Polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts and preparation method and application thereof

Through electrospinning and in-situ growth, iron and zinc bimetallic catalysts are loaded on the polymer fiber membrane to form a heterostructure, which solves the problems of catalyst active components loss and low efficiency of complex wastewater treatment, and achieves high efficiency and stability Catalytic effect and reusability of catalytic film.

CN118719153BActive Publication Date: 2024-11-26SHANDONG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411226687.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-26
Estimated Expiration
2044-09-03

Smart Images

  • Figure CN118719153B_ABST
    Figure CN118719153B_ABST
Patent Text Reader

Abstract

The present invention proposes a polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts and a preparation method and application thereof, which belongs to the technical field of catalytic membrane degradation and treatment of organic pollutants in wastewater, and can solve the problems that the powder catalyst agglomerates during the catalytic process, resulting in reduced catalytic efficiency, cumbersome recovery process, and single advanced oxidation technology is difficult to treat complex wastewater and has low degradation efficiency. The technical scheme includes the steps of preparing electrostatically spun polymer fiber membranes and in-situ growth of iron and zinc catalysts. The construction of heterogeneous structures between iron and zinc catalysts enables the coupling of photocatalysis and Fenton catalysis processes, greatly improving the ability and efficiency of degrading organic matter in wastewater. At the same time, the introduction of the membrane avoids the dispersion and separation recovery process of the powder catalyst, has good reusability, and proposes a novel and reliable method for the preparation of catalytic membranes, and provides an effective method for its application in wastewater degradation treatment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalytic membrane degradation treatment of organic pollutants in wastewater, and specifically relates to a polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts, and a preparation method and application thereof. Background Art

[0002] With the rapid development of industry and agriculture, the pollution of the environment by production wastewater is becoming increasingly serious. More and more organic pollutants such as dyes, pesticides and antibiotics are discharged into the water, and the types of difficult-to-biodegrade organic matter in the water are increasing, causing great harm to my country's ecological environment and biodiversity. Biological and physical methods are difficult to treat complex wastewater, while chemical methods can directly mineralize pollutants in wastewater, but a single advanced oxidation technology is increasingly unable to meet the degradation requirements of complex wastewater. How to efficiently and quickly treat complex wastewater has become a challenge.

[0003] The coupling of advanced oxidation technologies provides a feasible method to overcome the above problems. In the wastewater treatment process, single redox technologies are applied in combination according to different environments and situations to optimize these technologies, maximize the effect and minimize the cost. Currently, common coupling technologies include electro-Fenton technology, ozone-Fenton technology and photo-Fenton technology. Among them, photo-Fenton catalytic technology combines photocatalytic technology with heterogeneous Fenton technology to exert synergistic effects, improve the efficiency of pollutant degradation, and reduce Fe compared with traditional Fenton catalytic method. 2+ The amount of ions used improves the utilization rate of H2O2 and the generation rate of •OH, and its reaction process is not affected by the acidity and alkalinity of the wastewater, and can be applied to the treatment of wastewater of any acidity and alkalinity. At the same time, by constructing a heterogeneous structure, the spatial separation of photogenerated carriers can be achieved to improve the photocatalytic efficiency, thereby achieving rapid degradation of pollutants.

[0004] However, the loss of active components of metal catalysts during the catalytic process cannot be completely avoided. At the same time, the surface energy of heterogeneous metal catalysts is high, and agglomeration will occur during use, which hinders practical application. Therefore, it is necessary to combine the catalyst with the carrier. The polymer porous membrane has the advantages of large specific surface area, simple operation, strong flexibility, low cost, low energy consumption and unique selectivity, and is an excellent carrier for fixing solid catalysts. The traditional phase transformation method for preparing polymer membranes is relatively complicated and the resulting membrane flux is low. Electrospun nanofiber membranes have the advantages of high porosity, high specific surface area, a wide range of raw material options, simple operation and strong structural adjustability, and are suitable for use as carriers for fixing catalysts. Compared with fixing methods such as coupling, layer-by-layer self-assembly, and co-doping, the catalyst grown in situ on the surface of the fiber membrane has more uniform active sites, higher stability and yield. This fixing method helps to improve the performance and stability of the catalyst and provide more effective support and promotion for the catalytic reaction.

[0005] In summary, the present application adopts electrospinning and in-situ catalyst growth to prepare efficient and reliable bimetallic heterostructure catalytic membranes for the degradation of organic pollutants, aiming to overcome the problems of low wastewater treatment efficiency and difficulty in treating complex wastewater by traditional polymer catalytic membranes and single advanced oxidation technology. Summary of the invention

[0006] In view of the technical problems that the above-mentioned powder catalyst is easy to agglomerate during catalysis, the recovery process is complicated, the recovery efficiency is low, the traditional membrane has limited specificity for ionic and molecular pollutants in sewage, and the single advanced oxidation technology is difficult to treat complex sewage and cannot meet the needs of degrading difficult-to-degrade sewage, this application proposes a polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts and its preparation method and application. The catalytic membrane has the characteristics of good stability, high catalytic efficiency, high hydrogen peroxide utilization efficiency, wide pH range of use, and reusability, and can achieve continuous and efficient degradation of organic pollutants in water.

[0007] To achieve the above object, the present invention provides a method for preparing a polymer fiber catalytic membrane loaded with an iron and zinc bimetallic catalyst, comprising the following steps.

[0008] (1) Preparation of polymer fiber membrane: Add dry polymer particles into a solvent, heat and stir to dissolve to form a polymer spinning solution, and then use electrospinning and hot pressing to obtain a polymer fiber membrane.

[0009] (2) Loading of iron catalyst on polymer fiber membrane: dissolving iron salt in ethanol to prepare iron salt seed solution A, dissolving iron salt in pure water to prepare iron salt aqueous solution and adding ammonium fluoride to obtain iron salt growth solution B, then soaking the polymer fiber membrane obtained in step (1) in solution A and drying it, and then placing it in solution B for in-situ growth of iron catalyst, and freeze-drying after the growth to obtain the polymer fiber membrane loaded with iron catalyst.

