Nitrogen-doped carbon modified high-entropy alloy catalyst as well as preparation method and application thereof
By modifying high-entropy alloy catalysts by nitrogen-doped carbon, the problems of narrow pH application range and low activity of single metal catalysts are solved, and efficient degradation of organic pollutants in water bodies within a wide pH range is achieved, and the characteristics of stability and reusability are achieved. .
Patent Information
- Application Number
- CN202411180785.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-27
AI Technical Summary
The existing single metal catalysts have problems such as narrow pH application range and low activity when catalyzed degradation of organic pollutants in water bodies, and high entropy alloys have not been studied in this field.
The high-entropy alloy catalyst is modified by nitrogen-doped carbon. By modifying the high-entropy alloy composed of metal elements such as Fe, Co, Ni, Cu, Mn and Zn, nanospherical particles are formed, and the catalytic activity is enhanced by hydrothermal method. and stability and recovery of catalyst through external magnetic field.
It has achieved high catalytic activity and good stability degradation of organic pollutants, has a wide pH range, can quickly degrade a variety of organic pollutants, and can be reused, and has environmentally friendly processes and low energy consumption.
Smart Images

Figure CN118976529A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of catalytic degradation of organic pollutants, for example, to a nitrogen-doped carbon-modified high-entropy alloy catalyst and a preparation method and application thereof. Background Art
[0002] The continuous accumulation of antibiotic residues in the environment, especially in freshwater ecosystems, poses a major threat to human health. In recent years, advanced oxidation technologies (AOPs) have been widely used to remove organic pollutants from water. Among them, molecular oxygen activation technology uses oxygen in the air as an oxidant to generate •OH and •O2 - Compared with other oxidants in advanced oxidation technologies, oxygen has the advantages of being green, clean, and widely available, and can avoid secondary pollution to the system caused by the addition of additional oxidants. The catalysts used to activate molecular oxygen mainly include two categories: precious metal catalysts and transition metal catalysts. Currently, single metal catalysts are widely studied due to their strong reducing properties, safety, simple operation, and low energy consumption, but their development and application are limited by their narrow pH range and low activity. Studies have shown that the introduction of other metal components to form multi-metal catalysts can improve these shortcomings.
[0003] The emerging high entropy alloys (HEAs) are alloys formed by five or more metal elements in equal or nearly equal proportions. They have tunable electronic structures and optimizable d-band centers, which provide the necessary conditions for them to become excellent catalysts. So far, no relevant research reports on the catalytic degradation of organic pollutants in water using high entropy alloys have been found. Summary of the invention
[0004] In order to provide a basic understanding of some aspects of the disclosed embodiments, a brief summary is given below. The summary is not an extensive review, nor is it intended to identify key / critical elements or delineate the scope of protection of these embodiments, but rather serves as a prelude to the detailed description that follows.
[0005] The embodiments of the present disclosure provide a nitrogen-doped carbon-modified high entropy alloy catalyst and a preparation method thereof. With a high entropy alloy as a matrix, effective catalytic degradation of organic matter in water is achieved through nitrogen-doped carbon modification, and the applicable range of water pH value is wide.
[0006] In some embodiments, the nitrogen-doped carbon-modified high entropy alloy catalyst, the high entropy alloy is a multi-component high entropy alloy including five or more of Fe, Co, Ni, Cu, Mn, Al and Zn, and the high entropy alloy includes at least Zn; the carbon component includes amorphous carbon and nanocrystalline graphitic carbon.
[0007] In some embodiments, the preparation method of the nitrogen-doped carbon modified high entropy alloy catalyst comprises: dissolving a plurality of metal salts of five or more metal elements selected from Fe, Co, Ni, Cu, Mn, Al and Zn in water in an amount equal to the molar ratio of metal atoms, stirring and dissolving to obtain solution A; wherein solution A comprises at least zinc salt; dissolving trimesic acid and an organic nitrogen source in an organic solvent to obtain solution B; the organic nitrogen source comprises melamine or polyvinyl pyrrolidone; mixing solution A with solution B, stirring and mixing to obtain a reaction liquid; placing the reaction liquid in a hydrothermal reactor, reacting at 120 to 180°C for a first preset time to obtain a reaction liquid; centrifuging the reaction liquid to obtain a precipitate, washing the precipitate and vacuum drying to obtain a multi-metal precursor; keeping the multi-metal precursor warm at a temperature of 600 to 900°C in an inert gas atmosphere for a second preset time, and then cooling to room temperature to obtain a nitrogen-doped carbon modified high entropy alloy catalyst.
[0008] The nitrogen-doped carbon-modified high-entropy alloy catalyst and the preparation method thereof provided in the embodiments of the present disclosure can achieve the following technical effects: The nitrogen-doped carbon-modified high-entropy alloy catalyst of the disclosed embodiment has high catalytic activity, good stability, and fast degradation speed; it has a wide range of pH value applications, and exhibits good degradation effects at pH values between 3 and 13; it has good universality and a wide range of applications, and can degrade a variety of organic pollutants. The catalyst is magnetic, and by applying an external magnetic field, the consumed catalyst can be easily recovered from the degradation reaction system, allowing for reuse without any substantial changes to its microstructure and performance.
[0009] The preparation method of the disclosed embodiment adopts the hydrothermal method to synthesize the high entropy alloy catalyst, which can form a uniform precursor solution and achieve effective mixing of elements at a relatively low temperature, thereby reducing energy consumption and the difficulty of synthesis. Moreover, the hydrothermal method conforms to the principles of green chemistry and reduces the harm to the environment by using environmentally friendly solvents (such as water and ethanol) and adjustable reaction conditions, making it more environmentally friendly.
[0010] The above general description and the following description are exemplary and explanatory only and are not intended to limit the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] One or more embodiments are exemplarily described by corresponding drawings, which do not limit the embodiments. Elements with the same reference numerals in the drawings are shown as similar elements, and the drawings do not constitute a scale limitation, and wherein: Figure 1 It is a flowchart of a method for preparing a nitrogen-doped carbon-modified high entropy alloy catalyst provided by an embodiment of the present disclosure; FIG. 2 (a) and FIG. 2 (b) are SEM images of a catalyst sample prepared in Example 1 provided in the embodiments of the present disclosure; Figure 3 is an X-ray diffraction pattern of various catalyst samples obtained in Example 1 of the presently disclosed embodiments; Figure 4 is an EDS spectrum of a catalyst sample prepared in Example 1 of the present disclosure; Figure 5 is a curve diagram of the removal effect of norfloxacin at different pH values of a catalyst sample obtained in Example 1 of the present disclosure; Figure 6 is a curve diagram of the removal effect of norfloxacin on various catalyst samples obtained in Example 1 of the disclosed embodiments at a pH value of 7; Figure 7 is a curve diagram of the removal effect of a catalyst sample obtained in Example 1 of the embodiments of the present disclosure on different organic pollutants; Figure 8 is a Raman spectrum of catalyst samples at different hydrothermal reaction temperatures of Examples 1 to 3 of the present disclosure; Fig. 9 It is a curve diagram of the removal effect of norfloxacin on various catalyst samples obtained in Examples 1 to 3 of the embodiments of the present disclosure at a pH value of 3; Fig.10 It is a curve diagram of the removal effect of norfloxacin on various catalyst samples obtained at different pyrolysis temperatures of Example 1, Example 4, Example 5 and Comparative Example 1 of the present disclosure at a pH value of 7; FIG. 11 (a) and FIG. 11 (b) are SEM images of a catalyst sample prepared in Example 6 provided in the embodiments of the present disclosure; Fig.12 is an X-ray diffraction pattern of various catalyst samples obtained in Example 6 of the presently disclosed embodiments; Fig.13 is a curve diagram of the removal effect of various catalyst samples obtained in Example 6 of the embodiments of the present disclosure on norfloxacin at a pH value of 3; Fig.14 is a curve diagram of the removal effect of norfloxacin on various catalyst samples obtained in Example 6 of the embodiments of the present disclosure at a pH value of 9; Fig.15 is a curve diagram of the removal effect of various catalyst samples obtained in Example 6 of the embodiments of the present disclosure on norfloxacin at a pH value of 11; Fig.16 are X-ray diffraction patterns of various catalyst samples obtained in Example 7 and Comparative Example 2 of the disclosed embodiments; Fig.17 is a curve diagram of the removal effect of norfloxacin at different pH values of a catalyst sample in Example 7 of the present disclosure; Fig.18 is a graph showing the nitrogen adsorption-desorption experimental characterization results of two catalyst samples obtained in Example 1 and Comparative Example 1 of the embodiments of the present disclosure; Fig.19 It is a curve diagram of the change rate of pore size-pore volume to pore volume of two catalyst samples obtained in Example 1 and Comparative Example 1 of the embodiments of the present disclosure. DETAILED DESCRIPTION
[0012] In order to be able to understand the features and technical contents of the embodiments of the present disclosure in more detail, the implementation of the embodiments of the present disclosure is described in detail below in conjunction with the accompanying drawings. The attached drawings are for reference only and are not used to limit the embodiments of the present disclosure. In the following technical description, for the convenience of explanation, a full understanding of the disclosed embodiments is provided through multiple details. However, one or more embodiments can still be implemented without these details. In other cases, to simplify the drawings, well-known structures and devices can be simplified for display.
