Cationic quaternary ammonium salt combined collecting agent for phosphorite reverse flotation desilicication and application of cationic quaternary ammonium salt combined collecting agent
Through the optimized design of combined collectors such as ester-based quaternary ammonium salts, the problems of foam overstability and slime sensitivity during the desilication process of phosphate ore reverse flotation have been solved, and efficient SiO2 removal and high-grade phosphate concentrate have been achieved. Production is suitable for a variety of phosphate rock properties and promotes the industrial application of phosphate rock flotation technology.
Patent Information
- Application Number
- CN202411056836.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-08-02
AI Technical Summary
Existing phosphate ore reverse flotation desilicon collectors have problems such as excessive foam stability, slime sensitivity, and poor selectivity. It is difficult to effectively separate silicate gangue minerals and phosphate ores, and single-component agents perform poorly under different ore properties. There are large differences and it is difficult to achieve industrial promotion.
Cationic quaternary ammonium salt collection prepared by a combination of ester quaternary ammonium salt, dodecyldimethylammonium chloride, tetradecyldimethylamine oxide, isodecyloxypropylamine, methyl oleate, and methanol Agent, by optimizing the proportion of ingredients, adjusting the pH value and reusing it to improve the collection effect.
It achieves the controllable stability and selective collection ability of foam, significantly improves the SiO2 removal rate, is suitable for different phosphate ore properties, reduces the dosage of chemicals, and meets the needs of high-grade and efficient desiliconization of phosphate concentrates.
Smart Images

Figure BDA0004976690540000061 
Figure BDA0004976690540000071 
Figure BDA0004976690540000081
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of phosphate ore flotation, and in particular to a cationic quaternary ammonium salt combined collector for reverse flotation desiliconization of phosphate ore and application thereof. Background Art
[0002] Phosphate ore is the material basis for the production of phosphoric acid, phosphate fertilizer, battery materials and other phosphorus-based chemical products. It plays an important role in the national economy and social development and is irreplaceable and non-renewable. There are a large number of silicate impurities such as quartz in silico-calcium phosphate ore. It is difficult to meet the requirements of downstream wet phosphoric acid production for phosphate concentrate by traditional single reverse flotation to remove carbonate. It is necessary to further adopt appropriate sorting methods to remove silicates.
[0003] In the phosphate ore flotation desiliconization process, direct flotation desiliconization has been industrialized, but the amount of collector used is large, the reagent system is complex, the fine tailings slurry is not easy to settle, and heated flotation is required when the ambient temperature is low, and the beneficiation cost is high. Compared with direct flotation, reverse flotation desiliconization process is simple, the amount of reagents used is small, it complies with the principle of "floating less and suppressing more", the temperature requirement is low, and the concentrate is easy to be processed later.
[0004] At present, the research on the desiliconization collector of phosphate ore reverse flotation in China is mainly based on fatty amines, ether amines and polyamines, but there are defects such as sensitivity to ore mud, large foam viscosity, poor selectivity and high reagent cost. Most of them remain in the laboratory research stage and are difficult to promote and apply. In recent years, the research on the application of quaternary ammonium salt cationic collectors in the desiliconization of phosphate ore reverse flotation has also been continuously concerned. For example, the CN 106238215A patent discloses a synthesis method of a novel quaternary ammonium salt cationic collector, but does not disclose the foam effect of actual application, and only involves a single actual mineral with a P2O5 grade of 23.46% and a SiO2 grade of 24%, and does not give the SiO2 index and removal effect of phosphate concentrate. CN 110721818A patent discloses a mixed formula collector of quaternary ammonium, fatty amine and etheramine for reverse flotation and desiliconization of magnesium-free phosphate concentrate, but the P2O5 grade of the phosphate concentrate after implementation and application is not more than 30%, which is still far from the superior product, and the key information of yield, recovery rate and SiO2 removal rate is not presented. CN 112474061A patent discloses a single-component ester-based quaternary ammonium salt cationic collector, which is limited to a Hubei silico-calcium phosphate ore in the embodiment, and the SiO2 optimal removal rate is only about 70%, and the collector dosage is larger than 1.0kg / t at this time. In addition, the properties of the same type of ores in various places are quite different, and the selective collection ability and foam stability of the single-component agent are bound to be quite different. The cases reflecting its universality should be presented as much as possible. In short, in the latest disclosed patent technology of cationic desiliconization collectors for reverse flotation of phosphate ore, there are few practical applications involving the combination of ester-based and hydroxyethyl quaternary ammonium salts and other synergists.