[0010] (3) Loading of zinc catalyst on polymer fiber membrane: zinc salt and sodium hydroxide are dissolved in ethanol to prepare zinc salt seed solution C, the polymer fiber membrane loaded with iron catalyst obtained in step (2) is soaked in solution C and then annealed, and the above soaking and annealing process is repeated 3 to 10 times to obtain a polymer fiber membrane loaded with iron catalyst and zinc oxide seeds; zinc salt and hexamethylenetetramine are dissolved in pure water to prepare zinc salt growth solution D, the polymer fiber membrane loaded with iron catalyst and zinc oxide seeds obtained above is placed in the growth solution D for in-situ growth of zinc catalyst, and after the growth is completed, the membrane is washed with deionized water and ethanol, and dried to obtain a polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts.

[0011] In this preparation method, electrospinning technology is used to prepare a polymer fiber membrane, and then iron and zinc catalysts are grown on the fiber membrane through in situ growth technology. The two catalysts can form a heterogeneous structure, which accelerates the electron transfer rate in the oxidation process, increases the density of photogenerated carriers, and greatly improves the catalytic efficiency of the prepared catalytic membrane.

[0012] Preferably, the polymer in step (1) is at least one of polyvinylidene fluoride, polyethersulfone, and polyetherimide, and the solvent is at least one of N-methylpyrrolidone, tetrahydrofuran, N, N-dimethylformamide, N, N-dimethylacetamide, and acetone.

[0013] Preferably, in the step (1), the mass fraction of the polymer in the spinning solution is 16-32%, the humidity of the spinning environment is 25-60%, the spinning distance is 5-25 cm, the feed rate is 0.5-1.5 mL / h, the spinning voltage is 5-25 kV, the hot pressing temperature is 30-100° C., and the hot pressing time is 1-60 min.

[0014] Preferably, in step (2), the concentration of the iron salt seed solution A is 0.5-4.0 mol / L, the concentration of the iron salt growth solution B is 0.05-0.5 mol / L, the mass of ammonium fluoride is 0.25 g-2.5 g, the immersion time is 5-60 min, the in-situ growth temperature is 30-100° C., and the growth time is 1-10 h.

[0015] Preferably, in step (3), the concentration of the zinc salt seed solution C is 0.00045-0.0045 mol / L, the soaking time is 5-60 min, the annealing temperature is 100-180° C., the annealing time is 5-60 min, the concentration of the zinc salt growth solution D is 0.01-0.05 mol / L, the concentration of the hexamethylenetetramine solution is 0.01-0.05 mol / L, the in-situ growth temperature is 80-150° C., and the growth time is 1-10 h.

[0016] The present invention also provides a polymer fiber catalytic membrane loaded with an iron and zinc bimetallic catalyst prepared by the method described in any one of the above technical solutions.

[0017] Preferably, the polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts has a thickness of 30 to 120 μm, is in the form of a flat membrane, and has a connected porous structure. The zinc catalyst is in the form of nanorods and evenly and densely covers the surface of the polymer membrane. The iron catalyst is assembled into a sheet on the surface of the polymer fiber and below the zinc catalyst. The two are interconnected and independent of each other. Figure 3 shown.

[0018] The present invention also provides a method for degrading organic pollutants using the above-mentioned polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts, comprising the following steps: using the polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts to perform Fenton catalysis, photocatalysis and photo-Fenton catalysis to generate strong oxidizing free radicals under certain temperature, pH, hydrogen peroxide concentration, and with or without light conditions to oxidatively degrade organic pollutants in wastewater.

[0019] Preferably, the pH value of the organic pollutant solution is 2-10, the temperature of the catalytic degradation reaction is 1-60° C., the molar ratio of the hydrogen peroxide to the organic pollutant is 1:1-150:1, the light source is sunlight or ultraviolet light, and the organic pollutant is at least one of a dye, phenols and their derivatives, antibiotics, environmental hormones and disinfection by-products, wherein the dye is selected from at least one of Congo red, rhodamine B, orange G and methylene blue, the phenols and their derivatives are selected from at least one of phenol, p-chlorophenol, p-nitrophenol, bisphenol A and 2-chlorophenol, the antibiotic is selected from at least one of ciprofloxacin, levofloxacin, sulfamethoxazole and clarithromycin, the environmental hormone is selected from at least one of cyanurate, soy isoflavones, estradiol, nitrotoluene and alkylphenols, and the disinfection by-product is at least one of chloroform, bromoform, formaldehyde and 2,4,6-trichlorophenol.

[0020] Compared with the prior art, the advantages and positive effects of the present invention lie in the following three aspects.

[0021] 1. The present invention provides an electrospinning method for preparing a polymer fiber membrane as a catalyst carrier. In the preparation process, the dried polymer particles are heated and stirred with a solvent to obtain a spinning solution, and a membrane carrier having the advantages of large pore size, high porosity, good pore connectivity, and low surface density is prepared under certain conditions by electrospinning technology. The preparation method is simple and easy to operate.

[0022] 2. The present invention provides a polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts by loading iron oxide and zinc oxide on a polymer fiber membrane by an in-situ growth method. The heterogeneous structure formed by the iron catalyst and the zinc catalyst allows the Fenton catalytic and photocatalytic processes to be coupled in one process, and the synergy of the two enhances the catalytic performance of the catalytic membrane. In the preparation process, the polymer fiber membrane is transformed into a polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts with high loading, high stability and high catalytic performance by iron salt immersion, zinc salt immersion and in-situ growth. The preparation method is simple and efficient.

[0023] 3. The polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts prepared by the above method can dynamically and continuously catalytically degrade organic pollutants and can be recycled and reused, avoiding the dispersion and separation process of powder catalysts. At the same time, the iron and zinc bimetallic catalysts simultaneously give the catalytic membrane photocatalytic properties and Fenton catalytic properties. The coupling of these two advanced oxidation technologies greatly improves the performance of the catalytic membrane. The polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts has good reusability, high catalytic rate, and can remove 99.9% of organic pollutants, providing a new and effective method for the treatment of complex wastewater. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is an electron microscope photo of the polymer fiber membrane.

