A cationic quaternary ammonium salt combined collector for reverse flotation desilication of phosphate rock and its application
By optimizing the design of combined collectors such as ester-based quaternary ammonium salts, the problems of excessive foam stability and mud sensitivity in phosphate rock reverse flotation were solved, achieving efficient separation of silicate gangue minerals and phosphate rock, reducing beneficiation costs and reagent usage, and meeting the requirements of phosphoric acid production.
Patent Information
- Application Number
- CN202411056836.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-08-02
AI Technical Summary
In existing reverse flotation desilication technology for phosphate rock, the amount of collector used is large, the reagent system is complex, the fine-particle tailings slurry is not easy to settle, heated flotation is required when the ambient temperature is low, the beneficiation cost is high, and a single collector is sensitive to slime and has poor selectivity, making it difficult to achieve efficient separation of silicate gangue minerals and phosphate rock.
A cationic quaternary ammonium salt combined collector, consisting of ester-based quaternary ammonium salt, dodecyl dimethyl ammonium chloride, tetradecyl dimethylamine oxide, isodexyloxypropylamine, methyl oleate, and methanol, was used to optimize the composition of the collector by adjusting the pH of the phosphate rock concentrate slurry and performing reverse flotation, thereby solving the problems of excessive foam stability and mud sensitivity.
It achieves effective control of foam, improves selective collection ability, significantly reduces SiO2 removal rate, meets the requirements of wet phosphoric acid production for phosphate concentrate, uses less reagent, and is environmentally friendly.
Smart Images

Figure BDA0004976690540000061 
Figure BDA0004976690540000071 
Figure BDA0004976690540000081
Abstract
Description
Technical Field
[0001] This invention relates to the field of phosphate rock flotation technology, and in particular to a cationic quaternary ammonium salt combined collector for reverse flotation desilication of phosphate rock and its application. Background Technology
[0002] Phosphate rock is the material basis for producing various phosphorus-based chemical products such as phosphoric acid, phosphate fertilizers, and battery materials. It occupies an important position and plays a vital role in national economic and social development, and is irreplaceable and non-renewable. Silicate phosphate rock contains a large amount of silicate impurities such as quartz. Traditional single reverse flotation for carbonate removal is insufficient to meet the requirements of downstream wet-process phosphoric acid production for phosphate concentrate. Therefore, further appropriate separation methods are needed to remove silicates.
[0003] In the desilication process of phosphate rock flotation, direct flotation has been industrialized, but it requires a large amount of collector, has a complex reagent system, and the fine-particle tailings slurry is difficult to settle. It also requires heated flotation at low ambient temperatures, resulting in high beneficiation costs. Compared to direct flotation, reverse flotation is simpler, uses less reagent, conforms to the principle of "less flotation, more suppression," has lower temperature requirements, and the concentrate is easier to process further.
[0004] Currently, domestic research on desilication collectors for phosphate rock reverse flotation mainly focuses on aliphatic amines, ether amines, and polyamines. However, these methods suffer from drawbacks such as sensitivity to slime, high foam viscosity, poor selectivity, and high reagent costs, and are mostly confined to the laboratory research stage, making widespread application difficult. In recent years, research on the application of quaternary ammonium salt cationic collectors in phosphate rock reverse flotation desilication has also received continuous attention. For example, patent CN 106238215A discloses a synthesis method for a novel quaternary ammonium salt cationic collector, but it does not disclose the foaming effect in actual application, and it only involves a single actual mineral with a P2O5 grade of 23.46% and a SiO2 grade of 24%, and it does not provide the SiO2 index and removal effect of the phosphate concentrate. Patent CN 110721818A discloses a mixed-formulation collector for desilication of magnesium-phosphate concentrate via reverse flotation, containing quaternary ammonium, fatty amine, and ether amine. However, after implementation, the P2O5 grade of the phosphate concentrate never exceeded 30%, falling short of superior grades, and key information regarding yield, recovery rate, and SiO2 removal rate was not presented. Patent CN 112474061A discloses a single-component ester-based quaternary ammonium salt cationic collector, but the examples only cover one type of Hubei siliceous-calcareous phosphate ore, and the optimal SiO2 removal rate was only around 70%, requiring a collector dosage exceeding 1.0 kg / t. Furthermore, the properties of similar ores vary significantly across regions, inevitably leading to substantial differences in the selective collecting ability and foam stability of single-component agents. Examples demonstrating universality should be presented as much as possible. In short, among the latest publicly disclosed patents for phosphate ore reverse flotation cationic desilication collectors, few involve practical applications involving the combined use of ester-based and hydroxyethyl quaternary ammonium salts with other synergists.