[0013] Unless otherwise stated, the term "plurality" means two or more.
[0014] In the embodiment of the present disclosure, the character " / " indicates that the preceding and following objects are in an "or" relationship. For example, A / B indicates: A or B.
[0015] The term "and / or" is a description of the association relationship between objects, indicating that three relationships can exist. For example, A and / or B means: A or B, or, A and B.
[0016] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present disclosure may be combined with each other.
[0017] An embodiment of the present disclosure provides a nitrogen-doped carbon-modified high-entropy alloy catalyst, which includes nanoparticles, the high-entropy alloy is a multi-component high-entropy alloy including five or more of Fe, Co, Ni, Cu, Mn, Al and Zn, and the high-entropy alloy includes at least Zn; the carbon component includes amorphous carbon and nanocrystalline graphitic carbon.
[0018] In the nitrogen-doped carbon modified high entropy alloy catalyst of the embodiment of the present disclosure, the high entropy alloy is a five-element or higher high entropy alloy including Zn. The electrode potential (E 0 (Fe 2+ / Fe 0)=-0.44v) is low, has strong reducing power, and is an effective electron donor; cobalt can not only catalyze reactions through traditional hydroxyl radical pathways, but also directly degrade organic matter through non-radical pathways, providing multiple degradation pathways. Nickel has efficient catalytic performance in degrading organic pollutants. For example, the structure composed of fine grains of nickel-aluminum alloy can provide a large number of active sites, which is conducive to the catalytic reaction. In the catalytic process, copper can promote the generation of active oxygen species, which are essential for the degradation of organic pollutants. Manganese can have good chemical stability and thermal stability, and can maintain stable catalytic activity in a wide temperature and pH range. The addition of zinc can effectively increase the specific surface area of the material. By controlling the pyrolysis temperature not higher than the boiling point of zinc during high-temperature pyrolysis, the zinc is partially volatilized, leaving gaps, and increasing the contact area between the catalyst and the organic pollutants. At the same time, the carbon component is coated / loaded on the surface of the nitrogen-modified high-entropy alloy nanoparticles. The confinement effect of the carbon coating / loading reduces the leaching of metal ions, which can provide the stability of the high-entropy alloy catalyst. Nitrogen doping can improve the electronic structure of the carbon material, further enhance the electron transfer rate, and thus enhance the catalytic activity. The synergistic effect between the various metal components of the high-entropy alloy, and between the metal and carbon components, accelerates electron transfer, making the high-entropy alloy catalyst have high catalytic activity and fast degradation rate; moreover, the pH value application range of the high-entropy alloy catalyst is wide, and it shows good degradation effect at pH values between 3-13, which optimizes the problem of narrow pH value response range of traditional catalysts.
[0019] The nitrogen-doped carbon-modified high entropy alloy catalyst of the disclosed embodiment is magnetic, and by applying an external magnetic field, the consumed catalyst can be conveniently recovered from the degradation reaction system, allowing for reuse without any substantial changes to its microstructure and performance.
[0020] Optionally, the high entropy alloy is a quinary high entropy alloy including Fe, Co, Ni, Cu and Zn.
[0021] Optionally, the high entropy alloy is a hexavalent high entropy alloy including Fe, Co, Ni, Cu, Mn and Zn.
[0022] The nitrogen-doped carbon-modified high entropy alloy catalyst of the disclosed embodiment is in the form of black powder.
[0023] The nitrogen-doped carbon-modified high entropy alloy catalyst of the embodiment of the present disclosure includes nano-spherical particles, and the particle size of the nano-spherical particles is less than or equal to 500 nm.
[0024] Optionally, the particle size of the nano-spherical particles is less than or equal to 400 nm.
[0025] Optionally, the particle size of the nano-spherical particles is less than or equal to 300 nm.
[0026] Optionally, the particle size of the nano-spherical particles is less than or equal to 200 nm.
[0027] Combination Figure 1 As shown, the embodiment of the present disclosure provides a method for preparing a carbon skeleton modified nitrogen-doped high entropy alloy catalyst, comprising the following steps: S10. Dissolve multiple metal salts of five or more metal elements selected from Fe, Co, Ni, Cu, Mn, Al and Zn in water in an amount equal to the metal atomic molar ratio, stir and dissolve to obtain solution A; wherein solution A includes at least zinc salt.
[0028] S20, dissolving trimesic acid and an organic nitrogen source in an organic solvent to obtain a solution B; the organic nitrogen source comprises melamine or polyvinyl pyrrolidone.
[0029] S30, mixing solution A and solution B, stirring and mixing, to obtain a solution to be reacted.
[0030] S40, placing the reaction liquid in a hydrothermal reactor, reacting at 120-180° C. for a first preset time to obtain a reaction liquid; centrifuging the reaction liquid to obtain a precipitate, washing the precipitate and vacuum drying it to obtain a multi-metal precursor.
[0031] S50, keeping the multi-metal precursor at a temperature of 600-900° C. in an inert gas atmosphere for a second preset time, and then cooling it to room temperature to obtain a nitrogen-doped carbon-modified high entropy alloy catalyst.
[0032] The method for preparing a nitrogen-doped carbon-modified high entropy alloy catalyst of the disclosed embodiment uses trimesic acid (H3BTC) as an organic carbon source ligand and melamine (Mel) or polyvinyl pyrrolidone (PVP) as a nitrogen source to prepare a multi-metal precursor through a hydrothermal reaction, and then the multi-metal precursor is subjected to high-temperature pyrolysis to obtain a nitrogen-doped carbon-modified high entropy alloy catalyst.
[0033] The preparation method of the disclosed embodiment uses a hydrothermal method to synthesize a high entropy alloy, which can form a uniform precursor solution, and can achieve effective mixing of elements at a lower temperature, reducing energy consumption and the difficulty of synthesis. The hydrothermal method complies with the principle of green chemistry, and reduces the harm to the environment by using environmentally friendly solvents (such as water and ethanol) and adjustable reaction conditions; and it is carried out in a closed system, which reduces the emission of harmful gases and is more environmentally friendly. In addition, the hydrothermal reaction can obtain a high entropy alloy in the form of nano-spherical particles, and the size of the nano-spherical particles is controllable, and the particle size of the obtained high entropy alloy catalyst nanoparticles is controlled to be less than or equal to 500nm.