[0025] Figure 2 This is an electron microscope photograph of a polymer fiber membrane loaded with iron catalyst.

[0026] Figure 3 This is an electron microscope photograph of a polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts. DETAILED DESCRIPTION

[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] The embodiment of the present invention provides a method for preparing a polymer fiber catalytic membrane loaded with an iron and zinc bimetallic catalyst, comprising the following steps.

[0029] (1) Preparation of polymer fiber membrane: Add dry polymer particles into a solvent, heat and stir to dissolve to form a polymer spinning solution, and then use electrospinning and hot pressing to obtain a polymer fiber membrane.

[0030] (2) Loading of iron catalyst on polymer fiber membrane: dissolving iron salt in ethanol to prepare iron salt seed solution A, dissolving iron salt in pure water to prepare iron salt aqueous solution and adding ammonium fluoride to obtain iron salt growth solution B, then immersing the polymer fiber membrane obtained in step (1) in solution A and drying it, then placing it in solution B for in-situ growth of iron catalyst, and freeze-drying after the growth to obtain a polymer fiber membrane loaded with iron catalyst.

[0031] (3) Loading of zinc catalyst on polymer fiber membrane: zinc salt and sodium hydroxide are dissolved in ethanol to prepare zinc salt seed solution C, the polymer fiber membrane loaded with iron catalyst obtained in step (2) is soaked in solution C and then annealed, and the above soaking and annealing process is repeated 3 to 10 times to obtain a polymer fiber membrane loaded with iron catalyst and zinc oxide seeds; zinc salt and hexamethylenetetramine are dissolved in pure water to prepare zinc salt growth solution D, the polymer fiber membrane loaded with iron catalyst and zinc oxide seeds obtained above is placed in the growth solution D for in-situ growth of zinc catalyst, and after the growth is completed, the membrane is washed with deionized water and ethanol, and dried to obtain a polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts.

[0032] The main feature of the preparation method provided by the above example is that the polymer spinning solution is prepared by electrostatic spinning technology to obtain a polymer fiber film, and then the iron oxide catalyst and the zinc oxide catalyst are loaded on the polymer fiber by the in-situ growth method, and finally the polymer fiber catalytic film loaded with iron and zinc bimetallic catalysts is obtained. Specifically, the polymer spinning solution is placed in a high-voltage electrostatic field, and under the action of the electric field force, the spinning solution is charged and deformed, and a Taylor cone droplet is formed at the end of the nozzle. When the charge repulsion on the surface of the droplet exceeds the surface tension, a jet is ejected at high speed on the surface of the droplet. These jets are stretched at high speed by the electric field force, the solvent evaporates and solidifies, and finally deposited on the receiving plate to form a polymer fiber. The polymer fiber obtained by spinning is subjected to hot pressing treatment, placed in an iron salt / ethanol solution and soaked, so that the iron ions are adsorbed on the nanofibers, and the iron ions are hydrolyzed in the aqueous solution to generate iron oxides, and then further nucleated and grown in a growth solution prepared by iron salt and ammonium fluoride, and finally the iron catalyst is grown in situ on the polymer fiber, and the polymer fiber catalytic film loaded with iron catalyst is obtained after freeze drying. Next, the dried polymer fiber catalytic membrane loaded with iron catalyst is immersed in a zinc salt seed solution. After repeated immersion and high-temperature annealing, zinc oxide crystal seeds are formed on the surface of the polymer fiber catalytic membrane loaded with iron catalyst. Subsequently, the zinc oxide crystal seeds grow in situ into zinc oxide nanorods in the growth solution. After drying, a polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts is obtained.

[0033] In the above steps, the catalytic membrane obtained by electrospinning technology and in-situ growth method, the zinc catalyst is evenly and densely covered on the surface of the polymer membrane, and the iron catalyst is assembled into a sheet on the surface of the polymer membrane and below the zinc catalyst, as shown in the attached Figure 3As shown. The iron and zinc catalysts have good binding properties and successfully constructed a bimetallic heterostructure, which is interconnected and separated. This structure allows the catalytic membrane to couple the two advanced oxidation technologies of photocatalysis and Fenton catalysis, and the electron transfer rate in the Fenton process is accelerated due to the presence of the heterostructure. The recombination rate of photogenerated carriers in the photocatalytic process is greatly reduced due to the presence of the heterostructure, and the carrier density is increased, which greatly improves the catalytic performance of the catalytic membrane, enhances the membrane's anti-pollution, antibacterial and self-cleaning capabilities, and can treat more complex wastewater. At the same time, the introduction of the membrane allows the catalyst to be recycled repeatedly, prevents the aggregation of the catalyst, improves the efficiency of the catalyst in degrading pollutants, and improves the ability to treat complex sewage. More importantly, the polymer fiber catalytic membrane has good permeability, excellent physical and chemical stability and flexibility. In actual applications, the catalytic membrane can maintain good anti-shrinkage ability in the face of harsh environmental conditions (high temperature, acid and alkali, etc.) and mechanical pressure generated by the components, avoiding membrane tearing, reduced flow rate, etc., and ensuring that the polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts maintains excellent catalytic effect and stability during the catalytic degradation of organic pollutants in wastewater at high temperature.