[0005] In the flotation practice, for the complex flotation system of silico-calcium phosphate ore rich in silicate gangue minerals, it is difficult to achieve a good separation effect by using a single collector, but the combination of collectors according to certain rules can often achieve unexpected results. Therefore, the development of a combination of collectors with a wide range of sources, excellent selective collection effect and controllable foam will be the key link for further reverse flotation of silico-calcium phosphate ore to remove silicon and extract phosphorus, and it is also an effective way to quickly realize the industrialization of phosphate ore flotation desiliconization. Summary of the invention
[0006] In view of this, the purpose of the present invention is to provide a cationic quaternary ammonium salt combination collector for reverse flotation desiliconization of phosphate ore and its application. The cationic quaternary ammonium salt combination collector provided by the present invention can solve the technical problems such as excessively stable foam viscosity and poor slime sensitivity and selectivity in the process of cationic reverse flotation desiliconization.
[0007] The invention provides a cationic quaternary ammonium salt combined collector, which contains the following components, measured by mass: 60-70 parts of ester quaternary ammonium salt, 15-20 parts of didodecyl dimethyl ammonium chloride, 3-5 parts of tetradecyl dimethyl amine oxide, 1-3 parts of isodecyloxypropylamine, 1-2 parts of methyl oleate and 10-15 parts of methanol.
[0008] Preferably, the ester-based quaternary ammonium salt is a mixture of mono-fatty acid ethyl ester-dihydroxyethyl methyl ammonium methyl sulfate and di-fatty acid ethyl ester-hydroxyethyl methyl ammonium methyl sulfate.
[0009] Preferably, the mass ratio of mono-fatty acid ethyl ester di-hydroxyethyl methyl ammonium methyl sulfate to di-fatty acid ethyl ester hydroxyethyl methyl ammonium methyl sulfate is 1:(1-10).
[0010] Preferably, the number of carbon atoms on the fatty acid carbon chain in the monoethyl fatty acid ester dihydroxyethyl methyl ammonium methyl sulfate and the diethyl fatty acid ester hydroxyethyl methyl ammonium methyl sulfate is 10-20.
[0011] Preferably, the mono-fatty acid ethyl ester dihydroxyethyl methyl ammonium methyl sulfate is one or more of ethyl laurate dihydroxyethyl methyl ammonium methyl sulfate, ethyl oleate dihydroxyethyl methyl ammonium methyl sulfate, ethyl palmitate dihydroxyethyl methyl ammonium methyl sulfate and ethyl stearate dihydroxyethyl methyl ammonium methyl sulfate.
[0012] Preferably, the bis-ethyl fatty acid ester hydroxyethyl methyl ammonium methyl sulfate is one or more of bis-ethyl laurate hydroxyethyl methyl ammonium methyl sulfate, bis-ethyl oleate hydroxyethyl methyl ammonium methyl sulfate, bis-ethyl palmitate hydroxyethyl methyl ammonium methyl sulfate and bis-ethyl stearate hydroxyethyl methyl ammonium methyl sulfate.
[0013] The present invention provides a method for reverse flotation desiliconization of phosphate ore, comprising the following steps:
[0014] a) adjusting the pH value of the phosphate concentrate slurry after magnesium removal to 6.5-8.5;
[0015] b) adding the cationic quaternary ammonium salt combined collector described in the above technical solution to the concentrate pulp treated in step a), and performing reverse flotation desiliconization to obtain a desiliconized phosphate concentrate pulp.
[0016] Preferably, in step a), the reagent used to adjust the pH value is one or more of lime, sodium hydroxide, sodium carbonate, sodium pyrophosphate and sodium citrate.
[0017] Preferably, in step b), the amount of the cationic quaternary ammonium salt combined collector is (100-400) g / t ore.
[0018] Preferably, the method further comprises: repeating step b) several times on the concentrate slurry treated in step b).