[0005] In flotation practice, for complex flotation systems of siliceous calcareous phosphate rock rich in silicate gangue minerals, using a single collector is often insufficient to achieve good separation results. However, combining collectors according to certain rules can often yield unexpected results. Therefore, developing a combination of collectors that are widely available, have excellent selective collecting effects, and allow for controllable froth is a key step in further reverse flotation desiliconization and phosphorus extraction of siliceous calcareous phosphate rock, and also an effective way to rapidly realize the industrialization of phosphate rock flotation desilication. Summary of the Invention
[0006] In view of this, the purpose of this invention is to provide a cationic quaternary ammonium salt combined collector for desilication of phosphate rock by reverse flotation and its application. The cationic quaternary ammonium salt combined collector provided by this invention can solve technical problems such as excessively stable foam viscosity and poor selectivity of slime during cationic reverse flotation desilication.
[0007] This invention provides a cationic quaternary ammonium salt combination collector, which contains the following components by weight: 60-70 parts of ester-based quaternary ammonium salt, 15-20 parts of dodecyl dimethyl ammonium chloride, 3-5 parts of tetradecyl dimethylamine oxide, 1-3 parts of isodexyloxypropylamine, 1-2 parts of methyl oleate, and 10-15 parts of methanol.
[0008] Preferably, the ester-based quaternary ammonium salt is a mixture of mono-fatty acid ethyl ester-based dihydroxyethyl methyl sulfate methyl ammonium and di-fatty acid ethyl ester-based hydroxyethyl methyl sulfate methyl ammonium.
[0009] Preferably, the mass ratio of mono-fatty acid ethyl ester-based dihydroxyethyl methyl sulfate ammonium to di-fatty acid ethyl ester-based hydroxyethyl methyl sulfate ammonium is 1:(1-10).
[0010] Preferably, the number of carbon atoms in the fatty acid carbon chain of both mono-fatty acid ethyl ester-based dihydroxyethyl methyl sulfate ammonium and di-fatty acid ethyl ester-based hydroxyethyl methyl sulfate ammonium is 10 to 20.
[0011] Preferably, the monofatty acid ethyl ester dihydroxyethyl methyl sulfate ammonium is one or more of ethyl laurate dihydroxyethyl methyl sulfate ammonium, ethyl oleate dihydroxyethyl methyl sulfate ammonium, ethyl palmitate dihydroxyethyl methyl sulfate ammonium, and ethyl stearate dihydroxyethyl methyl sulfate ammonium.
[0012] Preferably, the difatty acid ethyl hydroxyethyl methyl sulfate ammonium is one or more of dilaurate ethyl hydroxyethyl methyl sulfate ammonium, dioleate ethyl hydroxyethyl methyl sulfate ammonium, bispalmitate ethyl hydroxyethyl methyl sulfate ammonium, and distearate ethyl hydroxyethyl methyl sulfate ammonium.
[0013] This invention provides a method for desilication of phosphate rock by reverse flotation, comprising the following steps:
[0014] a) Adjust the pH of the demagnesified phosphate rock concentrate slurry to 6.5–8.5;
[0015] b) Add the cationic quaternary ammonium salt combined collector described in the above technical solution to the concentrate slurry after step a), and perform reverse flotation desilication to obtain desilicationized phosphate rock concentrate slurry.
[0016] Preferably, in step a), the reagent used to adjust the pH value is one or more of lime, sodium hydroxide, sodium carbonate, sodium pyrophosphate, and sodium citrate.
[0017] Preferably, in step b), the amount of the cationic quaternary ammonium salt combined collector is (100-400) g / t ore.
[0018] Preferably, it further includes: repeating step b) several times with the concentrate slurry that has been processed in step b).