[0034] In a preferred embodiment, the polymer in step (1) is at least one of polyvinylidene fluoride, polyethersulfone, and polyetherimide, and the solvent is at least one of N-methylpyrrolidone, tetrahydrofuran, N, N-dimethylformamide, N, N-dimethylacetamide, and acetone. The mass fraction of the polymer in the spinning solution is 16-32%, the spinning environment humidity is 25-60%, the spinning distance is 5-25 cm, the feed rate is 0.5-1.5 mL / h, the spinning voltage is 5-25 kV, the hot pressing temperature is 30-100 ° C, and the hot pressing time is 1-60 min. The mass fraction of the polymer in the spinning solution is limited in this embodiment because, when the mass fraction is lower than 16%, the viscosity of the spinning solution is too low, so that the jet is prone to uneven force during the stretching process and cannot form fibers with uniform diameters; when the mass fraction is higher than 32%, the polymer molecular chains are tightly entangled, and the molecular chains entangled with each other under the same electric field tension cannot whip freely in the radial direction of the jet, causing serious fiber bonding. It is understandable that the mass fraction of the polymer in the polymer spinning solution can also be any value within the above range. The choice of solvent in the embodiment is not limited to that listed in the above embodiment, and can also be other substances reasonably selected and adjusted by technicians in this field according to common sense. This embodiment also limits the scope of spinning conditions because, when the setting values ​​of each condition are lower than the lower limit of the limited range, the spinning solution jet is unevenly stressed during the stretching process and the solvent evaporation rate is insufficient, and it is impossible to form fibers with uniform diameters; when the setting values ​​of each condition are higher than the upper limit of the limited range, the speed of the spinning jet is accelerated, so that the time required for the jet to reach the receiving roller is shortened, and the instability increases. At the same time, too short a time makes it impossible for the solvent in the jet to completely volatilize, and the residual solvent makes the fibers on the roller that are not completely solidified to stick to each other, or even stick to form a sheet without a fiber structure. It can be understood that the spinning condition value can also be any value within the above ranges. Those skilled in the art can adjust it according to the actual reaction situation.

[0035] In a preferred embodiment, in step (2), the concentration of the iron salt seed solution A is 0.5-4.0 mol / L, the concentration of the iron salt growth solution B is 0.05-0.5 mol / L, the mass of ammonium fluoride is 0.25 g-2.5 g, the soaking time is 5-60 min, the in-situ growth temperature is 30-100 ° C, and the growth time is 1-10 h. When the concentration of the iron salt seed solution A is lower than 0.5 mol / L and the soaking time is lower than 5 min, the iron ion concentration is low and the soaking time is too short, which is not conducive to the adsorption and loading of the iron catalyst seeds; when the concentration of the iron salt seed solution A is higher than 4.0 mol / L and the soaking time is higher than 60 min, the catalyst will eventually accumulate densely on the fiber membrane, reducing the effective area of ​​the catalyst and the catalytic efficiency. It can be understood that the concentration of the iron salt seed solution A and the soaking time can also be any value in the above range. This embodiment also defines the concentration of the iron salt growth solution B in the iron catalyst growth stage as 0.05-0.5 mol / L, the mass of ammonium fluoride as 0.25 g-2.5 g, the in-situ growth temperature as 30-100 ° C, and the growth time as 1-10 h. The reason is that when the concentration of the iron salt growth solution B is lower than 0.05 mol / L, the mass of ammonium fluoride is lower than 0.25 g, the growth temperature is lower than 30 ° C, and the growth time is lower than 1 h, it is not conducive to the intrinsic energy balance between the crystallographic characteristics and the growth domain, and is not conducive to the nucleation growth of the iron catalyst. When the concentration of the iron salt growth solution B is higher than 0.5 mol / L, the mass of ammonium fluoride is higher than 2.5 g, the growth temperature is higher than 100 ° C, and the in-situ growth time is greater than 10 h, it is difficult to generate an iron catalyst with a higher effective surface area, which is not conducive to preferentially exposing more active crystal faces during thermodynamic equilibrium, and is not conducive to the exposure of iron catalytic active sites, affecting the catalytic efficiency of the catalytic film. At the same time, the higher growth temperature also causes energy waste. It is understandable that the values ​​of the various conditions in the in-situ growth stage of the iron catalyst can also be any value within the above ranges, and those skilled in the art can adjust them according to the actual reaction conditions.

[0036] In a preferred embodiment, in step (3), the concentration of the zinc salt seed solution C is 0.00045-0.0045 mol / L, the soaking time is 5-60 min, the annealing temperature is 100-180° C., the annealing time is 5-60 min, the concentration of the zinc salt growth solution D is 0.01-0.05 mol / L, the concentration of the hexamethylenetetramine solution is 0.01-0.05 mol / L, the in-situ growth temperature is 80-150° C., and the growth time is 1-10 h. In this example, the concentration of zinc salt seed solution C, soaking time, annealing temperature and annealing time are limited. The reason is that when the concentration of zinc salt seed solution C is lower than 0.00045 mol / L, the soaking time is lower than 5 min, the annealing temperature is lower than 100 ° C, and the annealing time is lower than 5 min, the molecular thermal motion in the solution is restricted, and the repulsion between the particles is relatively large, which is not conducive to the preparation of the seed solution, affecting the successful conversion of zinc salt into zinc oxide crystal seeds, and is not conducive to the uniform loading of zinc oxide seeds on the surface of the polymer film, affecting the uniform growth of zinc catalysts and the formation of heterogeneous structures. When the concentration of zinc salt seed solution C is higher than 0.0045 mol / L, the soaking time is lower than 60 min, the annealing temperature is higher than 180 ° C, and the annealing time is higher than 60 min, the catalyst will be densely accumulated on the fiber membrane, reducing the effective area of ​​the catalyst and the catalytic efficiency. At the same time, the excessively high annealing temperature affects the stability of the polymer film. It can be understood that the values ​​of each condition in the above zinc oxide seed loading stage can also be any point value within the above range. In this example, the concentration of zinc salt growth solution D is limited to 0.01~0.05mol / L, the concentration of hexamethylenetetramine solution is limited to 0.01~0.05mol / L, the in-situ growth temperature is limited to 80~150℃, and the growth time is limited to 1~10h. The reason is that when the concentration of zinc salt growth solution D is lower than 0.01mol / L, the concentration of hexamethylenetetramine solution is lower than 0.01mol / L, the growth temperature is lower than 80℃, and the growth time is lower than 1h, it is not conducive to the intrinsic energy balance between crystallographic features and growth domains, and is not conducive to the nucleation growth of zinc catalysts. When the concentration of zinc salt growth solution D is higher than 0.05mol / L, the concentration of hexamethylenetetramine solution is higher than 0.05mol / L, the growth temperature is higher than 150℃, and the growth time is higher than 10h, it is difficult to generate zinc catalysts with higher effective surface areas, which is not conducive to preferentially exposing more active crystal faces during thermodynamic equilibrium, is not conducive to the exposure of catalytic active sites, is not conducive to the construction of heterogeneous structures, and affects the catalytic efficiency of the catalytic film. At the same time, the higher growth temperature also causes energy waste. It is understandable that the values ​​of the various conditions in the in-situ growth stage of the zinc catalyst can also be any value within the above range, and those skilled in the art can adjust them according to the actual reaction conditions.