[0019] Compared with the prior art, the present invention provides a cationic quaternary ammonium salt combined collector for reverse flotation desiliconization of phosphate ore and its application. In parts by mass, the cationic quaternary ammonium salt combined collector provided by the present invention contains the following components: 60-70 parts of ester quaternary ammonium salt, 15-20 parts of didodecyl dimethyl ammonium chloride, 3-5 parts of tetradecyl dimethyl amine oxide, 1-3 parts of isodecyloxypropylamine, 1-2 parts of methyl oleate, and 10-15 parts of methanol. The present invention can solve the technical problems of high foam over-stability viscosity and poor ore slime sensitivity selectivity in the process of cationic reverse flotation desiliconization by optimizing the composition of the collector. DETAILED DESCRIPTION
[0020] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] The invention provides a cationic quaternary ammonium salt combined collector for reverse flotation desiliconization of phosphate ore. The cationic quaternary ammonium salt combined collector comprises the following components in parts by mass: 60-70 parts of ester-based quaternary ammonium salt, 15-20 parts of didodecyldimethylammonium chloride, 3-5 parts of tetradecyldimethylamine oxide, 1-3 parts of isodecyloxypropylamine, 1-2 parts of methyl oleate and 10-15 parts of methanol.
[0022] In the collector provided by the present invention, the ester-based quaternary ammonium salt is preferably a mixture of mono-ethyl fatty acid ester-based dihydroxyethyl methyl ammonium methyl sulfate and bis-ethyl fatty acid ester-based hydroxyethyl methyl ammonium methyl sulfate; the mass ratio of mono-ethyl fatty acid ester-based dihydroxyethyl methyl ammonium methyl sulfate to bis-ethyl fatty acid ester-based hydroxyethyl methyl ammonium methyl sulfate is preferably 1:(1-10), specifically 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9 or 1:10.
[0023] In the collector provided by the present invention, in the ester-based quaternary ammonium salt, the number of carbon atoms on the fatty acid carbon chain in the mono-fatty acid ethyl ester dihydroxyethyl methyl ammonium methyl sulfate and the di-fatty acid ethyl ester hydroxyethyl methyl ammonium methyl sulfate is preferably 10 to 20, specifically 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20.
[0024] In the collector provided by the present invention, in the ester-based quaternary ammonium salt, the mono-fatty acid ethyl ester-based dihydroxyethyl methyl ammonium methyl sulfate is preferably one or more of ethyl laurate-based dihydroxyethyl methyl ammonium methyl sulfate, ethyl oleate-based dihydroxyethyl methyl ammonium methyl sulfate, ethyl palmitate-based dihydroxyethyl methyl ammonium methyl sulfate and ethyl stearate-based dihydroxyethyl methyl ammonium methyl sulfate; the bis-fatty acid ethyl ester-based hydroxyethyl methyl ammonium methyl sulfate is preferably one or more of ethyl dilaurate-based hydroxyethyl methyl ammonium methyl sulfate, ethyl dioleate-based hydroxyethyl methyl ammonium methyl sulfate, ethyl dipalmitate-based hydroxyethyl methyl ammonium methyl sulfate and ethyl distearyl hydroxyethyl methyl ammonium methyl sulfate.
[0025] In the collector provided by the present invention, the content of the ester quaternary ammonium salt can be 60 parts, 61 parts, 62 parts, 63 parts, 64 parts, 65 parts, 66 parts, 67 parts, 68 parts, 69 parts or 70 parts by mass.
[0026] In the collector provided by the present invention, the content of the didodecyl dimethyl ammonium chloride can be 15 parts, 15.5 parts, 16 parts, 16.5 parts, 17 parts, 17.5 parts, 18 parts, 18.5 parts, 19 parts, 19.5 parts or 20 parts by mass.
[0027] In the collector provided by the present invention, the content of the tetradecyl dimethyl amine oxide can be 3 parts, 3.1 parts, 3.2 parts, 3.3 parts, 3.4 parts, 3.5 parts, 3.6 parts, 3.7 parts, 3.8 parts, 3.9 parts, 4 parts, 4.1 parts, 4.2 parts, 4.3 parts, 4.4 parts, 4.5 parts, 4.6 parts, 4.7 parts, 4.8 parts, 4.9 parts or 5 parts by mass.
[0028] In the collector provided by the present invention, the content of the isodecyloxypropylamine can be specifically 1 part, 1.1 parts, 1.2 parts, 1.3 parts, 1.4 parts, 1.5 parts, 1.6 parts, 1.7 parts, 1.8 parts, 1.9 parts, 2 parts, 2.1 parts, 2.2 parts, 2.3 parts, 2.4 parts, 2.5 parts, 2.6 parts, 2.7 parts, 2.8 parts, 2.9 parts or 3 parts by mass.
[0029] In the collector provided by the present invention, the content of methyl oleate can be 1 part, 1.1 parts, 1.2 parts, 1.3 parts, 1.4 parts, 1.5 parts, 1.6 parts, 1.7 parts, 1.8 parts, 1.9 parts or 2 parts by mass.
