorine from hydrogen chloride and a preparation method and application thereof. The catalyst can not only achieve efficient catalysis of hydrogen chloride in a fluoride atmosphere, but also has good stability and a long service life.
[0006] In order to achieve the above technical effects, the present invention adopts the following technical solutions:
[0007] A catalyst for preparing chlorine from hydrogen chloride, comprising a carrier and an active component loaded on the carrier,
[0008] The carrier is activated alumina, and the active components include copper salt, alkali metal salt, rare earth metal salt and polyphosphate. The polyphosphate in the polyphosphate forms a coordination bond with the copper ion in the copper salt.
[0009] The copper salt is selected from copper chloride, copper nitrate or copper acetate;
[0010] The alkali metal salt is selected from the chloride or nitrate of lithium, the chloride or nitrate of sodium or the chloride or nitrate of potassium;
[0011] The rare earth metal salt is selected from at least one of nitrate or chloride of lanthanum, nitrate or chloride of cerium, or nitrate or chloride of samarium;
[0012] The polyphosphate is sodium tripolyphosphate;
[0013] The mass percentages of active ingredients and carriers are as follows:
[0014] 8-20wt% of copper salt, 0.05-5wt% of alkali metal salt, 4-20wt% of rare earth metal salt, 0.05-2wt% of polyphosphate and 55-80wt% of activated alumina.
[0015] Preferably, the copper salt is copper chloride or copper nitrate; and the alkali metal is sodium chloride or potassium chloride.
[0016] Preferably, the mass percentages of the active ingredient and the carrier are as follows:
[0017] 8-17wt% of copper salt, 1-4wt% of alkali metal salt, 7-18wt% of rare earth metal salt, 0.2-1.5wt% of sodium tripolyphosphate, and 65-80wt% of carrier.
[0018] The present invention also provides a method for preparing the above catalyst, comprising the following steps:
[0019] S1. Dissolving a copper salt, an alkali metal salt, a rare earth metal salt and sodium tripolyphosphate in a solvent to obtain a mixed solution;
[0020] S2. The carrier is added to the mixed solution obtained in step S1, and the solid intermediate product is collected by filtration after standing;
[0021] S3. The solid intermediate product collected in step S2 is dried, kept at 250°C, calcined, and cooled to obtain a catalyst.
[0022] Preferably, in step S1, the mass ratio of the amount of solvent to the copper salt is (4-9): 1. Further preferably, the mass ratio of the amount of solvent to the copper salt is (4-7): 1.
[0023] Preferably, in step S1, the specific operation of the dissolving process in the solvent is as follows: after the copper salt, alkali metal salt, rare earth metal salt and polyphosphate are added into the solvent, they are stirred in a constant temperature water bath at 40°C-60°C for 0.5h-2h until the solute is completely dissolved.
[0024] Preferably, in step S1, the solvent is water or acetic acid solution; further preferably, the concentration of the acetic acid solution is 5%-25%; more preferably, the concentration of the acetic acid solution is 20%.
[0025] Preferably, in step S2, the mass ratio of the carrier to the mixed solution is 1:(1-3); further preferably, the mass ratio of the carrier to the mixed solution is 1:1.5.
[0026] Preferably, in step S2, the standing time is 4h-8h; further preferably, the standing time is 6h.
[0027] Preferably, in step S3, the drying method is drying at 90°C-130°C for 3h-10h; further preferably, the drying method is drying at 100°C-120°C for 6h-10h.
[0028] Preferably, in step S3, the calcination method is calcination at 550°C-650°C for 4h-10h; further preferably, the calcination method is calcination at 580°C-650°C for 5h-8h.
[0029] The present invention also provides the use of the catalyst or the catalyst prepared by the preparation method to catalyze hydrogen chloride to produce chlorine in a fluoride atmosphere.
[0030] Preferably, the application method is as follows:
[0031] The catalyst is loaded into the constant temperature zone of the fixed bed reactor. After the temperature of the fixed bed is stabilized, O2 and fluoride-containing HCl are introduced. After being preheated to the reaction temperature, a reaction occurs in the catalyst bed to produce Cl2.
[0032] Preferably, the fluoride includes at least one of HF, hydrofluorocarbon and hydrochlorofluorocarbon; further preferably, the concentration of HF is 100-1000 ppm; the concentration of hydrofluorocarbon is 100-300 ppm; the concentration of hydrochlorofluorocarbon is 50-200 ppm.