[0037] The embodiment of the present invention also provides a polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts prepared by the method described in the above embodiment.

[0038] In a preferred embodiment, the polymer catalytic membrane loaded with iron and zinc bimetallic catalysts has a thickness of 30 to 120 μm and is in the form of a flat membrane with a connected porous structure. The zinc catalyst is in the form of nanorods and is evenly and densely covered on the surface of the polymer membrane. The iron catalyst is assembled into a sheet on the surface of the polymer fiber and below the zinc catalyst. Figure 3 The present invention limits the thickness of the polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts to 30-120 μm. The reason is that when the thickness of the polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts is less than 30 μm, the residence time of the organic wastewater solution passing through the membrane during the catalytic process is short, and the catalytic efficiency is low; when the thickness is higher than 120 μm, the membrane resistance increases, and the flux of the organic wastewater solution passing through the membrane decreases, which is not conducive to the large-scale treatment of organic wastewater and reduces the wastewater treatment volume.

[0039] An embodiment of the present invention also provides a method for catalytically degrading organic pollutants in wastewater using the polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts as described in the above embodiment, comprising the following steps: using the polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts to perform Fenton catalysis, photocatalysis or photo-Fenton catalysis to generate strong oxidizing free radicals under certain temperature, pH, hydrogen peroxide concentration, and the presence or absence of sunlight or ultraviolet light conditions to oxidatively degrade the organic pollutants in the wastewater.

[0040] In a preferred embodiment, the pH of the organic pollutant solution is 2-10, the temperature of the catalytic reaction is 1-60°C, the molar ratio of the hydrogen peroxide to the organic pollutant is 1:1-150:1, and the illumination is a light source such as sunlight, ultraviolet light, and visible light. In this embodiment, the pH of the catalytic reaction is limited to 2-10 because the polymer catalytic membrane loaded with iron and zinc bimetallic catalysts has excellent catalytic effects within this pH range, and this pH range covers almost all pH environments of wastewater, thereby eliminating the need for the complex operation of adjusting the pH twice before and after wastewater treatment, greatly simplifying the wastewater treatment process and reducing costs. At the same time, it will not cause the pH required in the traditional wastewater treatment process to be too low or too high, thereby corroding equipment and polluting the environment. In addition, the molar ratio of hydrogen peroxide to organic pollutants is also limited in this embodiment. The main reason is that within this ratio range, the free radicals generated by the decomposition of hydrogen peroxide by the catalytic membrane have the best oxidative degradation effect on organic pollutants. If it is lower than 1:1, the amount of hydrogen peroxide added is insufficient, and sufficient free radicals for oxidizing pollutants cannot be generated, resulting in poor degradation effect. If it is higher than 150:1, hydrogen peroxide is wasted and costs are increased. It is understandable that the molar ratio of hydrogen peroxide to organic pollutants can also be any value within the above range, and those skilled in the art can adjust the above parameters according to the actual reaction conditions.

[0041] In a preferred embodiment, the organic pollutant is at least one of dyes, phenols and their derivatives, antibiotics, environmental hormones and disinfection by-products, wherein the dye is selected from at least one of Congo red, rhodamine B, orange G and methylene blue, the phenols and their derivatives are selected from at least one of phenol, p-chlorophenol, p-nitrophenol, bisphenol A and 2-chlorophenol, the antibiotic is selected from at least one of ciprofloxacin, levofloxacin, sulfamethoxazole and clarithromycin, the environmental hormone is selected from at least one of cyanurate, soy isoflavones, estradiol, nitrotoluene and alkylphenols, and the disinfection by-product is at least one of chloroform, bromoform, formaldehyde and 2,4,6-trichlorophenol.

[0042] In order to more clearly and in detail introduce the polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts provided by the embodiments of the present invention, it will be described below in conjunction with specific embodiments.

[0043] Example 1

[0044] The polymer fiber membrane was prepared by electrospinning. Specifically, 5 g of polyvinylidene fluoride was dissolved in 15 g of N, N-dimethylacetamide solvent and stirred to obtain a spinning solution. Then, electrospinning was performed at a voltage of 9 kV, a feed rate of 0.6 mL / h, a spinning distance of 15 cm, a spinning environment temperature of 25 ° C, and an ambient humidity of 40%. The collected fiber membrane was placed in a hot press and hot pressed at 65 ° C for 15 minutes to obtain a polymer fiber membrane.

[0045] The iron catalyst was loaded on the polymer fiber membrane by the in-situ growth method. Specifically, 13.5g of ferric chloride was weighed and dissolved in 50mL of ethanol to obtain 1mol / L of iron salt seed solution A; 4.1g of ferric chloride was weighed and dissolved in 50mL of deionized water and 1.39g of ammonium fluoride was added to obtain 0.3mol / L of iron salt growth solution B. Then the polyvinylidene fluoride fiber membrane obtained above was placed in the above iron salt seed solution A and soaked for 20min, then dried in a 50℃ oven for 1h, and then placed in the above iron salt growth solution B and reacted at 50℃ for 6 hours. After the reaction was completed, the membrane was washed 3 times with deionized water and then freeze-dried to obtain a polyvinylidene fluoride polymer fiber membrane loaded with iron catalyst.