[0030] In the collector provided by the present invention, the content of methanol can be 10 parts, 10.5 parts, 11 parts, 11.5 parts, 12 parts, 12.5 parts, 13 parts, 13.5 parts, 14 parts, 14.5 parts or 15 parts by mass.
[0031] The present invention also provides a method for reverse flotation desiliconization of phosphate ore, comprising the following steps:
[0032] a) adjusting the pH value of the phosphate concentrate slurry after magnesium removal to 6.5-8.5;
[0033] b) adding the cationic quaternary ammonium salt combined collector described in the above technical solution to the concentrate pulp treated in step a), and performing reverse flotation desiliconization to obtain a desiliconized phosphate concentrate pulp.
[0034] In the method provided by the present invention, in step a), the phosphate concentrate slurry after magnesium removal is preferably obtained by reverse flotation magnesium removal from silico-calcium phosphate ore; the number of reverse flotation magnesium removal is preferably multiple times, that is, the phosphate concentrate slurry after magnesium removal is subjected to reverse flotation magnesium removal several times; the number of reverse flotation magnesium removal can specifically be 2 to 3 times.
[0035] In the method provided by the present invention, in step a), the reagent used to adjust the pH value is one or more of lime, sodium hydroxide, sodium carbonate, sodium pyrophosphate and sodium citrate.
[0036] In the method provided by the present invention, in step a), the pH value can be specifically adjusted to 6.5, 6.6, 6.7, 6.8, 6.9, 7, 7.1, 7.2, 7.3, 7.4, 7.5, 7.6, 7.7, 7.8, 7.9, 8, 8.1, 8.2, 8.3, 8.4 or 8.5.
[0037] In the method provided by the present invention, in step b), the amount of the cationic quaternary ammonium salt combination collector is preferably (100-400) g / t ore, specifically 100 g / t ore, 120 g / t ore, 150 g / t ore, 170 g / t ore, 200 g / t ore, 230 g / t ore, 250 g / t ore, 270 g / t ore, 300 g / t ore, 320 g / t ore, 350 g / t ore, 370 g / t ore or 400 g / t ore.
[0038] In the method provided by the present invention, in step b), the cationic quaternary ammonium salt combination collector is preferably added to the ore pulp in the form of an aqueous solution; the concentration of the aqueous solution is preferably 1 to 5wt%, specifically 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt% or 5wt%.
[0039] The method provided by the present invention preferably further comprises: repeating step b) several times, specifically 2 to 5 times, on the concentrate slurry treated in step b). In the present invention, during the process of repeating step b), the operating conditions each time can be the same or different.
[0040] The technical solution provided by the present invention can solve the technical problems such as excessively stable foam viscosity and poor selectivity of ore slime in the process of cationic reverse flotation desiliconization by optimizing the composition of the collector. More specifically, the technical solution of the present invention has the following beneficial effects:
[0041] 1. The cationic quaternary ammonium salt combined collector of the present invention is prepared by mixing ester-based quaternary ammonium salt, didodecyl dimethyl ammonium chloride, tetradecyl dimethyl amine oxide, isodecyloxypropylamine, methyl oleate and methanol as raw materials. The raw materials are widely available and can be directly dissolved in water without adding auxiliary solvents such as acetic acid or hydrochloric acid, and the method of use is simple.
[0042] 2. The cationic quaternary ammonium salt combined collector prepared by the present invention can exert the synergistic effect of various functional groups, effectively alleviate the excessive stability of foam caused by the sensitivity of mineral mud, and realize the effective controllability of desiliconization foam.
[0043] 3. The cationic quaternary ammonium salt combined collector prepared by the present invention has a strong selective collection ability, can efficiently separate silicate gangue minerals from phosphate rock, and has a significant SiO2 removal effect.
[0044] 4. The cationic quaternary ammonium salt combined collector formula provided by the present invention has no toxic side effects, is easily degradable, and does not pollute the environment.
[0045] For the purpose of greater clarity, the invention is described in detail through the following examples.
[0046] The raw materials and instrument information used in the following examples are shown in Table 1.
[0047] Table 1
[0048]
[0049] Example 1
[0050] The cationic quaternary ammonium salt combined collector for reverse flotation desiliconization of phosphate ore of this embodiment contains the following components by mass: ester quaternary ammonium salt: 65 parts; didodecyl dimethyl ammonium chloride: 20 parts; tetradecyl dimethyl amine oxide: 3 parts; isodecyloxypropylamine: 1 part; methyl oleate: 1 part; methanol: 10 parts. The ester quaternary ammonium salt is composed of laurate ethyl dihydroxyethyl methyl ammonium methyl sulfate and dilaurate ethyl hydroxyethyl methyl ammonium methyl sulfate in a mass ratio of 1:1.