[0034] The preparation method of the embodiment of the present disclosure adds melamine as a nitrogen source during the hydrothermal synthesis process. After the nitrogen species are introduced into the carbon layer, the difference in electronegativity is used, and the nitrogen atom can greatly affect the charge distribution of the carbon material, so that vacancies or defective sites are generated in the carbon structure, accelerating electron transfer and improving its catalytic degradation performance. Melamine or polyvinyl pyrrolidone not only serves as a nitrogen source, but also provides a reducing atmosphere as a carbon source during high-temperature pyrolysis, so that the metal reduction in MOF is more sufficient. Trimellitic acid, as a polycarboxylic acid, has high chemical stability. Its abundant carboxyl groups can form stable complexes with metal ions, which provides a basis for the synthesis of metal organic frameworks (MOFs) with high chemical stability. At the same time, during the high-temperature carbonization process, the trimesic acid-based MOF can maintain its structural stability and form a carbon skeleton structure. MOFs prepared from trimesic acid can have a high specific surface area after carbonization, and this high specific surface area is conducive to increasing the number of active sites of the catalyst, thereby enhancing the catalytic efficiency.
[0035] In the preparation method of the disclosed embodiment, Zn is added to the high entropy alloy material. The boiling point of Zn is relatively low at about 900°C. During the high-temperature pyrolysis process, by controlling the pyrolysis temperature within the range of 600-900°C, a portion of Zn is volatilized, leaving pores, so that the material has a porous structure and forms nanoparticles with a high specific surface area. This increases the number of active sites on the catalyst surface, increases the contact area with organic pollutants, and improves the degradation rate and activity.
[0036] In step S10 of the preparation method of the embodiment of the present disclosure, the metal salts of the seven metals are soluble salts, so as to be soluble in water to form solution A. The specific metal salts are not limited and are determined according to actual conditions.
[0037] Optionally, the metal salt of Fe includes Fe(NO3)3•9H2O, Fe(CH3COO)3•4H2O or FeCl3•6H2O.
[0038] Alternatively, the metal salt of Co includes Co(NO3)2·6H2O, Co(CH3COO)2·4H2O or CoCl2·6H2O.
[0039] Optionally, the metal salt of Ni includes Ni(NO3)2·6H2O, Ni(CH3COO)2·4H2O or NiCl2·6H2O.
[0040] Optionally, the metal salt of Cu includes Cu(NO3)2·3H2O, Cu(CH3COO)2·H2O or CuCl2·2H2O.
[0041] Optionally, the metal salt of Zn includes Zn(NO3)2·6H2O, Zn(CH3COO)2·2H2O or ZnCl2·6H2O.
[0042] Alternatively, the metal salt of Mn includes Mn(NO3)2·6H2O, Mn(CH3COO)2·4H2O or MnCl2·4H2O.
[0043] Optionally, the metal salt of Al includes Al(NO3)3·9H2O, Al(CH3COO)3·2H2O or AlCl3·6H2O.
[0044] In some embodiments, in step S10, the ratio of the amount of the substance of one metal atom to water is controlled to be 1-2 mmol: 15-30 mL. In this embodiment, each metal atom is added in an equimolar ratio, that is, the ratio of the amount of the substance of each metal atom to water is the same and is within 1-2 mmol: 15-30 ml. That is, in solution A, the molar concentration of the metal atom of each metal salt is about 0.03-0.13 mol / L.
[0045] Optionally, in step S10, the ratio of the amount of the substance of one metal atom to water is controlled to be 1.5 mmol: 20 mL. That is, in solution A, the molar concentration of the metal atom of each metal salt is about 0.075 mol / L.
[0046] In step S10, the stirring and dissolving time is not limited, as long as each metal salt is dissolved and mixed evenly. For example, stirring is performed for 20 to 50 minutes.
[0047] In some embodiments, in step S20, the ratio of trimesic acid to the organic solvent is 4-8 mmol: 15-30 mL.
[0048] Optionally, in step S20, the ratio of trimesic acid to the organic solvent is 5-6 mmol:20 mL.
[0049] Optionally, in step S20, the ratio of trimesic acid to the organic solvent is 5.5 mmol:20 mL.
[0050] In some embodiments, in step S20, the ratio of the organic nitrogen source to the organic solvent is 0.2-1 g: 15-30 mL.
[0051] Optionally, in step S20, the ratio of the organic nitrogen source to the organic solvent is 0.3-0.9 g: 15-25 mL.
[0052] Optionally, in step S20, the ratio of the organic nitrogen source to the organic solvent is 0.5-0.8 g: 18-23 mL.
[0053] Optionally, in step S20, the ratio of the organic nitrogen source to the organic solvent is 0.6 g﹕20 mL.
[0054] In step S20 of the embodiment of the present disclosure, the organic solvent includes anhydrous ethanol, dimethylformamide (DMF) or ethylene glycol.
[0055] In step S20, during the process of dissolving trimesic acid and the organic nitrogen source in the organic solvent, stirring can be performed to accelerate dissolution. The stirring time is not limited, as long as the trimesic acid and the organic nitrogen source are completely dissolved. For example, stirring is performed for 20 to 50 minutes.
[0056] In some embodiments, in step S30, mixing solution A with solution B includes: adding solution A to solution B at a rate of 5 to 15 mL / s.
[0057] Optionally, in step S30, the rate at which solution A is added to solution B is 6 to 14 mL / s.
[0058] Optionally, in step S30, the rate at which solution A is added to solution B is 7 to 13 mL / s.
[0059] Optionally, in step S30, the rate of adding solution A to solution B is 8 to 12 mL / s.
[0060] Optionally, in step S30, the rate of adding solution A to solution B is 9-11 mL / s.
[0061] Optionally, in step S30, the rate of adding solution A into solution B is 10 mL / s.
[0062] In step S40, the reaction liquid is placed in a hydrothermal reaction kettle for hydrothermal reaction, and the hydrothermal reaction temperature is controlled within the range of 120 to 180° C. The hydrothermal reaction temperature is low and the energy consumption is low. Specifically, the hydrothermal reaction temperature can be any temperature within the range of 120 to 180° C., for example, 120° C., 130° C., 140° C., 150° C., 160° C., 170° C., and 180° C., and the like.
[0063] Optionally, the reaction liquid is placed in a hydrothermal reactor and reacted at 130-160° C. for a first preset time to obtain a reaction liquid.
[0064] Optionally, the reaction liquid is placed in a hydrothermal reactor and reacted at 150° C. for a first preset time to obtain a reaction liquid.
[0065] In some embodiments, in step S40, the first preset duration is 20 to 30 hours.
[0066] Optionally, in step S40, the first preset duration is 22 to 28 hours.
[0067] Optionally, in step S40, the first preset duration is 24 hours.
[0068] In step S40, during the process of washing the precipitate and then vacuum drying, the specific washing method is not limited, as long as the soluble impurities in the reaction solution can be removed. Optionally, washing includes: washing the precipitate with deionized water and the organic solvent in step S20 N times, respectively, and the value of N is not limited and is determined according to actual conditions. For example, N is any positive integer greater than 1, specifically, N is 2, 3, 4, 5 or 6.
[0069] In step S40, during the process of vacuum drying the precipitate after washing, the vacuum drying includes: drying in a vacuum environment at 50-100° C. The drying time is not limited and is determined according to actual conditions.
[0070] Optionally, in step S40, the vacuum drying time is 6 to 10 hours.
[0071] Optionally, in step S40, the vacuum drying time is 8 hours.
[0072] Optionally, in step S40, vacuum drying includes: drying in a vacuum environment at 50-80° C. for 6-10 hours.
[0073] Optionally, in step S40, vacuum drying includes: drying in a vacuum environment at 60° C. for 8 hours.
[0074] Optionally, in step S40, the vacuum drying process is performed using a vacuum drying oven, that is, the washed precipitate is placed in a vacuum drying oven for vacuum drying.