[0019] Compared with existing technologies, this invention provides a cationic quaternary ammonium salt combined collector for desilication of phosphate rock via reverse flotation and its application. By weight, the cationic quaternary ammonium salt combined collector provided by this invention contains the following components: 60-70 parts of ester-based quaternary ammonium salt, 15-20 parts of dodecyl dimethyl ammonium chloride, 3-5 parts of tetradecyl dimethylamine oxide, 1-3 parts of isodexyloxypropylamine, 1-2 parts of methyl oleate, and 10-15 parts of methanol. This invention, through optimized design of the collector's composition, can solve technical problems such as excessively stable foam viscosity and poor selectivity in cationic reverse flotation desilication, particularly regarding slime sensitivity. Detailed Implementation
[0020] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0021] This invention provides a cationic quaternary ammonium salt combined collector for reverse flotation desilication of phosphate rock, which contains the following components by mass: 60-70 parts of ester-based quaternary ammonium salt, 15-20 parts of dodecyl dimethyl ammonium chloride, 3-5 parts of tetradecyl dimethylamine oxide, 1-3 parts of isodexyloxypropylamine, 1-2 parts of methyl oleate, and 10-15 parts of methanol.
[0022] In the collector provided by the present invention, the ester-based quaternary ammonium salt is preferably a mixture of monofatty acid ethyl ester dihydroxyethyl methyl sulfate ammonium and difatty acid ethyl ester hydroxyethyl methyl sulfate ammonium; the mass ratio of monofatty acid ethyl ester dihydroxyethyl methyl sulfate ammonium to difatty acid ethyl ester hydroxyethyl methyl sulfate ammonium is preferably 1:(1-10), specifically 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9 or 1:10.
[0023] In the collector provided by the present invention, the number of carbon atoms on the fatty acid carbon chain of the mono-fatty acid ethyl ester-dihydroxyethyl methyl sulfate ammonium salt and the di-fatty acid ethyl ester-hydroxyethyl methyl sulfate ammonium salt is preferably 10 to 20, specifically 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 or 20.
[0024] In the collector provided by the present invention, the ester-based quaternary ammonium salt, wherein the monofatty acid ethyl ester-based dihydroxyethyl methyl sulfate ammonium is preferably one or more of ethyl laurate-based dihydroxyethyl methyl sulfate ammonium, ethyl oleate-based dihydroxyethyl methyl sulfate ammonium, ethyl palmitate-based dihydroxyethyl methyl sulfate ammonium, and ethyl stearate-based dihydroxyethyl methyl sulfate ammonium; wherein the difatty acid ethyl ester-based hydroxyethyl methyl sulfate ammonium is preferably one or more of dilaurate-based hydroxyethyl methyl sulfate ammonium, dioleate-based hydroxyethyl methyl sulfate ammonium, dipalmitate-based hydroxyethyl methyl sulfate ammonium, and distearate-based hydroxyethyl methyl sulfate ammonium.
[0025] In the collector provided by the present invention, the content of the ester-based quaternary ammonium salt, by mass, can be 60 parts, 61 parts, 62 parts, 63 parts, 64 parts, 65 parts, 66 parts, 67 parts, 68 parts, 69 parts, or 70 parts.
[0026] In the collector provided by the present invention, the content of the didodecyl dimethyl ammonium chloride, by weight, can be 15 parts, 15.5 parts, 16 parts, 16.5 parts, 17 parts, 17.5 parts, 18 parts, 18.5 parts, 19 parts, 19.5 parts, or 20 parts.
[0027] In the collector provided by the present invention, the content of tetradecyl dimethylamine oxide, by weight, can specifically be 3 parts, 3.1 parts, 3.2 parts, 3.3 parts, 3.4 parts, 3.5 parts, 3.6 parts, 3.7 parts, 3.8 parts, 3.9 parts, 4 parts, 4.1 parts, 4.2 parts, 4.3 parts, 4.4 parts, 4.5 parts, 4.6 parts, 4.7 parts, 4.8 parts, 4.9 parts, or 5 parts.
[0028] In the collector provided by the present invention, the content of isodexylpropylamine, by weight, can be 1 part, 1.1 parts, 1.2 parts, 1.3 parts, 1.4 parts, 1.5 parts, 1.6 parts, 1.7 parts, 1.8 parts, 1.9 parts, 2 parts, 2.1 parts, 2.2 parts, 2.3 parts, 2.4 parts, 2.5 parts, 2.6 parts, 2.7 parts, 2.8 parts, 2.9 parts, or 3 parts.
[0029] In the collector provided by the present invention, the content of methyl oleate, by mass, can be 1 part, 1.1 parts, 1.2 parts, 1.3 parts, 1.4 parts, 1.5 parts, 1.6 parts, 1.7 parts, 1.8 parts, 1.9 parts, or 2 parts.
[0030] In the collector provided by the present invention, the content of methanol, by mass, can be 10 parts, 10.5 parts, 11 parts, 11.5 parts, 12 parts, 12.5 parts, 13 parts, 13.5 parts, 14 parts, 14.5 parts, or 15 parts.