[0033] Preferably, the molar ratio of HCl to O2 is 2:1; the reaction temperature is 360°C-410°C, and the reaction pressure is normal pressure; further preferably, the reaction temperature is 360°C-390°C.
[0034] Preferably, the volume space velocity of HCl is 240h -1 -1600h -1 Further preferably, the volumetric space velocity of HCl is 320h -1 -960h -1 .
[0035] The beneficial effects of the present invention are as follows:
[0036] 1. The catalyst prepared by the present invention is applied to HCl gas containing multiple gaseous fluorides. The catalyst contacts O2 and by-product HCl gas, and there is no need to separate and purify the HCl gas in the industry, thereby saving process costs. Compared with the existing copper-based catalyst, in an HCl atmosphere containing 1200ppm of fluorides, the conversion rate of HCl after the reaction temperature is 365°C and the reaction time is 720h is maintained at 99.4% of the conversion rate after the reaction time is 8h, thereby achieving high catalytic activity of the catalyst at a relatively low reaction temperature and in a fluorine-containing atmosphere. Meanwhile, during the application process, the catalyst will not be rapidly deactivated due to the presence of fluorides, so that the catalyst can still have high activity, stability and certain corrosion resistance in the presence of fluorides.
[0037] 2. The present invention adds rare earth metal salt and sodium tripolyphosphate to improve the catalytic activity of the catalyst. At the same time, since each P atom in the polyphosphate is connected to four O atoms through a covalent bond to form a stable tetrahedral structure, and a coordination bond is formed between the polyphosphate ion and the copper ion, the addition of sodium tripolyphosphate can improve the thermal stability of the copper-based catalyst.
[0038] 3. The preparation process of the catalyst of the present invention is simple and the reaction conditions are mild; compared with ruthenium-based catalysts, it uses non-precious metals such as copper and rare earth metals, which is low-cost and suitable for industrial production; compared with chromium-based catalysts, the catalyst does not contain toxic component elements such as chromium and will not cause secondary pollution to the environment; the main advantages and beneficial effects of the catalyst are resistance to corrosion by fluorine-containing gases, long service life, and good thermal stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is a SEM image of the catalyst for catalytic oxidation of fluorine-containing hydrogen chloride prepared in Example 1.
[0040] Figure 2 This is the thermogravimetric diagram of the catalyst of Example 6 after continuous evaluation for 1200 hours in an atmosphere of gaseous fluoride containing various impurities. DETAILED DESCRIPTION
[0041] The present invention will be further described below in conjunction with embodiments and drawings.
[0042] The raw materials and experimental equipment used in the examples and comparative examples are all commercially available raw materials and experimental equipment commonly used in the art, and their specific sources are not described in detail here.
[0043] The conversion rate of hydrogen chloride is calculated by iodine titration and acid-base titration. After the reaction is stable, samples are taken at intervals of 24 hours. Three parallel samples are taken each time, and the conversion rate of hydrogen chloride is averaged. The test principle is as follows:
[0044] Cl2+2KI=2KCl+I2;
[0045] I2+2Na2S2O3=2NaI+Na2S4O6;
[0046] HCl+NaOH=NaCl+H2O;
[0047] The reaction product is absorbed by excess KI solution, and the amount of iodine is titrated with Na2S2O3 solution to indirectly determine the amount of chlorine gas, and then the amount of HCl involved in the reaction is determined; the amount of unreacted HCl is titrated with NaOH solution, and the conversion rate of HCl is calculated.
[0048] The specific analysis process is as follows:
[0049] a) Titration of I2: Pass the mixed gas at the reactor outlet into 150ml KI solution, sampling time 2min, Cl2 and KI fully react to generate I2, titrate the generated iodine with 0.5mol / L Na2S2O3 standard solution until it turns light yellow, then add 1mL starch solution, and continue titrating until the blue color just disappears, i.e. reaching the titration endpoint. Record the volume of Na2S2O3 solution consumed, and then calculate the amount of HCl consumed;
[0050] b) Titration of hydrochloric acid in the sample: Add 2-3 drops of phenolphthalein reagent to the sample after the titration in step a), and titrate with a calibrated 0.2 mol / L NaOH standard solution until it becomes colorless, which is the titration end point. Record the volume of NaOH solution consumed in the titration and calculate the amount of HCl in the sample gas to be tested. The volume of Na2S2O3 solution consumed is recorded as V1, and the volume of NaOH solution consumed is recorded as V2. The calculation formula for HCl conversion rate is: HCl conversion rate = 0.5V1 / (0.5V1+0.2V2)×100%.