[0075] Step S50 of the disclosed embodiment is a step of obtaining a nitrogen-doped carbon-modified high entropy alloy catalyst by high-temperature pyrolysis of a multi-metal precursor, wherein the high-temperature pyrolysis temperature is controlled within a range of 600 to 900° C. The pyrolysis temperature can cause a portion of Zn to pyrolyze and volatilize, thereby forming catalyst nanoparticles with a high specific surface area. Optionally, the high-temperature pyrolysis temperature is 800° C.
[0076] Optionally, the hydrothermal reaction product is kept at 800° C. for a second preset time in an inert gas atmosphere.
[0077] In some embodiments, in step S50, the multi-metal precursor is kept at a temperature of 600-900° C. in an inert gas atmosphere for a second preset time, comprising: placing the multi-metal precursor in an inert gas atmosphere, heating the temperature to 600-900° C. at a rate of 3-8° C. / min and keeping the temperature for the second preset time. In this embodiment, by controlling the heating rate, it is possible to better ensure that all parts of the sample can reach the desired temperature uniformly.
[0078] Optionally, the temperature is raised to 600-900° C. at a rate of 4-6° C. / min and maintained for a second preset time.
[0079] Optionally, the temperature is raised to 600-900° C. at a rate of 5° C. / min and maintained for a second preset time.
[0080] In some embodiments, in step S50, the inert gas includes nitrogen or argon.
[0081] In some embodiments, in step S50, the second preset time length is 1 to 3 hours.
[0082] Optionally, in step S50, the second preset time length is 2 hours.
[0083] In some embodiments, in step S50, cooling to room temperature includes: cooling to room temperature at a rate of 3 to 8°C / min.
[0084] Optionally, in step S50, cooling to room temperature includes: cooling to room temperature at a rate of 4-6°C / min.
[0085] Optionally, in step S50, cooling to room temperature includes: cooling to room temperature at a rate of 5°C / min.
[0086] The embodiments of the present disclosure also provide the use of the nitrogen-doped carbon-modified high entropy alloy catalyst prepared by the aforementioned nitrogen-doped carbon-modified high entropy alloy catalyst or the aforementioned method for preparing the nitrogen-doped carbon-modified high entropy alloy catalyst in degrading organic pollutants in water bodies.
[0087] In the application of the disclosed embodiments, the nitrogen-doped carbon-modified high entropy alloy catalyst has good universality and a wide range of applications, and can degrade a variety of organic pollutants in water bodies. It can be applied to the degradation of organic pollutants in water bodies with a pH between 3 and 13, and the degradation rate can reach more than 80% within 40 minutes. At a pH of 7, it can degrade organic substances such as norfloxacin, rhodamine B, methyl orange, methylene blue and tetracycline hydrochloride, and can degrade more than 95% within 40 minutes.
[0088] Specific examples are provided below to more specifically illustrate the nitrogen-doped carbon-modified high entropy alloy catalyst and its preparation method and application according to the embodiments of the present disclosure.
[0089] Example 1 FeCoNiCuZn-based high entropy alloy catalyst A method for preparing a nitrogen-doped carbon-modified high entropy alloy catalyst comprises the following steps: S101. Dissolve Fe(NO3)3·9H2O, Co(NO3)2·6H2O, Ni(NO3)2·6H2O, Cu(NO3)2·3H2O and Zn(NO3)2·6H2O in deionized water in an equimolar ratio, and stir for 30 minutes to obtain solution A. The ratio of the amount of each metal salt to deionized water is 1.5 mmol: 20 mL.
[0090] S201, dissolving trimesic acid and an organic nitrogen source in anhydrous ethanol, stirring for 30 minutes, and obtaining solution B; the organic nitrogen source includes melamine (Mel), wherein the ratio of trimesic acid to anhydrous ethanol is 5.5mmol﹕20mL; the ratio of melamine (Mel) to anhydrous ethanol is 0.2-1g﹕20mL.
[0091] S301, adding solution A to solution B at a rate of 10 mL / s, stirring for 30 min, and mixing to obtain a reaction solution, wherein the volume ratio of solution A to solution B is 1:1.
[0092] S401, placing the reaction liquid in a hydrothermal reactor, reacting at 150° C. for 24 hours to obtain a reaction liquid; centrifuging the reaction liquid to obtain a precipitate, washing the precipitate and vacuum drying it at 60° C. for 8 hours to obtain a pentametal precursor.
[0093] S501. Put the multi-metal precursor into a porcelain boat and place it in a tubular furnace. Heat it to 800°C at a rate of 5°C / min in an argon inert gas atmosphere and keep it warm for 2 hours. Then cool it to room temperature to obtain a nitrogen-doped carbon-modified FeCoNiCuZn-based high entropy alloy catalyst.
[0094] The nitrogen-doped carbon-modified FeCoNiCuZn-based high-entropy alloy catalyst prepared in Example 1 is a black powder and includes nanoparticles. The nanoparticles are basically spherical, and the particle size of the spherical particles is in the range of 100nm to 200nm; the high-entropy alloy is a five-element high-entropy alloy including Fe, Co, Ni, Cu and Zn; and the carbon component includes amorphous carbon and nanocrystalline graphitic carbon.
[0095] In this Example 1, different catalyst samples are obtained by adjusting the amount of melamine in step S201. Specifically, the amounts of melamine are 0.3 g, 0.6 g and 0.9 g, respectively. The corresponding catalyst samples are recorded as HEAs@CN3-800, HEAs@CN6-800 and HEAs@CN9-800, respectively.
[0096] Meanwhile, in this embodiment 1, comparative experiment 1 was carried out, in which no melamine was added in step S201, that is, the amount of melamine was 0 g, and the remaining steps and parameters remained unchanged, and a catalyst comparative sample was obtained, which was recorded as HEAs@C-800.
[0097] As shown in the scanning electron microscope photos (SEM photos) of HEAs@CN6-800 in Figures 2 (a) and 2 (b), it can be seen that spherical particles are formed in the powdered catalyst and are uniform in size, with a particle size of approximately 100 nm to 200 nm.
[0098] like Figure 3 The X-ray diffraction patterns of HEAs@CN3-800, HEAs@CN6-800, HEAs@CN9-800, and HEAs@C-800 are shown in Fig. Figure 3 It can be observed that the four samples all have characteristic peaks at 43.3°, 50.4° and 74.1°, corresponding to the (111), (200) and (220) crystal planes, respectively (PDF#04-0836 is the XRD curve of the FCC structure high entropy alloy obtained from the standard card database in the XRD data analysis software (jade6)), indicating that the obtained samples all have a face-centered cubic (FCC) structure, which is consistent with the literature report. This also shows that the five-element metal precursor is successfully converted into a high-purity high-entropy alloy phase. It can be seen that with the addition of Mel, the intensity of the diffraction peak increases. This may be because Mel not only acts as a nitrogen source during the pyrolysis process, but also provides a reducing atmosphere, making the metal reduction more complete. The diffraction peak is the strongest when the Mel doping amount is 0.6g. As the doping amount continues to increase, the intensity of the diffraction peak weakens. This may be because the addition of excessive Mel will form more amorphous carbon on the sample surface.
[0099] Figure 4 This is the EDS spectrum of HEAs@CN6-800. It can be seen that the distribution of iron, cobalt, nickel, copper and zinc elements is relatively uniform. The presence of nitrogen and carbon elements indicates that nitrogen doping is successful. At the same time, the content of zinc is less than that of other metals, indicating that part of zinc volatilizes during the pyrolysis process.
[0100] In this Example 1, an application experiment 1-1 of the degradation of organic pollutants in water was carried out. As follows: a norfloxacin (NOR) solution with an initial concentration C0 of 20 ppm was used as the liquid to be degraded, and the pH of the liquid to be degraded was adjusted with 0.1 mol / L NaOH and 0.1 mol / L H2SO4 to obtain 6 kinds of liquids to be degraded with pH values of 3, 5, 7, 9, 11 and 13 respectively; the HEAs@CN6-800 catalyst sample in Example 1 was added to the 6 kinds of liquids to be degraded respectively, stirred, and the timing was started when the addition was made; wherein, the dosage of the HEAs@CN6-800 catalyst sample was 1 g / L. During the degradation process, 3 mL of the degradation liquid was removed at regular intervals and the catalyst was filtered out with a 0.22 μm filter membrane, placed in a 1 cm quartz cuvette, and the absorbance was detected with a UV-visible spectrophotometer to determine the concentration C of norfloxacin. t . Get Figure 5 The removal effect curve of norfloxacin at different pH values is shown.