[0046] The zinc catalyst was loaded on the polymer fiber membrane loaded with the iron catalyst by the in-situ growth method. Specifically, at 65°C, 13.75 mg of zinc acetate dihydrate and 5 mg of sodium hydroxide were added to 45 mL of ethanol and stirred for 1.5 hours to dissolve, and a 0.0014 mol / L zinc salt seed solution C was obtained. The dried polymer fiber membrane loaded with the iron catalyst was soaked in the above seed solution for 10 min and annealed at 150°C for 10 min, and the process was repeated five times to load the zinc catalyst seeds. Subsequently, 0.45 g of zinc nitrate hexahydrate and 0.225 g of hexamethylenetetramine were dissolved in 50 mL of deionized water and stirred for 30 min to obtain a 0.03 mol / L zinc salt growth solution D, and the polymer fiber membrane loaded with the iron catalyst and the zinc catalyst seeds was placed in the above zinc salt growth solution D, and reacted at 90°C for 4 hours. After the reaction, the membrane was washed with deionized water and ethanol 5 times and then dried in a 60°C oven to obtain a polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts.

[0047] The polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts degrades organic pollutants. Specifically, the obtained polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts is added to a methyl orange solution, and a catalytic reaction is carried out under the conditions of room temperature, pH=2, and ultraviolet light irradiation, wherein the molar ratio of hydrogen peroxide to methyl orange is 60:1.

[0048] Example 2

[0049] The preparation method of the polymer fiber membrane is the same as that of Example 1, except that the polymer used is polyetherimide, and the solvent used is 12 g of N-methylpyrrolidone and 3 g of tetrahydrofuran.

[0050] The method for loading the iron catalyst on the polymer fiber membrane is the same as that in Example 1.

[0051] The method for loading the polymer fiber membrane with an iron and zinc bimetallic catalyst is the same as that in Example 1, except that the zinc salt used is zinc sulfate.

[0052] The method for degrading organic pollutants using the polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts is the same as that in Example 1.

[0053] Example 3

[0054] The preparation method of the polymer fiber membrane is the same as that of Example 1, except that the polymer used is polyethersulfone.

[0055] The method for loading the iron catalyst on the polymer fiber membrane is the same as that in Example 1, except that the iron salt used is ferric sulfate.

[0056] The method for loading the polymer fiber membrane with an iron and zinc bimetallic catalyst is the same as that in Example 1, except that the zinc salt used is zinc sulfite.

[0057] The method for degrading organic pollutants using the polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts is the same as that in Example 1.

[0058] Example 4

[0059] The preparation method of the polymer fiber membrane is the same as that of Example 2.

[0060] The method for loading the iron catalyst on the polymer fiber membrane is the same as that in Example 1, except that the concentration of the iron salt growth solution B is 0.4 mol / L.

[0061] The method for loading the polymer fiber membrane with iron and zinc bimetallic catalysts is the same as that in Example 1, except that the concentration of the zinc salt seed solution C used is 0.0025 mol / L, and the concentration of the zinc salt growth solution D is 0.04 mol / L.

[0062] The method for degrading organic pollutants by the polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts is the same as that in Example 1, except that the organic pollutant used is Congo red.

[0063] Example 5

[0064] The preparation method of the polymer fiber membrane is the same as that of Example 2, except that the mass of the polyetherimide is 6 g.

[0065] The method for loading the iron catalyst on the polymer fiber membrane is the same as that in Example 1, except that the concentration of the iron salt growth solution B is 0.2 mol / L.

[0066] The method for loading the polymer fiber membrane with iron and zinc bimetallic catalysts is the same as that in Example 1, except that the concentration of the zinc salt seed solution C used is 0.0035 mol / L, and the concentration of the zinc salt growth solution D is 0.045 mol / L.

[0067] The method for degrading organic pollutants by the polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts is the same as that in Example 1, except that the organic pollutant used is phenol.

[0068] Example 6

[0069] The preparation method of the polymer fiber membrane is the same as that of Example 2.

[0070] The method for loading the iron catalyst on the polymer fiber membrane is the same as that in Example 1.

[0071] The method for loading the polymer fiber membrane with an iron and zinc bimetallic catalyst is the same as that in Example 1, except that the type of zinc salt used is zinc nitrite.

[0072] The method for degrading organic pollutants using the polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts is the same as that in Example 1, except that the pH value of the solution is 4.

[0073] Example 7

[0074] The preparation method of the polymer fiber membrane is the same as that of Example 2.

[0075] The method for loading the iron catalyst on the polymer fiber membrane is the same as that in Example 1, except that the concentration of the iron salt seed solution A is 0.8 mol / L.

[0076] The method for loading the polymer fiber membrane with an iron and zinc bimetallic catalyst is the same as that in Example 1, except that the type of zinc salt used is zinc sulfate.

[0077] The method for degrading organic pollutants by the polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts is the same as that in Example 1, except that the pH of the solution is 6, and the organic pollutant used is ciprofloxacin.

[0078] Example 8

[0079] The preparation method of the polymer fiber membrane is the same as that of Example 2.

[0080] The method for loading the iron catalyst on the polymer fiber membrane is the same as that in Example 1, except that the concentration of the iron salt seed solution A is 1.2 mol / L.

[0081] The method for loading the polymer fiber membrane with an iron and zinc bimetallic catalyst is the same as that in Example 1, except that the type of zinc salt used is zinc sulfite.

[0082] The method for degrading organic pollutants by the polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts is the same as that in Example 1, except that the pH of the solution is 10 and the organic pollutant used is ciprofloxacin.

[0083] Example 9

[0084] The preparation method of the polymer fiber membrane is the same as that of Example 2.

[0085] The method for loading the iron catalyst on the polymer fiber membrane is the same as that in Example 1.

[0086] The method of loading the polymer fiber membrane with iron and zinc bimetallic catalyst is the same as that in Example 1, except that the thickness of the catalyst membrane is 80 μm.

[0087] The method for degrading organic pollutants by the polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts is the same as that in Example 1, except that the molar ratio of hydrogen peroxide to methyl orange is 20:1.