[0051] Example 1
[0052] A catalyst for preparing chlorine from hydrogen chloride is prepared by the following method:
[0053] 25.72g CuCl2·2H2O, 5.64g KCl, 13.52g SmCl3 and 0.75g Na5P3O 10 Dissolve in 115.0g water to obtain a mixed solution, then impregnate 150g of activated alumina carrier with the mixed solution and let it stand for 6h; filter out the excess impregnation solution after standing, collect the solid intermediate product and put it in an oven to dry at 120℃ for 10h, then place it in a muffle furnace and heat it to 250℃, keep it warm for 2h, and then calcine it at 550℃ for 8h to obtain the catalyst. Figure 1 As shown, the SEM results show that the catalyst prepared in Example 1 has flaky and granular structures of tens to hundreds of nanometers formed on its surface.
[0054] The above 20g catalyst was loaded into a fixed bed reactor with a size of 1100mmר26mm. After preheating to the reaction temperature, O2 and HCl (containing 1000ppm HF and 200ppm CHF3) were introduced in a molar ratio of 1:2 at a volume space velocity of 320h -1 The reaction temperature is 365°C, the reaction pressure is normal pressure, the conversion rate of HCl is 83.7% after 8 hours of reaction, the conversion rate of HCl is 83.5% after 480 hours of continuous reaction, and the conversion rate of HCl is 83.2% after 720 hours. The hot spot temperature is 380.1°C, and the catalyst has good stability.
[0055] Comparative Example 1
[0056] The difference from Example 1 is that no Na5P3O is added to the active component. 10 .
[0057] The copper-based catalyst was loaded into a reactor, and the reaction conditions were the same as those in Example 1. After 8 hours of reaction, the conversion rate of HCl was 82.8%. After 200 hours of continuous reaction, the conversion rate of HCl was 80.1%, and the hot spot temperature was 395.7°C.
[0058] Comparative Example 2
[0059] The difference from Example 1 is that the active component Na5P3O 10 The amount added was 4.8 g.
[0060] The above catalyst was loaded into a reactor, and after preheating and stabilization, the reaction conditions were the same as those in Example 1. After 8 hours of reaction, the conversion rate of HCl was 83.4%, and after 480 hours of continuous reaction, the conversion rate of HCl was 82.9%, and the hot spot temperature was 387.8°C.
[0061] Example 2
[0062] The difference from Example 1 is that the solvent is an equal mass of 20% acetic acid solution, and the other preparation components and methods are the same as those of Example 1. Under the reaction conditions of Example 1, the conversion rate of HCl is 84.1% after 8 hours of reaction, and the conversion rate of HCl is 84% after 480 hours of continuous reaction.
[0063] Comparative Example 3
[0064] The difference from Example 1 is that the reaction temperature is 350°C.
[0065] The above catalyst was loaded into a reactor, the reaction temperature was 350° C., and the other reaction conditions were the same as those in Example 1. After 8 h of reaction, the conversion rate of HCl was 70.5%.
[0066] Comparative Example 4
[0067] 30.864gCuCl2·2H2O, 6.768gKCl, 24.576gCeCl3·7H2O, and 14.87gSmCl3 were dissolved in 205.85g water to obtain a mixed solution, and 180g of an activated alumina carrier was soaked in the mixed solution and allowed to stand for 6 hours; the remaining preparation methods were the same as those in Example 1; under the reaction conditions of Example 1, the conversion rate of HCl was 83.2% after 8 hours of reaction, the hot spot temperature was 407.7°C, and the conversion rate of HCl was 74.9% after 240 hours of continuous reaction.
[0068] It can be seen from the results of Example 1 and Comparative Example 1 that adding Na5P3O 10 Salt can improve the conversion rate of HCl. It has little effect on the conversion rate of HCl in the initial stage of the reaction and does not significantly change the catalytic activity, but it can improve the thermal stability of the catalyst. The hot spot temperature drops by 15.6°C and the heat release of the reaction is reduced. The reason is that the negatively charged phosphate can form a stable coordination compound with the transition metal cation, reducing the loss of active components at high temperatures.
[0069] It can be seen from Example 1 and Comparative Example 2 that when Na5P3O 10 When the addition amount of Na5P3O was reduced, the conversion rate of HCl increased slightly, and the amount of floating powder after calcination was less, indicating that Na5P3O 10 The amount of addition is not the more the better. Adding an appropriate amount of Na5P3O 10 It can be loaded into the pores of the activated alumina carrier instead of the surface, reducing the loss caused by the components being loaded onto the surface.