[0101] pass Figure 5It can be seen that the degradation effect is excellent in the pH range of 3 to 11, and the removal rate of norfloxacin is more than 95% within 40 minutes. Under acidic conditions, the degradation rate is 96.22% at pH 3 and 98.30% at pH 5; under alkaline conditions, the degradation rate is 97.15% at pH 9, 98.12% at pH 11, and 74.04% at pH 13; at pH 7, all norfloxacin can be removed. At pH 13, due to the strong alkalinity, hydroxylation may occur on the catalyst surface, resulting in the occupation of surface active sites, thereby reducing the contact between the catalyst and the active sites and slowing down the degradation rate.
[0102] Similarly, HEAs@CN3-800 and HEAs@CN9-800, as well as HEAs@C-800 of comparative experiment 1, were subjected to degradation application experiments according to the above-mentioned degradation application experiment 1-1, wherein pH value 7 was selected to obtain the following Figure 6 The removal effect curve of norfloxacin by different catalysts at pH 7 is shown. Figure 6 It can be seen that when the Mel doping amount is 0, the removal rate of the catalyst for norfloxacin is 86.10%. After adding an appropriate amount of Mel, it can be clearly observed that the degradation performance of norfloxacin is improved. When the Mel addition amount is 0.3g, the removal rate of norfloxacin reaches 95.5%, which shows that the doping of Mel can effectively improve the catalytic activity of the catalyst. When the Mel addition amount is 0.6g, the degradation effect is the best, and all NOR can be removed within 40min. When the Mel doping amount is further increased to 0.9g, the removal rate is 97.6%.
[0103] In this Example 1, the degradation application experiment 1-2 of organic pollutants in water was also carried out. As follows: a variety of common organic pollutants in the environment were selected for experiments, including organic dyes rhodamine B (RhB), methyl orange (MO), methylene blue (MB) and antibiotics metronidazole (MNZ), norfloxacin (NOR) and tetracycline hydrochloride (TCH). The above 6 different organic pollutants were prepared with an initial concentration C0 of 20ppm, and the pH value of each degraded liquid was adjusted to 7 using 1mol / L NaOH and 1mol / L H2SO4; then, the HEAs@CN6-800 catalyst sample in Example 1 was added to each degraded liquid, stirred, and the timing was started when it was added; wherein, the addition amount of the HEAs@CN6-800 catalyst sample was 1g / L. During the degradation process, 3 mL of the degradation solution was taken out at regular intervals and filtered with a 0.22 μm filter membrane to remove the catalyst. The solution was placed in a 1 cm quartz cuvette and the absorbance was measured with a UV-visible spectrophotometer to determine the concentration of organic pollutants contained in each solution. t . Get Figure 7 The removal effect curve of different organic pollutants is shown.
[0104] pass Figure 7 It can be seen that for dye pollutants, the degradation rates of methylene blue (MB) and methyl orange (MO) are relatively fast, and they can be completely removed within 20 minutes after the catalyst is added. Rhodamine B (RhB) can also be degraded by 97.11% within 40 minutes; for antibiotic pollutants, tetracycline hydrochloride (TCH) and norfloxacin (NOR) can be completely removed within 40 minutes, and the degradation performance of metronidazole (MNZ) is relatively poor, and 65.04% can be removed in 40 minutes, which may be attributed to the high stability given to it by the nitro and imidazole rings in the metronidazole molecule. It can be observed that the catalyst has good universality, and can almost completely remove most organic pollutants in a short time, with excellent degradation performance. This strongly proves that the HEAs@CN6-800 catalyst is suitable for wastewater environments containing a variety of organic pollutants, and can adapt to the complex components in various industrial wastewaters in practical applications, providing an efficient solution for wastewater treatment.
[0105] Example 2 The difference from Example 1 is that in step S201, the ratio of melamine (Mel) to anhydrous ethanol is 0.6 g: 20 mL; in step S401, the reaction liquid is placed in a hydrothermal reactor and reacted at 120° C. for 24 hours to obtain a reaction liquid. The remaining steps and parameters are the same as in Example 1.
[0106] The nitrogen-doped carbon-modified FeCoNiCuZn-based high entropy alloy catalyst prepared in Example 2 is denoted as HEAs@CN6-800'.
[0107] Example 3 The difference from Example 1 is that in step S201, the ratio of melamine (Mel) to anhydrous ethanol is 0.6 g: 20 mL; in step S401, the reaction liquid is placed in a hydrothermal reactor and reacted at 180° C. for 24 hours to obtain a reaction liquid. The remaining steps and parameters are the same as in Example 1.
[0108] The nitrogen-doped carbon-modified FeCoNiCuZn-based high entropy alloy catalyst prepared in Example 3 is denoted as HEAs@CN6-800".
[0109] In Examples 1 to 3, catalyst samples (HEAs@CN6-800, HEAs@CN6-800' and HEAs@CN6-800") with hydrothermal reaction temperatures of 120°C, 150°C and 180°C were obtained, and Raman spectroscopy was performed on the three catalyst samples to obtain the following results: Figure 8The Raman spectra of the catalysts at different hydrothermal reaction temperatures are shown in Figure 2. Figure 8 As shown, the three catalyst samples all have -1 and 1850cm -1 Two peaks appeared near the D peak and the G peak. The D peak represents the lattice defects and disorder in the carbon material, which is usually related to the sp 3 The G peak represents the sp 2 In-plane stretching vibration of hybridized carbon atoms. Usually the ratio of the D peak to the G peak intensity (I D / I G ) is an important indicator to measure the degree of graphitization of carbon components. It is generally believed that I D / I G The smaller the graphitization degree is, the higher the graphitization degree is. However, unlike crystalline carbon materials, in amorphous carbon, the higher I D / I G The ratio indicates that there are more amorphous structures and defects in the sample. This is because the production of nanocrystalline graphite will enhance the intensity of the D peak by reducing the bond torsion and bond angle of disordered carbon atoms and tightening the corresponding state vibration density. Therefore, I D / I G The larger the value, the higher the degree of graphitization. Combined with XRD, it can be seen that the carbon component in HEAs@CN-800 is amorphous carbon. When the hydrothermal temperature increases from 120℃ to 180℃, I D / I G The ratio of increases from 0.96 to 1.02, so increasing the hydrothermal temperature is conducive to the formation of nanocrystalline graphite and the degree of graphitization in the catalyst is improved. Fig. 9 It can be seen from the degradation effect curve graph and Table 1 that the graphitization degree of the catalyst of the embodiment of the present disclosure is closely related to the electron transfer rate of the catalyst. The higher the graphitization degree, the higher the electron mobility, thereby improving the catalytic performance of the catalyst.