[0051] After all the above raw materials are mixed in proportion, they are added into water at room temperature to prepare a 1 wt % aqueous solution which is directly used as a reverse flotation desiliconizing collector.
[0052] For a low-grade calcium-silicon phosphate ore in Fuquan, Guizhou, the P2O5 grade of the demagnesium concentrate obtained after two anion reverse flotation was 19.72%, the MgO content was 0.85%, and the SiO2 content was 44.26%. When the cationic reverse flotation was used for desiliconization, the pH value of the demagnesium concentrate slurry was first adjusted to 6.5 with sodium carbonate, and the combined collector of the present invention was added with 250g / t ore for the first roughing desiliconization, and 150g / t ore for the second time. After two roughing desiliconizations, a P2O5 grade of 35.16%, a MgO content of 0.99%, a SiO2 content of 6.06%, and a SiO2 removal rate of 94.17% can be obtained. The specific index analysis results are shown in Table 2 below.
[0053] Table 2
[0054]
[0055] Example 2
[0056] The cationic quaternary ammonium salt combined collector for reverse flotation desiliconization of phosphate ore of this embodiment contains the following components by mass: ester quaternary ammonium salt: 65 parts; didodecyl dimethyl ammonium chloride: 15 parts; tetradecyl dimethyl amine oxide: 5 parts; isodecyloxypropylamine: 2 parts; methyl oleate: 2 parts; methanol: 11 parts. Among them, the ester quaternary ammonium salt is composed of oleyl ethyl dihydroxyethyl methyl ammonium methyl sulfate and dioleyl ethyl hydroxyethyl methyl ammonium methyl sulfate in a mass ratio of 1:5.
[0057] After all the above raw materials are mixed in proportion, they are added into water at room temperature to prepare a 2 wt % aqueous solution which is directly used as a reverse flotation desiliconizing collector.
[0058] For a medium-low grade calcium-silicon phosphate ore in Weng'an, Guizhou, the demagnesium concentrate obtained after anion reverse flotation has a P2O5 grade of 25.70%, a MgO content of 0.86%, and a SiO2 content of 28.86%. The cationic reverse flotation desiliconization is carried out four times. Before desiliconization, the pH value of the demagnesium concentrate slurry is adjusted to 7.0 with lime. Each time the combined collector of the present invention is added for roughing desiliconization, 200g / t ore is added. After four roughings, a P2O5 grade of 35.82%, a MgO content of 0.75%, a SiO2 content of 5.68%, and a SiO2 removal rate of 89.93% can be obtained. The specific index analysis results are shown in Table 3 below.
[0059] Table 3
[0060]
[0061] Example 3
[0062] The cationic quaternary ammonium salt combined collector for reverse flotation desiliconization of phosphate ore of this embodiment contains the following components by mass: ester quaternary ammonium salt: 70 parts; didodecyl dimethyl ammonium chloride: 15 parts; tetradecyl dimethyl amine oxide: 3 parts; isodecyloxypropylamine: 1 part; methyl oleate: 1 part; methanol: 10 parts. The ester quaternary ammonium salt is composed of ethyl palmitate dihydroxyethyl methyl ammonium methyl sulfate and ethyl dipalmitate hydroxyethyl methyl ammonium methyl sulfate in a mass ratio of 1:10.
[0063] After all the above raw materials are mixed in proportion, they are added into water at room temperature to prepare a 5wt% aqueous solution which is directly used as a reverse flotation desiliconizing collector.
[0064] For a fine-grained high-grade calcium-silicon phosphate ore in Kaiyang, Guizhou, the P2O5 grade of the demagnesium concentrate obtained after an anion reverse flotation was 30.04%, the MgO content was 1.16%, and the SiO2 content was 13.62%. The cationic reverse flotation desiliconization was carried out five times. Before desiliconization, the pH value of the demagnesium concentrate slurry was adjusted to 7.5 with sodium pyrophosphate. Each time the combined collector of the present invention was added for roughing desiliconization, 200g / t of ore was added. After five roughings, a P2O5 grade of 35.53%, a MgO content of 0.91%, a SiO2 content of 5.88%, and a SiO2 removal rate of 72.52% were obtained. The specific index analysis results are shown in Table 4 below.