[0031] This invention also provides a method for desilication of phosphate rock by reverse flotation, comprising the following steps:
[0032] a) Adjust the pH of the demagnesified phosphate rock concentrate slurry to 6.5–8.5;
[0033] b) Add the cationic quaternary ammonium salt combined collector described in the above technical solution to the concentrate slurry after step a), and perform reverse flotation desilication to obtain desilicationized phosphate rock concentrate slurry.
[0034] In the method provided by the present invention, in step a), the demagnesified phosphate rock concentrate slurry is preferably obtained by reverse flotation demagnesification of siliceous calcium phosphate rock; the reverse flotation demagnesification is preferably performed multiple times, that is, the demagnesified phosphate rock concentrate slurry is subjected to reverse flotation demagnesification several times; the reverse flotation demagnesification is specifically performed 2 to 3 times.
[0035] In the method provided by the present invention, in step a), the reagent used to adjust the pH value is one or more of lime, sodium hydroxide, sodium carbonate, sodium pyrophosphate, and sodium citrate.
[0036] In the method provided by the present invention, in step a), the pH value can be specifically adjusted to 6.5, 6.6, 6.7, 6.8, 6.9, 7, 7.1, 7.2, 7.3, 7.4, 7.5, 7.6, 7.7, 7.8, 7.9, 8, 8.1, 8.2, 8.3, 8.4 or 8.5.
[0037] In the method provided by the present invention, in step b), the amount of the cationic quaternary ammonium salt combined collector is preferably (100-400) g / t ore, specifically 100 g / t ore, 120 g / t ore, 150 g / t ore, 170 g / t ore, 200 g / t ore, 230 g / t ore, 250 g / t ore, 270 g / t ore, 300 g / t ore, 320 g / t ore, 350 g / t ore, 370 g / t ore or 400 g / t ore.
[0038] In the method provided by the present invention, in step b), the cationic quaternary ammonium salt combined collector is preferably added to the slurry in the form of an aqueous solution; the concentration of the aqueous solution is preferably 1 to 5 wt%, specifically 1 wt%, 1.5 wt%, 2 wt%, 2.5 wt%, 3 wt%, 3.5 wt%, 4 wt%, 4.5 wt%, or 5 wt%.
[0039] In the method provided by the present invention, it is preferable to further include: repeating step b) of the concentrate slurry after the treatment in step b) several times, specifically 2 to 5 times. In the present invention, the operating conditions can be the same or different each time step b) is repeated.
[0040] The technical solution provided by this invention, through optimized design of the collector's composition, can solve technical problems such as excessively stable and high-viscosity foam, and poor selectivity due to mud sensitivity during cation reverse flotation desilication. More specifically, the technical solution of this invention has the following beneficial effects:
[0041] 1. The cationic quaternary ammonium salt combination collector of the present invention is made by mixing ester-based quaternary ammonium salt, dodecyl dimethyl ammonium chloride, tetradecyl dimethylamine oxide, isodexyloxypropylamine, methyl oleate and methanol as raw materials. The raw materials are widely available and can be directly dissolved in water without the need to add co-solvents such as acetic acid or hydrochloric acid. The method of use is simple.
[0042] 2. The cationic quaternary ammonium salt combined collector prepared by this invention can exert the synergistic effect of various functional groups, effectively alleviate the over-stability of foam caused by the sensitivity of sludge, and achieve effective and controllable desilication foam.
[0043] 3. The cationic quaternary ammonium salt combined collector prepared by this invention has strong selective collecting ability, can efficiently separate silicate gangue minerals from phosphate rock, and has a significant SiO2 removal effect.
[0044] 4. The cationic quaternary ammonium salt combined collector formulation provided by this invention has no toxic side effects, is easily degradable, and will not cause pollution to the environment.
[0045] For clarity, the following examples will be used to provide a detailed description.
[0046] The information on raw materials and instruments used in the following examples is shown in Table 1 below.
[0047] Table 1
[0048]
[0049] Example 1
[0050] The cationic quaternary ammonium salt combined collector for reverse flotation desilication of phosphate rock in this embodiment contains the following components by weight: ester-based quaternary ammonium salt: 65 parts; didodecyl dimethyl ammonium chloride: 20 parts; tetradecyl dimethylamine oxide: 3 parts; isodexoxypropylamine: 1 part; methyl oleate: 1 part; methanol: 10 parts. The ester-based quaternary ammonium salt is composed of ethyl laurate-dihydroxyethyl methyl sulfate ammonium and diethyl laurate-dihydroxyethyl methyl sulfate ammonium in a 1:1 weight ratio.