[0110] Degradation application experiments 1-3 were carried out on the catalyst samples HEAs@CN6-800, HEAs@CN6-800' and HEAs@CN6-800" obtained in Examples 1 to 3, as well as the comparative catalyst sample HEAs@C-800. As follows: the liquid to be degraded is a norfloxacin (NOR) solution with an initial concentration of 20 ppm and a pH value of 3 (the pH value adjustment method can refer to the aforementioned degradation application experiment 1-1, which will not be repeated here). The liquid to be degraded was prepared in 4 parallel portions, and HEAs@CN6-800, HEAs@CN6-800', HEAs@CN6-800" and HEAs@C-800 were added respectively, and the dosage of each catalyst sample was 1 g / L. During the degradation process, 3 mL of the degradation liquid was removed at regular intervals and the catalyst was filtered out with a 0.22 μm filter membrane, placed in a 1 cm quartz cuvette, and the absorbance was detected with a UV-visible spectrophotometer to determine the concentration C of norfloxacin. The following is obtained: Fig. 9 The removal effect curve of norfloxacin by the catalyst obtained at different hydrothermal reaction temperatures when the pH value is 3 is shown. Fig. 9 It can be seen that under the acidic condition of pH 3 in water, after 40 minutes, the degradation rate of the catalyst (HEAs@CN6-800') obtained at 120℃ was 87.42%; the degradation rate of the catalyst (HEAs@CN6-800) obtained at 150℃ was 96.22%; the degradation rate of the catalyst (HEAs@CN6-800") obtained at 180℃ was 84.45%; all of them had good degradation rates. The degradation rate of HEAs@C-800 without nitrogen doping was 81.87%.
[0111] Similarly, HEAs@CN6-800, HEAs@CN6-800', HEAs@CN6-800" and HEAs@C-800 were subjected to degradation experiments using the above-mentioned degradation application experiments 1-3 for degradation solutions with pH values of 7, 9 and 11, respectively (norfloxacin solution with an initial concentration of 20 ppm), and the degradation rates at 40 min were obtained (as shown in Table 1), and the degradation trends of the catalyst samples at different pH values were consistent.
[0112] Table 1
[0113] Example 4 The difference from Example 1 is that in step S201, the ratio of melamine (Mel) to anhydrous ethanol is 0.6 g:20 mL; in step S501, the temperature is raised to 600° C. (ie, the pyrolysis temperature is 600° C.); the remaining steps and parameters are the same as in Example 1.
[0114] The nitrogen-doped carbon-modified FeCoNiCuZn-based high entropy alloy catalyst prepared in Example 4 is denoted as HEAs@CN6-600.
[0115] Example 5 Different from Example 1, in step S201, the ratio of melamine (Mel) to anhydrous ethanol is 0.6 g:20 mL; in step S501, the temperature is raised to 900° C. (ie, the pyrolysis temperature is 900° C.); the remaining steps and parameters are the same as in Example 1.
[0116] The nitrogen-doped carbon-modified FeCoNiCuZn-based high entropy alloy catalyst prepared in Example 5 is denoted as HEAs@CN6-900.
[0117] Comparative Example 1 FeCoNiCu-based high entropy alloy catalyst The difference between this comparative example 1 and the embodiment 1 is that in step S101, Fe(NO3)3·9H2O, Co(NO3)2·6 H2O, Ni(NO3)2·6 H2O and Cu(NO3)2·3 H2O are dissolved in deionized water in an equimolar ratio, stirred and dissolved for 30 minutes to obtain solution A. The ratio of the amount of each metal salt to deionized water is 1.5mmol﹕20mL. In step S201, the ratio of melamine (Mel) to anhydrous ethanol is 0.6g﹕20mL; then, the quaternary metal precursor is obtained in step S401. The other steps and parameters are the same as those in embodiment 1.
[0118] The catalyst obtained in Comparative Example 1 is a carbon-nitrogen modified and doped FeCoNiCu-based high entropy alloy catalyst without Zn element, which is recorded as FeCoNiCu@CN6-800.
[0119] Degradation application experiments 1-4 were carried out on the four catalyst samples obtained in Example 1, Example 4, Example 5 and Comparative Example 1. The liquid to be degraded is a norfloxacin (NOR) solution with an initial concentration of 20 ppm and a pH value of 7 (the pH value adjustment method can refer to the aforementioned degradation application experiment 1-1, which will not be repeated here). Four parallel portions of the liquid to be degraded were prepared, and HEAs@CN6-600, HEAs@CN6-800, HEAs@CN6-900 and FeCoNiCu@CN6-800 were added respectively, and the dosage of each catalyst sample was 1 g / L. For the rest of the operations, refer to the aforementioned degradation application experiment 1-3. Fig.10 The removal effect curve of norfloxacin by the catalysts obtained at different pyrolysis temperatures when the pH value is 7 is shown. Fig.10As shown in the figure, after 40 minutes of degradation, the degradation rate of the catalyst obtained at 600℃ pyrolysis temperature is 82.5%, the degradation rate of the catalyst obtained at 800℃ pyrolysis temperature is 100%, and the degradation rate of the catalyst obtained at 900℃ pyrolysis temperature is 89.7%. The degradation rate of the comparative catalyst obtained at 800℃ without adding Zn is 78.3%. It can be seen that the introduction of Zn element and controlling the pyrolysis temperature in the range of 600℃~800℃ can significantly improve the degradation rate.
[0120] In the above-mentioned Examples 1 to 5, “HEAs” stands for “FeCoNiCuZn”.
[0121] Example 6 A method for preparing a nitrogen-doped carbon-modified high entropy alloy catalyst comprises the following steps: S102. Dissolve Fe(NO3)3·9H2O, Co(NO3)2·6H2O, Ni(NO3)2·6H2O, Cu(NO3)2·3H2O and Zn(NO3)2·6H2O in deionized water in an equimolar ratio, and stir for 30 minutes to obtain solution A. The ratio of the amount of each metal salt to deionized water is 1.5mmol:20mL.
[0122] S202, dissolving trimesic acid and an organic nitrogen source in anhydrous ethanol, stirring for 30 minutes, and obtaining solution B; the organic nitrogen source includes polyvinyl pyrrolidone (PVP), wherein the ratio of trimesic acid to anhydrous ethanol is 5.5mmol﹕20mL; the ratio of polyvinyl pyrrolidone (PVP) to anhydrous ethanol is 0.2-1g﹕20mL.
[0123] S302, adding solution A to solution B at a rate of 10 mL / s, stirring for 30 min, and mixing to obtain a reaction solution, wherein the volume ratio of solution A to solution B is 1:1.
[0124] S402, placing the reaction liquid in a hydrothermal reactor, reacting at 120°C to 180°C for 24 hours to obtain a reaction liquid; centrifuging the reaction liquid to obtain a precipitate, washing the precipitate and vacuum drying it at 60°C for 8 hours to obtain a pentametal precursor.
[0125] S502, placing the multi-metal precursor into a porcelain boat and placing it in a tubular furnace, heating it to 800°C at a rate of 5°C / min in an argon inert gas atmosphere and keeping it warm for 2 hours, then cooling it to room temperature to obtain a nitrogen-doped carbon-modified FeCoNiCuZn-based high entropy alloy catalyst.
[0126] In this Example 6, polyvinyl pyrrolidone (PVP) is used as a nitrogen source to prepare a nitrogen-doped carbon-modified FeCoNiCuZn-based high entropy alloy catalyst, which is a black powder and includes nanoparticles. The nanoparticles are basically spherical, and the particle size of the spherical particles is in the range of 100nm to 200nm; the high entropy alloy is a five-element high entropy alloy including Fe, Co, Ni, Cu and Zn; and the carbon component includes amorphous carbon and nanocrystalline graphite.
[0127] In this Example 6, different catalyst samples are obtained by adjusting the hydrothermal reaction temperature in step S402. Specifically, when the ratio of PVP to anhydrous ethanol in step S202 is 0.6 g:20 mL, and the hydrothermal reaction temperatures are 120°C, 150°C and 180°C, respectively, catalyst samples are obtained, which are respectively recorded as catalyst sample I, catalyst sample II and catalyst sample III.
[0128] In this Example 6, a comparative experiment 2 was conducted, in which no polyvinyl pyrrolidone (PVP) was added in step S202, that is, the amount of polyvinyl pyrrolidone was 0 g, and the hydrothermal reaction temperature in step S402 was 150° C., correspondingly obtaining catalyst sample comparison II.
[0129] As shown in the scanning electron microscope photos (SEM photos) of catalyst sample II in Figures 11 (a) and 11 (b), it can be seen that the catalyst includes a large number of spherical particles with a particle size within 400nm, and most of the particle sizes are distributed between 100nm and 200nm; and it can be seen that the morphology is consistent with that of the catalyst obtained by using melamine as the nitrogen source.