[0065] Table 4
[0066]
[0067] From Examples 1 to 3, it can be seen that the cationic quaternary ammonium salt combined collector of the present invention can obtain excellent mineral processing indicators when flotating silicon-calcium phosphate ore, with P2O5 grades greater than 34%, MgO contents less than 1%, P2O5 recovery rates and SiO2 removal rates both above 70%, and reaching the index requirements of wet-process phosphoric acid superior grade I phosphate concentrate. At the same time, it can also be seen that the collector of the present invention has low reagent dosage when used for high-silicon demagnesium concentrate, and has good adaptability to the separation of low-grade phosphate ore with multiple impurity components.
[0068] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A cationic quaternary ammonium salt combined collector for reverse flotation desiliconization of phosphate ore, characterized in that: The invention comprises the following components in parts by mass: 60-70 parts of ester quaternary ammonium salt, 15-20 parts of didodecyldimethylammonium chloride, 3-5 parts of tetradecyldimethylamine oxide, 1-3 parts of isodecyloxypropylamine, 1-2 parts of methyl oleate and 10-15 parts of methanol.
2. The cationic quaternary ammonium salt combined collector according to claim 1, characterized in that: The ester-based quaternary ammonium salt is a mixture of mono-fatty acid ethyl ester-based dihydroxyethyl methyl ammonium methyl sulfate and di-fatty acid ethyl ester-based hydroxyethyl methyl ammonium methyl sulfate.
3. The cationic quaternary ammonium salt combined collector according to claim 2, characterized in that: The mass ratio of the mono-ethyl fatty acid ester-based di-hydroxyethyl methyl ammonium methyl sulfate to the di-ethyl fatty acid ester-based hydroxyethyl methyl ammonium methyl sulfate is 1:(1-10).
4. The cationic quaternary ammonium salt combined collector according to claim 2, characterized in that: The carbon number of the fatty acid carbon chain in the mono-ethyl fatty acid ester di-hydroxyethyl methyl ammonium methyl sulfate and the di-ethyl fatty acid ester hydroxyethyl methyl ammonium methyl sulfate is 10 to 20.
5. The cationic quaternary ammonium salt combined collector according to claim 4, characterized in that: The mono-fatty acid ethyl ester dihydroxyethyl methyl ammonium methyl sulfate is one or more of ethyl laurate dihydroxyethyl methyl ammonium methyl sulfate, ethyl oleate dihydroxyethyl methyl ammonium methyl sulfate, ethyl palmitate dihydroxyethyl methyl ammonium methyl sulfate and ethyl stearate dihydroxyethyl methyl ammonium methyl sulfate.
6. The cationic quaternary ammonium salt combined collector according to claim 4, characterized in that: The bis-ethyl fatty acid ester hydroxyethyl methyl ammonium methyl sulfate is one or more of bis-ethyl laurate hydroxyethyl methyl ammonium methyl sulfate, bis-ethyl oleate hydroxyethyl methyl ammonium methyl sulfate, bis-ethyl palmitate hydroxyethyl methyl ammonium methyl sulfate and bis-ethyl stearate hydroxyethyl methyl ammonium methyl sulfate.
7. A method for reverse flotation desiliconization of phosphate ore, characterized in that: The following steps are involved: a) adjusting the pH value of the phosphate concentrate slurry after magnesium removal to 6.5-8.5; b) adding the cationic quaternary ammonium salt combined collector according to any one of claims 1 to 6 to the concentrate pulp treated in step a), and performing reverse flotation desiliconization to obtain a desiliconized phosphate concentrate pulp.
8. The method according to claim 7, characterized in that In step a), the reagent used to adjust the pH value is one or more of lime, sodium hydroxide, sodium carbonate, sodium pyrophosphate and sodium citrate.
9. The method according to claim 7, characterized in that: In step b), the dosage of the cationic quaternary ammonium salt combined collector is (100-400) g / t ore.
10. The method according to claim 7, characterized in that Also includes: The concentrate slurry that has completed the treatment in step b) is subjected to step b) for several times.
Citation Information
Patent Citations
Collophane quaternary ammonium salt cationic collector, synthesis method and application of collophane quaternary ammonium salt cationic collector
CN106238215A
Collecting agent for reverse flotation and re-desilicication of magnesium-removed phosphate concentrate
CN110721818A
Ester group-containing quaternary ammonium salt cation collecting agent and preparation method and application thereof
CN112474061A
Cited By
A preparation method and application of functional fatty acid
CN119751354A