[0051] After mixing all the above raw materials in the specified proportions, add them to water at room temperature to prepare a 1wt% aqueous solution, which can be used directly as a reverse flotation desilication collector.
[0052] For a low-grade siliceous calcium phosphate ore from Fuquan, Guizhou, the demagnesified concentrate obtained after two anion reverse flotation processes had a P2O5 grade of 19.72%, MgO content of 0.85%, and SiO2 content of 44.26%. During cationic reverse flotation desilication, the pH of the demagnesified concentrate slurry was first adjusted to 6.5 with sodium carbonate. In the first roughing desilication, 250 g / t of the combined collector of this invention was added, and in the second, 150 g / t of ore was added. After two roughing desilication processes, a P2O5 grade of 35.16%, MgO content of 0.99%, and SiO2 content of 6.06% were obtained, with a SiO2 removal rate of 94.17%. Specific index analysis results are shown in Table 2 below.
[0053] Table 2
[0054]
[0055] Example 2
[0056] The cationic quaternary ammonium salt combined collector for reverse flotation desilication of phosphate rock in this embodiment contains the following components by weight: ester-based quaternary ammonium salt: 65 parts; didodecyl dimethyl ammonium chloride: 15 parts; tetradecyl dimethylamine oxide: 5 parts; isodexyloxypropylamine: 2 parts; methyl oleate: 2 parts; methanol: 11 parts. The ester-based quaternary ammonium salt is composed of ethyl oleate-based dihydroxyethyl methyl sulfate ammonium and diethyl oleate-based dihydroxyethyl methyl sulfate ammonium in a mass ratio of 1:5.
[0057] After mixing all the above raw materials in the specified proportions, add them to water at room temperature to prepare a 2wt% aqueous solution, which can be used directly as a reverse flotation desilication collector.
[0058] For a medium-low grade siliceous-calcium phosphate ore from Weng'an County, Guizhou Province, the demagnesified concentrate obtained after one anion reverse flotation had a P2O5 grade of 25.70%, MgO content of 0.86%, and SiO2 content of 28.86%. Cationic reverse flotation was then performed four times for desilication. Before desilication, the pH of the demagnesified concentrate slurry was adjusted to 7.0 with lime. Each roughing desilication stage involved adding 200 g / t of the combined collector of this invention. After four roughing stages, a P2O5 grade of 35.82%, MgO content of 0.75%, and SiO2 content of 5.68% were obtained, with a SiO2 removal rate of 89.93%. Specific index analysis results are shown in Table 3 below.
[0059] Table 3
[0060]
[0061] Example 3
[0062] The cationic quaternary ammonium salt combined collector for reverse flotation desilication of phosphate rock in this embodiment contains the following components by weight: ester-based quaternary ammonium salt: 70 parts; dodecyl dimethyl ammonium chloride: 15 parts; tetradecyl dimethylamine oxide: 3 parts; isodexyloxypropylamine: 1 part; methyl oleate: 1 part; methanol: 10 parts. The ester-based quaternary ammonium salt is composed of ethyl palmitate-based dihydroxyethyl methyl sulfate ammonium and ethyl palmitate-based dihydroxyethyl methyl sulfate ammonium in a mass ratio of 1:10.
[0063] After mixing all the above raw materials in the specified proportions, add them to water at room temperature to prepare a 5wt% aqueous solution, which can be used directly as a reverse flotation desilication collector.
[0064] For a fine-grained, high-grade siliceous-calcium phosphate ore from Kaiyang, Guizhou, the demagnesified concentrate obtained after one anion reverse flotation had a P2O5 grade of 30.04%, MgO content of 1.16%, and SiO2 content of 13.62%. Cationic reverse flotation was then performed five times for desilication. Before desilication, the pH of the demagnesified concentrate slurry was adjusted to 7.5 with sodium pyrophosphate. Each roughing desilication stage involved adding 200 g / t of the combined collector of this invention. After five roughing stages, a P2O5 grade of 35.53%, MgO content of 0.91%, and SiO2 content of 5.88% were obtained, with a SiO2 removal rate of 72.52%. Specific index analysis results are shown in Table 4 below.