[0088] Example 10

[0089] The preparation method of the polymer fiber membrane is the same as that of Example 2.

[0090] The method for loading the iron catalyst on the polymer fiber membrane is the same as that in Example 1.

[0091] The method of loading the polymer fiber membrane with iron and zinc bimetallic catalyst is the same as that in Example 1, except that the thickness of the catalyst membrane is 100 μm.

[0092] The method for degrading organic pollutants by the polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts is the same as that in Example 1, except that the molar ratio of hydrogen peroxide to methyl orange is 40:1.

[0093] Embodiment 11

[0094] The preparation method of the polymer fiber membrane is the same as that of Example 2.

[0095] The method for loading the iron catalyst on the polymer fiber membrane is the same as that in Example 1.

[0096] The method of loading the polymer fiber membrane with iron and zinc bimetallic catalyst is the same as that in Example 1, except that the thickness of the catalytic membrane is 120 μm.

[0097] The method for degrading organic pollutants by the polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts is the same as that in Example 1, except that the molar ratio of hydrogen peroxide to methyl orange is 80:1.

[0098] Example 12

[0099] The preparation method of the polymer fiber membrane is the same as that of Example 2.

[0100] The method for loading the iron catalyst on the polymer fiber membrane is the same as that in Example 1.

[0101] The method for loading the polymer fiber membrane with iron and zinc bimetallic catalysts is the same as that in Example 11.

[0102] The method for degrading organic pollutants by the polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts is the same as that in Example 1, except that the molar ratio of hydrogen peroxide to methyl orange is 120:1.

[0103] Example 13

[0104] The preparation method of the polymer fiber membrane is the same as that of Example 2.

[0105] The method for loading the iron catalyst on the polymer fiber membrane is the same as that in Example 1.

[0106] The method for loading the polymer fiber membrane with iron and zinc bimetallic catalysts is the same as that in Example 1.

[0107] The method for degrading organic pollutants by the polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts is the same as that in Example 1, except that a xenon lamp is used to simulate sunlight during the catalytic degradation process.

[0108] Comparative Example 1

[0109] The preparation method of the polymer fiber membrane is the same as that of Example 2.

[0110] The method for degrading organic pollutants by the polymer fiber membrane is the same as that in Example 1.

[0111] Comparative Example 2

[0112] The preparation method of the polymer fiber membrane is the same as that of Example 2.

[0113] The method for loading the iron catalyst on the polymer fiber membrane is the same as that in Example 1.

[0114] The method for degrading organic pollutants using the polymer catalytic membrane loaded with iron catalyst is the same as that in Example 1.

[0115] Comparative Example 3

[0116] The preparation method of the polymer fiber membrane is the same as that of Example 2.

[0117] The method for loading the iron catalyst on the polymer fiber membrane is the same as that in Example 1.

[0118] The method of loading the polymer fiber membrane with iron and zinc bimetallic catalyst is the same as that in Example 1

[0119] The method for degrading organic pollutants by the polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts is the same as that in Example 1, except that there is no light source irradiation during the catalytic degradation process.

[0120] Performance Testing

[0121] 1. Catalytic performance

[0122] The relevant performance test data of the catalytic degradation of organic pollutants by the catalytic membranes prepared in Examples 1-13 of the present invention and Comparative Examples 1-3 are shown in Table 1.

[0123] The analytical method of organic degradation adopted by the present invention is absorbance method, specifically, dyes such as methyl orange and orange yellow G have maximum absorbance in the visible light region, and are proportional to their content, so the content of different stages of degradation is measured by colorimetry. The testing method of phenolic substances is 4-aminoantipyrine method, i.e., phenolic compounds react with 4-aminoantipyrine at pH=10 or so in the presence of potassium ferrocyanide to generate orange-red indole antipyrine dye, and the color is proportional to the content of phenolic compounds within a certain concentration range, so the content of different stages is measured by colorimetry. In addition, environmental hormones such as soybean isoflavones, antibiotics such as ciprofloxacin and disinfection byproducts such as 2,4,6-trichlorophenol are measured by high performance liquid chromatography.

[0124] The calculation formula for the degradation rate of organic pollutants is: Degradation rate (%) = (mass of degraded organic matter / initial mass of organic matter) × 100%.

[0125] Table 1 Relevant performance test data of catalytic degradation of organic pollutants by catalytic membrane

[0126] Degradation time Final degradation rate Example 1 10 minutes 99.9% Example 2 10 minutes 99.8% Example 3 10 minutes 99.7 Example 4 10 minutes 98.5% Example 5 11 minutes 98.6% Example 6 40 minutes 99.2% Example 7 70 minutes 98.9% Example 8 120 minutes 98.6% Example 9 20 minutes 99.5% Example 10 14 minutes 99.6% Embodiment 11 14 minutes 98.9% Example 12 12 minutes 99.4% Embodiment 13 10 minutes 99.5% Comparative Example 1 60 minutes 0 Comparative Example 2 60 minutes 32.4% Comparative Example 3 600 minutes 99.2%

[0127] As shown in Table 1, the polymer fiber catalytic membrane of the iron and zinc bimetallic catalyst prepared by the embodiment of the present invention has excellent catalytic performance for different organic pollutants, and the catalytic membrane avoids the secondary separation of the catalyst, reducing the cost. The polymer fiber catalytic membrane of the iron and zinc bimetallic catalyst prepared by different iron salts and zinc salts all has excellent catalytic performance. The polymer fiber catalytic membrane of the iron and zinc bimetallic catalyst prepared by the embodiment of the present invention not only has excellent catalyst performance under acidic conditions, but also has good catalytic performance under neutral to alkaline conditions. In Example 7, under the condition of pH 6, the degradation rate of methyl orange in 70 minutes reaches 98.9%, which is much higher than the effect of the existing catalyst. In Example 1, when light-Fenton catalysis is carried out under the conditions of room temperature, pH=2, ultraviolet irradiation, and the molar ratio of hydrogen peroxide to methyl orange is 60:1, at 10min, the degradation rate of methyl orange reaches 99.9%. Compared with the comparative example 1, which takes 600 minutes to degrade the catalytic reaction without light irradiation, this has a significant advantage, indicating that the heterogeneous structure constructed by the combination of iron and zinc catalysts realizes the coupling of two advanced oxidation technologies, greatly improving the rate of wastewater treatment by the catalytic membrane. It also has a significant advantage over the polymer catalytic membrane loaded with iron catalyst in comparative example 2, because the construction of the heterogeneous structure accelerates the electron transfer rate in the catalytic process, increases the density of photogenerated carriers, and strengthens the redox ability of the entire system to organic pollutants, thereby improving the degradation rate of the catalytic membrane.