[0130] like Fig.12 The X-ray diffraction patterns of catalyst sample Ⅰ, catalyst sample Ⅱ and catalyst sample Ⅲ shown in FIG. Fig.12 It can be seen that the three catalyst samples all have characteristic peaks at 43.3°, 50.4° and 74.1°, corresponding to the (111), (200) and (220) crystal planes, respectively, indicating that the obtained catalyst samples all have a face-centered cubic (FCC) structure. This also shows that the five-element metal precursor is successfully converted into a high-purity high-entropy alloy phase. At the same time, it was found that the diffraction peak of the sample was the strongest at 150°C, indicating that the crystallinity is best at this temperature and the appropriate temperature is conducive to the growth of crystals.
[0131] In this Example 6, the degradation application experiment 2-1 of organic pollutants in water was carried out. The liquid to be degraded is a norfloxacin (NOR) solution with an initial concentration of 20 ppm and a pH value of 3 (the pH value adjustment method can refer to the aforementioned degradation application experiment 1-1, which will not be repeated here). The liquid to be degraded is prepared in 4 parallel portions, and catalyst sample I, catalyst sample II, catalyst sample III and catalyst sample comparison II are added respectively, and the addition amount of each catalyst sample is 1g / L. The rest of the operations refer to the aforementioned degradation application experiment 1-3. Obtain the following Fig.13 The removal effect curve of norfloxacin by the catalysts obtained at different hydrothermal reaction temperatures at a pH value of 3 is shown in FIG. Fig.13 It can be seen that under the acidic condition of pH 3 in water, after 30 minutes, the degradation rate of catalyst sample I obtained at 120°C was 87.38%; the degradation rate of catalyst sample II obtained at 150°C was 95.11%; the degradation rate of catalyst sample III obtained at 180°C was 98.12%; all of them have good degradation rates. The degradation rate of catalyst sample II is 77.70%, which shows that nitrogen doping can significantly improve the degradation performance of the catalyst.
[0132] Similarly, for catalyst sample I, catalyst sample II, catalyst sample III and catalyst sample comparison II, degradation experiments were carried out using the above-mentioned degradation application experiment 2-1 for degradation solutions with pH values of 9 and 11 (norfloxacin solution with an initial concentration of 20 ppm), and the corresponding Fig.14 and Fig.15 , Fig.14 The removal effect curve of norfloxacin on the catalyst obtained at different hydrothermal reaction temperatures with a pH value of 9 is shown in FIG. Fig.15 The figure is a curve diagram of the removal effect of norfloxacin by the catalysts obtained at different hydrothermal reaction temperatures at a pH value of 11. The corresponding degradation rate data are shown in Table 2.
[0133] Table 2
[0134] It can be seen that the nitrogen-doped carbon-modified FeCoNiCuZn-based high entropy alloy catalyst obtained in Example 6 has a good degradation rate for organic pollutants in water.
[0135] Example 7 A method for preparing a carbon skeleton modified nitrogen-doped high entropy alloy catalyst comprises the following steps: S103, Fe(NO3)3·9H2O, Co(NO3)2·6H2O, Ni(NO3)2·6H2O, Cu(NO3)2·3H2O, Mn(NO3)2·6H2O and Zn(NO3)2·6H2O were dissolved in deionized water in an equimolar ratio, stirred and dissolved for 30 minutes to obtain solution A. The ratio of the amount of each metal salt to deionized water was 1.5mmol:20mL.
[0136] S203, dissolving trimesic acid and an organic nitrogen source in anhydrous ethanol, stirring for 30 minutes, and obtaining solution B; the organic nitrogen source includes melamine (Mel), wherein the ratio of trimesic acid to anhydrous ethanol is 5.5mmol﹕20mL; the ratio of melamine (Mel) to anhydrous ethanol is 0.2-1g﹕20mL.
[0137] S303, adding solution A to solution B at a rate of 10 mL / s, stirring for 30 min, and mixing to obtain a reaction solution, wherein the volume ratio of solution A to solution B is 1:1.
[0138] S403, placing the reaction liquid in a hydrothermal reactor, reacting at 120°C to 180°C for 24 hours to obtain a reaction liquid; centrifuging the reaction liquid to obtain a precipitate, washing the precipitate and vacuum drying it at 60°C for 8 hours to obtain a hexametal precursor.
[0139] S503, placing the multi-metal precursor into a porcelain boat and placing it in a tubular furnace, heating it to 800°C at a rate of 5°C / min in an argon inert gas atmosphere and keeping it warm for 2 hours, then cooling it to room temperature to obtain a nitrogen-doped carbon-modified FeCoNiCuMnZn-based high entropy alloy catalyst.
[0140] In this Example 7, melamine (Mel) is used as a nitrogen source to prepare a nitrogen-doped carbon-modified FeCoNiCuMnZn-based high-entropy alloy catalyst, which is a black powder and includes nanoparticles. The nanoparticles are basically spherical, and the particle size is mainly distributed in the range of 100nm to 200nm; the high-entropy alloy is a hexameric high-entropy alloy including Fe, Co, Ni, Cu, Mn and Zn; and the carbon component includes amorphous carbon and nanocrystalline graphitic carbon.
[0141] In this Example 7, specifically, the ratio of Mel to anhydrous ethanol in step S203 is 0.6 g﹕20 mL, and the hydrothermal reaction temperature in step S403 is 150° C., thereby preparing catalyst sample V (FeCoNiCuMnZn@CN6-800).
[0142] Meanwhile, in this Example 7, a comparative experiment 3 was conducted, in which no melamine was added in step S203, that is, the amount of melamine was 0 g, and the remaining steps and parameters remained unchanged, and a catalyst comparative sample V (FeCoNiCuMnZn@C-800) was obtained accordingly.
[0143] Comparative Example 2 FeCoNiCuMn-based high entropy alloy catalyst The difference between this comparative example 2 and example 7 is that in step S103, Fe(NO3)3·9H2O, Co(NO3)2·6 H2O, Ni(NO3)2·6 H2O, Cu(NO3)2·3 H2O and Mn(NO3)2·6 H2O are dissolved in deionized water in an equimolar ratio, stirred and dissolved for 30 minutes to obtain solution A. The ratio of the amount of each metal salt to deionized water is 1.5mmol﹕20mL. Then, what is obtained in step S401 is a five-element metal precursor. The other steps and parameters are the same as those in example 7.
[0144] Comparative Example 2 obtained a carbon-nitrogen modified and doped FeCoNiCuMn-based high entropy alloy catalyst (denoted as FeCoNiCuMn@CN6-800) without the Zn element.
[0145] like Fig.16 The X-ray diffraction patterns of the catalyst sample V, the catalyst comparison sample V and the FeCoNiCuMn@CN6-800 of the comparative example 2 are shown in FIG. Fig.16 It can be observed that all three have generated the high entropy alloy phase of FCC. After adding the nitrogen source (Mel), the diffraction peak of FeCoNiCuMnZn@CN6-800 is stronger, indicating better crystallinity, because the nitrogen source will provide a reducing atmosphere during the pyrolysis process, making the metal reduction more complete.
[0146] In this Example 7, the degradation application experiment 3-1 of organic pollutants in water was carried out. A norfloxacin (NOR) solution with an initial concentration C0 of 20 ppm was prepared as the liquid to be degraded, and its pH value was adjusted in the manner of the degradation application experiment 1-1 to obtain four kinds of liquids to be degraded with pH values of 3, 7, 9 and 11 respectively; the catalyst sample V in Example 7 was added to the four kinds of liquids to be degraded respectively, and the dosage of the catalyst sample V was 1 g / L. During the degradation process, 3 mL of the degradation liquid was removed at regular intervals and the catalyst was filtered out with a 0.22 μm filter membrane, placed in a 1 cm quartz cuvette, and the absorbance was detected with a UV-visible spectrophotometer to determine the concentration C of norfloxacin. t . Get Fig.17 The removal effect curve of catalyst sample V on norfloxacin at different pH values is shown.