[0065] Table 4
[0066]
[0067] As demonstrated in Examples 1-3, the cationic quaternary ammonium salt combined collector of the present invention achieves excellent beneficiation indicators in the flotation of silica-calcium phosphate rock. The P2O5 grade is greater than 34%, the MgO content is less than 1%, and the P2O5 recovery and SiO2 removal rates are both above 70%, meeting the requirements for Class I superior grade phosphate concentrate produced by wet-process phosphate flotation. Furthermore, the collector of the present invention requires low reagent dosage when used with high-silica magnesium-removed concentrates and exhibits good adaptability to the beneficiation of low-grade phosphate rock with multiple impurities.
[0068] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A cationic quaternary ammonium salt combined collector for desilication of phosphate rock by reverse flotation, characterized in that, By weight, it contains the following components: 60-70 parts of ester-based quaternary ammonium salt, 15-20 parts of dodecyl dimethyl ammonium chloride, 3-5 parts of tetradecyl dimethylamine oxide, 1-3 parts of isodexyloxypropylamine, 1-2 parts of methyl oleate, and 10-15 parts of methanol.
2. The cationic quaternary ammonium salt combined collector according to claim 1, characterized in that, The ester-based quaternary ammonium salt is a mixture of mono-fatty acid ethyl ester-based dihydroxyethyl methyl sulfate methyl ammonium and di-fatty acid ethyl ester-based hydroxyethyl methyl sulfate methyl ammonium.
3. The cationic quaternary ammonium salt combined collector according to claim 2, characterized in that, The mass ratio of mono-fatty acid ethyl ester-based dihydroxyethyl methyl sulfate ammonium to di-fatty acid ethyl ester-based hydroxyethyl methyl sulfate ammonium is 1:(1-10).
4. The cationic quaternary ammonium salt combined collector according to claim 2, characterized in that, The number of carbon atoms in the fatty acid carbon chain of both mono-fatty acid ethyl ester-based dihydroxyethyl methyl sulfate ammonium and di-fatty acid ethyl ester-based hydroxyethyl methyl sulfate ammonium is 10 to 20.
5. The cationic quaternary ammonium salt combined collector according to claim 4, characterized in that, The monofatty acid ethyl ester dihydroxyethyl methyl sulfate ammonium is one or more of ethyl laurate dihydroxyethyl methyl sulfate ammonium, ethyl oleate dihydroxyethyl methyl sulfate ammonium, ethyl palmitate dihydroxyethyl methyl sulfate ammonium, and ethyl stearate dihydroxyethyl methyl sulfate ammonium.
6. The cationic quaternary ammonium salt combined collector according to claim 4, characterized in that, The difatty acid ethyl ester-based hydroxyethyl methyl sulfate ammonium is one or more of dilaurate ethyl ester-based hydroxyethyl methyl sulfate ammonium, dioleate ethyl ester-based hydroxyethyl methyl sulfate ammonium, bispalmitate ethyl methyl sulfate ammonium, and distearate ethyl ester-based hydroxyethyl methyl sulfate ammonium.
7. A method for desilication of phosphate rock by reverse flotation, characterized in that, Includes the following steps: a) Adjust the pH of the demagnesified phosphate rock concentrate slurry to 6.5–8.5; b) Add the cationic quaternary ammonium salt combined collector according to any one of claims 1 to 6 to the concentrate slurry treated in step a), and perform reverse flotation desilication to obtain desilicationized phosphate rock concentrate slurry.
8. The method according to claim 7, characterized in that, In step a), the reagent used to adjust the pH value is one or more of lime, sodium hydroxide, sodium carbonate, sodium pyrophosphate, and sodium citrate.
9. The method according to claim 7, characterized in that, In step b), the amount of the cationic quaternary ammonium salt combined collector is (100-400) g / t ore.
10. The method according to claim 7, characterized in that, Also includes: Repeat step b) several times with the concentrate slurry that has been processed in step b).
Citation Information
Patent Citations
Collophane quaternary ammonium salt cationic collector, synthesis method and application of collophane quaternary ammonium salt cationic collector
CN106238215A
Collecting agent for reverse flotation and re-desilicication of magnesium-removed phosphate concentrate
CN110721818A
Ester group-containing quaternary ammonium salt cation collecting agent and preparation method and application thereof
CN112474061A
Silicon-calcium phosphate ore reverse flotation, desilicification and decontamination combined collector, and preparation method and application thereof
CN110152889A
Collecting agent for reverse flotation desilicication of clay type lithium ore as well as preparation method and application of collecting agent