[0070] It can be seen from Example 1 and Example 2 that, under the same other conditions, using a certain concentration of acetic acid instead of water as a solvent can make the metal salt more evenly dispersed, inhibit the hydrolysis of copper ions, improve the utilization of the active sites of the catalyst, effectively improve the conversion rate of HCl, the fluctuation of the conversion rate is small, and the corrosion resistance is good.
[0071] It can be seen from Example 1 and Comparative Example 3 that the reaction temperature will significantly affect the activity of the catalyst, and a certain reaction temperature needs to be reached for the catalyst to have a certain reaction activity.
[0072] According to the results of Example 1 and Comparative Example 4, from the perspective of catalytic efficiency, the synergistic effect of multiple rare earth metal salts can improve the catalytic activity of the catalyst, but the heat release is large, and the conversion rate decreases significantly after 240 hours of continuous reaction, which may be related to the loss of active components at high temperature, and the thermal stability is relatively poor.
[0073] Example 3
[0074] 38.58gCuCl2·2H2O, 10.14gKCl, 30.72gLaCl3·nH2O, 30.63gCeCl3·7H2O, 1.25gNa5P3O 10 The solid intermediate product was collected and placed in an oven to dry at 120°C for 10 hours, and then placed in a muffle furnace to calcine at 580°C for 6 hours to obtain the catalyst.
[0075] The above catalyst was loaded into the reactor, and O2 and HCl (containing 100 ppm HF and 100 ppm CHF3) were introduced in a molar ratio of 1:2 at a volume space velocity of 265 h -1 The reaction temperature was 375°C, the reaction pressure was normal pressure, and the conversion rate of HCl was 81.6% after 8 hours of reaction. The conversion rate of HCl was 79.8% after 720 hours of continuous reaction.
[0076] When comparing the examples horizontally, the selectivity of Example 3 is not as good as that of Example 1. The initial activity of the catalysts of Example 3 and Example 1 is not much different. The stability during long-term evaluation is slightly lower than that of Example 1 because different rare earth metal salts have different effects on the performance of the catalyst. As for the thermal stability of the catalyst, from the experimental results, the effect of samarium chloride is better than the synergistic effect of cerium and lanthanum.
[0077] Comparative Example 5
[0078] The difference from Example 3 is that Raschig ring carrier is used instead of activated alumina beads.
[0079] The above catalyst was loaded into a reactor, and the reaction conditions were the same as those in Example 3. After 8 hours of reaction, the conversion rate of HCl was 77.2%.
[0080] It can be seen from Example 3 and Comparative Example 5 that under the same reaction conditions, the use of different catalyst carriers has a greater impact on the catalytic activity. Carriers with different pore structures will affect the loading of active components and the gas adsorption and desorption process, thereby affecting the performance of the catalyst. The catalyst using Raschig rings as carriers has fragmentation after the reaction, and its strength and corrosion resistance are relatively poor.
[0081] Comparative Example 6
[0082] The difference from Example 3 is that the catalyst was calcined at 680°C for 12 hours. The reaction conditions were the same as those in Example 3, and the conversion rate of HCl was measured to be 74.4% after 8 hours of reaction.
[0083] It can be seen from Example 3 and Comparative Example 6 that the calcination temperature and calcination time of the catalyst have a certain influence on the activity of the catalyst. This is because the catalyst is more likely to sinter at high temperatures, and the active components are unevenly distributed, resulting in relatively low catalytic activity.
[0084] Comparative Example 7
[0085] The difference from Example 3 is that an equal amount of phosphorus trichloride is added instead of sodium tripolyphosphate. The significance of this comparative example is to add only phosphorus element but not provide a tetrahedral structure to bond with copper ions, thereby verifying the contribution of sodium tripolyphosphate to the stability of the catalyst.
[0086] The reaction conditions were the same as those in Example 3. After 8 h of reaction, the conversion rate of HCl was measured to be 60.3%.
[0087] It can be seen from Example 3 and Comparative Example 7 that compared with the addition of sodium tripolyphosphate, the activity of the catalyst prepared by adding non-polyphosphate is low. This is because each P atom in tripolyphosphate is connected to 4 O atoms by covalent bonds to form a stable tetrahedral structure, and at the same time, a coordination bond is formed between the polyphosphate ion and the copper ion. Therefore, the addition of sodium tripolyphosphate can improve the thermal stability of the copper-based catalyst.