[0147] Depend on Fig.17As shown in the figure, catalyst sample V can be almost completely degraded within 40 min, with a degradation rate of 98.9% at pH 3, 99.1% at pH 7, 97% at pH 9, and 95.82% at pH 11. It has a good degradation effect in a wide pH range.
[0148] Similarly, for FeCoNiCuMn@CN6-800 in Comparative Example 2, the degradation application experiment 3-1 was adopted to select the degradation liquid with pH values of 3, 9 and 11 for degradation experiment, and the degradation rate at 40 min was obtained, as shown in Table 3. Its degradation trend is consistent with that of catalyst sample V.
[0149] Table 3
[0150] It can be seen that the degradation rate of FeCoNiCuMn@CN6-800 without the introduction of Zn element at each pH value is significantly reduced.
[0151] In the examples disclosed herein, the HEAs@CN6-800 catalyst in Example 1 (abbreviated as FeCoNiCuZn@CN) and the FeCoNiCu-based high entropy alloy catalyst in Comparative Example 1 (abbreviated as FeCoNiCu@CN) were subjected to nitrogen adsorption-desorption experiments, and the pore characteristics and specific surface area of the catalysts with and without the addition of metal Zn were characterized by the nitrogen adsorption-desorption experiments, and the effect of the addition of Zn on the specific surface area and pore size of the catalyst was explored. The results are as follows: Fig.18 As shown, it can be seen that the N2 adsorption-desorption isotherm of FeCoNiCuZn@CN6-800 has an obvious H3 type hysteresis loop in the relative pressure range of 0.45~1.0, showing a typical IV type adsorption isotherm, indicating that mesopores exist in the FeCoNiCuZn@CN6-800 catalyst. On the other hand, the FeCoNiCu@CN6-800 catalyst has a similar hysteresis loop shape, but the adsorption-desorption isotherm is significantly lower than that of the FeCoNiCuZn@CN6-800 catalyst, indicating that a part of the metal Zn is evaporated and leaves gaps as a sacrificial template during the pyrolysis process, which improves the pore structure of the catalyst. In addition, combined with the average pore size distribution diagram ( Fig.19 ) and the Brunauer-Emmet-Teller formula in Table 4, the addition of metallic Zn significantly increased the specific surface area and pore volume of the catalyst, while the pore size was reduced, which indicates that part of the Zn as a sacrificial template is of great significance to improving the performance of the catalyst.
[0152] Table 4
[0153] The present application is not limited to the structures that have been described above and shown in the drawings, and various modifications and changes may be made without departing from the scope thereof. The scope of the present application is limited only by the appended claims.
[0154] In the present application, each embodiment may focus on the differences from other embodiments, and the same or similar parts between the embodiments may refer to each other.
Claims
1. A nitrogen-doped carbon-modified high entropy alloy catalyst, characterized in that: The high entropy alloy is a multi-component high entropy alloy including five or more of Fe, Co, Ni, Cu, Mn, Al and Zn, and the high entropy alloy includes at least Zn; the carbon component includes amorphous carbon and nanocrystalline graphite carbon.
2. The nitrogen-doped carbon-modified high entropy alloy catalyst according to claim 1, characterized in that: The nano-spherical particles are included, and the particle size of the nano-spherical particles is less than or equal to 500nm.
3. The nitrogen-doped carbon-modified high entropy alloy catalyst according to claim 1, characterized in that: The high entropy alloy is a quinary high entropy alloy comprising Fe, Co, Ni, Cu and Zn; or, The high entropy alloy is a hexameric high entropy alloy including Fe, Co, Ni, Cu, Mn and Zn.
4. The method for preparing a nitrogen-doped carbon-modified high entropy alloy catalyst according to any one of claims 1 to 3, characterized in that: include: Dissolve multiple metal salts of five or more metal elements selected from Fe, Co, Ni, Cu, Mn, Al and Zn in water in an amount equal to the metal atomic molar ratio, and stir to dissolve to obtain a solution A; wherein the solution A includes at least a zinc salt; Dissolving trimesic acid and an organic nitrogen source in an organic solvent to obtain a solution B; the organic nitrogen source comprises melamine or polyvinyl pyrrolidone; Mix solution A and solution B, stir and mix well to obtain a reaction solution; Placing the reaction liquid in a hydrothermal reactor and reacting it at 120-180° C. for a first preset time to obtain a reaction liquid; centrifuging the reaction liquid to obtain a precipitate, washing the precipitate and vacuum drying it to obtain a multi-metal precursor; The multi-metal precursor is kept at a temperature of 600-900° C. in an inert gas atmosphere for a second preset time period, and then cooled to room temperature to obtain a nitrogen-doped carbon-modified high entropy alloy catalyst.
5. The method for preparing a nitrogen-doped carbon-modified high entropy alloy catalyst according to claim 4, characterized in that: Metal salts of five or more metal elements selected from Fe, Co, Ni, Cu, Mn, Al and Zn are dissolved in water in an amount equal to the molar ratio of the metal atoms, so as to control the amount of the substance containing one of the metal atoms to water at a ratio of 1 to 2 mmol: 15 to 30 mL.
6. The method for preparing a nitrogen-doped carbon-modified high entropy alloy catalyst according to claim 4, characterized in that: In the step of dissolving trimesic acid and an organic nitrogen source in an organic solvent, the ratio of trimesic acid to the organic solvent is 4-8 mmol﹕15-30 mL; and / or the ratio of the organic nitrogen source to the organic solvent is 0.3-0.9 g﹕15-25 mL.
7. The method for preparing a nitrogen-doped carbon-modified high entropy alloy catalyst according to claim 4, characterized in that: Mixing solution A with solution B comprises: adding solution A to solution B at a rate of 5 to 15 mL / s; and / or, Mixing solution A and solution B includes: adding solution A to solution B at a volume ratio of solution A to solution B of 0.8 to 1.2:
1.
8. The method for preparing a nitrogen-doped carbon-modified high entropy alloy catalyst according to claim 4, characterized in that: The hydrothermal reaction product is kept at a temperature of 600 to 900° C. in an inert gas atmosphere for a second preset time period, comprising: The multi-metal precursor is placed in an inert gas atmosphere, heated to 600-900° C. at a rate of 3-8° C. / min and kept at this temperature for a second preset time.
9. The method for preparing a nitrogen-doped carbon-modified high entropy alloy catalyst according to claim 4, characterized in that: In the step of washing the precipitate and then vacuum drying the precipitate, the vacuum drying comprises: drying in a vacuum environment at 50-100°C.
10. Use of the nitrogen-doped carbon-modified high entropy alloy catalyst as described in any one of claims 1 to 3 or the nitrogen-doped carbon-modified high entropy alloy catalyst prepared by the preparation method of the nitrogen-doped carbon-modified high entropy alloy catalyst as described in any one of claims 4 to 9 in degrading organic pollutants in water.
Citation Information
Patent Citations
High-entropy alloy for sewage degradation and preparing method thereof
CN105088048A
Method for degrading dye wastewater by using high-entropy alloy
CN111533191A
Preparation method and application of high-entropy alloy catalyst
CN117696071A
ZIF-based high-entropy alloy catalyst as well as preparation method and application thereof
CN118437336A
Cited By
Method for catalytically decomposing lignin in supercritical ammonia by using high-entropy alloy catalyst
CN119633838A
High-entropy alloy / nitrogen-doped carbon nano catalytic material as well as preparation method and application thereof
CN119972150A
A high-entropy alloy / nitrogen-doped carbon nanocatalytic material, its preparation method and application
CN119972150B
High-catalysis and high-performance carbon nano composite material, preparation method and application
CN121575438A