[0128] 2. Stability of polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts

[0129] In order to further investigate the stability of the polymer catalytic membrane loaded with iron and zinc bimetallic catalysts, the stability of the polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts was monitored under different reaction times. The results are shown in Table 2.

[0130] Table 2 Stability data of polymer fiber catalytic membranes loaded with iron and zinc bimetallic catalysts

[0131]

[0132] From the results in Table 2, it can be seen that the polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts prepared by the embodiment of the present invention still maintains good stability and reusability after 10 cycles of catalytic degradation of methyl orange and phenol under conditions with and without light. Combined with the above catalytic performance test, it can be seen that the presence or absence of light affects the catalytic efficiency of the catalytic membrane, but does not affect the stability of the catalytic membrane, that is, the catalytic membrane of the present invention itself has good stability.

Claims

1. A method for preparing a polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts, characterized in that: The method is prepared by the following steps: (1) preparing a polymer fiber membrane: adding dried polymer particles to a solvent, heating and stirring to dissolve the particles, forming a polymer spinning solution, and obtaining a polymer fiber membrane by electrospinning and hot pressing. The polymer is at least one of polyvinylidene fluoride, polyether sulfone, and polyetherimide. The solvent is N-methylpyrrolidone, tetrahydrofuran, N, N-dimethylformamide, N, At least one of N-dimethylacetamide and acetone; (2) loading of iron catalyst on polymer fiber membrane: dissolving iron salt in ethanol to prepare iron salt seed solution A with a concentration of 0.5-4.0 mol / L, dissolving iron salt in pure water and adding 0.25 g-2.5 g of ammonium fluoride to obtain iron salt growth solution B with a concentration of 0.05-0.5 mol / L, then soaking the polymer fiber membrane obtained in step (1) in solution A for 5-60 min and drying it, then placing it in solution B at 30-100° C. for 1-10 h of in-situ growth of iron catalyst, and freeze-drying after the growth to obtain a polymer fiber membrane loaded with iron catalyst; (3) loading of zinc catalyst on polymer fiber membrane: dissolving zinc salt and sodium hydroxide in ethanol to prepare zinc salt seed solution C with a concentration of 0.00045-0.0045 mol / L, soaking the polymer fiber membrane loaded with iron catalyst obtained in step (2) in solution C for 5 ~60min later, annealing is carried out at 100~180℃, and the above immersion and annealing process is repeated 3~10 times to obtain a polymer fiber membrane loaded with iron catalyst and zinc oxide seeds; zinc salt is added to a hexamethylenetetramine aqueous solution with a concentration of 0.01~0.05mol / L to obtain a zinc salt growth solution D with a concentration of 0.01~0.05mol / L, and the polymer fiber membrane loaded with iron catalyst and zinc oxide seeds obtained above is placed in the growth solution D to carry out in-situ growth of zinc catalyst for 1~10h at 80~150℃, and after the growth is completed, the membrane is washed with deionized water and ethanol, and dried to obtain a flat polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts with a thickness of 30~120μm, which has a connected porous structure, and the zinc catalyst is uniformly and densely covered on the surface of the polymer membrane in the form of nanorods, and the iron catalyst is assembled into sheets on the surface of the polymer fiber and under the zinc catalyst, and the two are interconnected and independent of each other.

2. The method for preparing a polymer fiber catalytic membrane loaded with an iron and zinc bimetallic catalyst according to claim 1, characterized in that: In the step (1), the mass fraction of the polymer in the spinning solution is 16-32%, the humidity of the spinning environment is 25-60%, the spinning distance is 5-25 cm, the feed rate is 0.5-1.5 mL / h, the spinning voltage is 5-25 kV, the hot pressing temperature is 30-100° C., and the hot pressing time is 1-60 min.

3. A polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts, characterized in that: The polymer fiber catalytic membrane is prepared by the method for preparing a polymer fiber catalytic membrane loaded with an iron and zinc bimetallic catalyst as described in any one of claims 1-2.

4. An application of the polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts as claimed in claim 3, characterized in that: Applied to degrade organic pollutants in water, the degradation method mainly includes the following steps: Fenton catalysis, photocatalysis and photo-Fenton catalysis were carried out on a polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts at 1-60°C, pH 2-10, different hydrogen peroxide concentrations, and with or without sunlight or ultraviolet light to generate strong oxidizing free radicals to oxidatively degrade organic pollutants in the wastewater. The molar ratio of hydrogen peroxide to organic pollutants was 1:1-150:

1.

5. An application of the polymer fiber catalytic membrane loaded with iron and zinc bimetallic catalysts as claimed in claim 3, characterized in that: The organic pollutant is at least one of dyes, phenols and their derivatives, antibiotics, environmental hormones and disinfection by-products, wherein the dye is selected from at least one of Congo red, rhodamine B, orange G and methylene blue, the phenols and their derivatives are selected from at least one of phenol, p-chlorophenol, p-nitrophenol, bisphenol A and 2-chlorophenol, the antibiotic is selected from at least one of ciprofloxacin, levofloxacin, sulfamethoxazole and clarithromycin, the environmental hormone is selected from at least one of cyanurate, soy isoflavones, estradiol, nitrotoluene and alkylphenols, and the disinfection by-product is at least one of chloroform, bromoform, formaldehyde and 2,4,6-trichlorophenol.