[0088] Example 4
[0089] 22.70 g CuCl2·2H2O, 3.78 g KCl, 10.52 g SmCl3, 20.3 g CeCl3·7H2O and 0.55 g Na5P3O 10The mixture was dissolved in 122.0 g of water to obtain a mixed solution, and then the mixed solution was used to impregnate 120 g of an activated alumina carrier and allowed to stand for 6 hours; the excess impregnation solution after standing was filtered off, and then the impregnated carrier was placed in an oven and dried at 100°C for 10 hours; finally, the dried catalyst precursor was placed in a muffle furnace and heated to 250°C, kept warm for 2 hours, and then calcined at 580°C for 8 hours to obtain the catalyst.
[0090] The above 25g catalyst was loaded into the reactor. After preheating and stabilization, O2 and HCl (containing 1000ppm HF) were introduced in a molar ratio of 1:2 at a volume space velocity of 385h -1 The reaction temperature is 365°C, the reaction pressure is normal pressure, the conversion rate of HCl is 86.8% after 8 hours of reaction, the conversion rate of HCl is 86.4% after 480 hours of continuous reaction, and the conversion rate of HCl is 85.2% after 1500 hours. The catalyst has good stability.
[0091] Example 5
[0092] 25.2g CuCl2·2H2O, 4.64g KCl, 11.2g Sm(NO3)3 and 0.72g Na5P3O 10 The mixed solution was dissolved in 227.0 g of water, and then the mixed solution was impregnated into 90 g of an activated alumina carrier and allowed to stand for 6 h. The excess impregnation solution was filtered off, and the impregnated carrier was placed in an oven and dried at 90 ° C for 10 h. Finally, the dried catalyst precursor was placed in a muffle furnace and heated to 250 ° C, kept warm for 2 h, and then calcined at 650 ° C for 8 h to obtain the catalyst.
[0093] The catalyst was loaded into the reactor, and HCl gas containing various fluorides (1000ppmHF, 100ppmCHF3, 50ppmCHClF2) and O2 were introduced at a volume space velocity of 1080h -1 , the reaction temperature was 390°C, the reaction pressure was normal pressure, and the conversion rate of HCl was 80.7% after 8 hours of reaction; the conversion rate of HCl was 80.1% after 600 hours of continuous reaction.
[0094] Example 6
[0095] The catalyst prepared in Example 1 was loaded into a reactor, and HCl gas containing various fluorides (200 ppm HF, 300 ppm CHF3, 100 ppm CHClF2) and O2 were introduced at a volume space velocity of 320 h -1 , the reaction temperature was 375°C, the reaction pressure was normal pressure, and the conversion rate of HCl was 84.7% after 8 hours of reaction; the conversion rate of HCl was 84.4% after 1200 hours of continuous reaction. The catalyst did not deactivate and still had a high catalytic activity.
[0096] The catalyst of Example 6 was characterized by thermogravimetric analysis after continuous use for 1200 hours. The catalyst was tested in an oxygen atmosphere at a temperature of 20°C to 800°C. Figure 2 , Figure 2 In the figure, the thermogravimetric (TG) curve (i.e., the solid line) represents the weight change of the sample with temperature during the programmed temperature process, and the vertical axis is the weight percentage, which represents the ratio of the sample weight at the current temperature to the initial weight; the thermogravimetric differential curve (i.e., the dotted line) has a vertical coordinate that is a differential of each point on the TG curve relative to the time coordinate, which represents the change in weight change rate with temperature, and its peak point is the temperature point at which each weight changes fastest. It can be seen from the figure that the catalyst prepared by the present invention has a small weight loss after 1200h of continuous reaction, and the main weight loss step below 100°C has a weight loss of 6.9106%, which may be the volatilization of water adsorbed on the catalyst; 200°C-800°C is the volatilization of the active component, and the total weight loss is small; the residual mass is 84.703%, which is a catalyst that has not undergone thermal decomposition, which shows that the catalyst prepared by the present invention has no deactivation phenomenon after long-term continuous reaction even in an environment containing HF and chlorine, fluorine and carbon organic matter, and has good corrosion resistance and thermal stability.
Claims
1. A catalyst for preparing chlorine from hydrogen chloride, It is characterized in that comprising a carrier and an active component loaded on the carrier, The carrier is activated alumina, and the active components include copper salt, alkali metal salt, rare earth metal salt and polyphosphate. The polyphosphate in the polyphosphate forms a coordination bond with the copper ion in the copper salt. The copper salt is selected from copper chloride, copper nitrate or copper acetate; The alkali metal salt is selected from the chloride or nitrate of lithium, the chloride or nitrate of sodium or the chloride or nitrate of potassium; The rare earth metal salt is selected from at least one of nitrate or chloride of lanthanum, nitrate or chloride of cerium, or nitrate or chloride of samarium; The polyphosphate is sodium tripolyphosphate; The mass percentages of active ingredients and carriers are as follows: 8-20wt% of copper salt, 0.05-5wt% of alkali metal salt, 4-20wt% of rare earth metal salt, 0.05-2wt% of polyphosphate and 55-80wt% of activated alumina; The preparation method of the catalyst for preparing chlorine from hydrogen chloride comprises the following steps: S1. Dissolving a copper salt, an alkali metal salt, a rare earth metal salt and sodium tripolyphosphate in a solvent to obtain a mixed solution; S2. The carrier is added to the mixed solution obtained in step S1, and the solid intermediate product is collected by filtration after standing; S3. The solid intermediate product collected in step S2 is dried, kept at 250°C, calcined, and cooled to obtain a catalyst.
2. The catalyst for preparing chlorine from hydrogen chloride as claimed in claim 1, It is characterized in that The copper salt is copper chloride or copper nitrate; the alkali metal is sodium chloride or potassium chloride; The mass percentages of active ingredients and carriers are as follows: 8-17wt% of copper salt, 1-4wt% of alkali metal salt, 7-18wt% of rare earth metal salt, 0.2-1.5wt% of sodium tripolyphosphate, and 65-80wt% of carrier.
3. A method for preparing a catalyst for preparing chlorine from hydrogen chloride according to any one of claims 1 or 2, It is characterized in that The steps include: S1. Dissolving a copper salt, an alkali metal salt, a rare earth metal salt and sodium tripolyphosphate in a solvent to obtain a mixed solution; S2. The carrier is added to the mixed solution obtained in step S1, and the solid intermediate product is collected by filtration after standing; S3. The solid intermediate product collected in step S2 is dried, kept at 250°C, calcined, and cooled to obtain a catalyst.
4. The preparation method according to claim 3, It is characterized in that In step S1, the mass ratio of the solvent to the copper salt is (4-9):1; In step S1, the specific operation of the dissolving process in the solvent is as follows: after the copper salt, alkali metal salt, rare earth metal salt and polyphosphate are added into the solvent, they are stirred in a constant temperature water bath of 40° C. to 60° C. for 0.5 h to 2 h until the solute is completely dissolved; In step S1, water or acetic acid solution is selected as the solvent, and the concentration of the acetic acid solution is 5%-25%.
5. The preparation method according to claim 3, It is characterized in that In step S2, the mass ratio of the carrier to the mixed solution is 1:(1-3); In step S2, the standing time is 4h-8h.
6. The preparation method according to claim 3, It is characterized in that In step S3, the drying method is drying at 90°C-130°C for 3h-10h; In step S3, the calcination method is calcination at 550°C-650°C for 4h-10h.
7. Use of the catalyst for preparing chlorine from hydrogen chloride as claimed in any one of claims 1 to 2 or the catalyst for preparing chlorine from hydrogen chloride obtained by the preparation method as claimed in any one of claims 3 to 6 in catalyzing the preparation of chlorine from hydrogen chloride in a fluoride atmosphere.
8. The use according to claim 7, It is characterized in that The application method is as follows: The catalyst was loaded into the constant temperature zone of the fixed bed reactor. After the fixed bed temperature stabilized, O 2 and fluoride-containing HCl, which are preheated to the reaction temperature and reacted on the catalyst bed to produce Cl 2 .
9. The use according to claim 8, It is characterized in that The fluoride includes at least one of HF, hydrofluorocarbon and hydrochlorofluorocarbon; the concentration of HF is 100-1000 ppm; the concentration of hydrofluorocarbon is 100-300 ppm; the concentration of hydrochlorofluorocarbon is 50-200 ppm.
10. The use according to claim 8, It is characterized in that HCl and O 2 The molar ratio is 2:1; the reaction temperature is 360°C-410°C, and the reaction pressure is normal pressure; The volumetric space velocity of HCl is 240h -1 -1600h -1 .