High-speed laser-assisted rolling equipment and method for manufacturing dissimilar metal foil strip
The copper/aluminum composite foil strip is pretreated and rolled by high-speed laser-assisted rolling equipment, which solves the problems of compounding difficulty and high energy consumption in the traditional process, and realizes efficient and low-cost copper/aluminum composite foil strip production.
Patent Information
- Application Number
- CN202411024734.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-01
AI Technical Summary
The process of manufacturing copper/aluminum composite foil strips in the existing technology has problems such as difficulty in compounding, low strength of the joint surface, low efficiency, and high energy consumption. In particular, the traditional rolling process has high equipment requirements and is not conducive to mass production.
High-speed laser-assisted rolling equipment and methods are used to pre-treat dissimilar metal foil strips, including pickling, water washing, drying, high-speed laser etching and heating, to improve the bonding strength of the materials, and perform asynchronous rolling in the rolling mill , reduce rolling force and energy consumption.
It achieves safe, efficient and easy-to-operate dissimilar metal foil strip rolling, improves the joint surface strength and production efficiency, reduces costs, and is suitable for large-scale industrial production.
Smart Images

Figure CN118719803A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of metal composite foil manufacturing, and more particularly to a high-speed laser-assisted rolling device and method for manufacturing heterogeneous metal foil strips. Background Art
[0002] Since the 1990s, with the increasing shortage of nonferrous metal resources, the price of copper has risen sharply, resulting in a significant increase in the production and use costs of copper manufacturers and customers. Therefore, on the basis of ensuring the performance of the original copper materials, the development of new materials to replace traditional materials has become a hot spot for research and development of domestic and foreign manufacturers. The use of alternative composite materials to reduce raw material costs has become a development trend in the production and application of copper materials at home and abroad.
[0003] Copper has good electrical conductivity and welding performance, but its resources are scarce and its processing is expensive; aluminum has good electrical conductivity and is relatively cheap, but aluminum's welding, arc extinguishing, wear resistance, electrical conductivity, and thermal conductivity are all worse than copper. In many cases, it is difficult to directly replace copper with aluminum. The foil formed by copper and aluminum composite can not only save the consumption of copper, but also maintain the advantages of pure copper materials such as ductility, conductivity, weldability, and corrosion resistance. In addition, my country's aluminum resources are very rich, and the price of aluminum is lower than that of copper. Its density is less than 1 / 3 of that of copper, which means that under the same weight, the length of aluminum is 3 times that of pure copper. Especially in the field of communications, the frequency of cable TV signals and mobile communication signals is relatively high, generally at 500-800MHz. Due to the "skin effect", the high-frequency current is concentrated on the surface of the conductor for transmission. When pure copper is used for information transmission, the copper in the center does not play the main role of transmitting signals. Therefore, using aluminum to partially replace the copper in the middle layer is a very ideal method, which can greatly save my country's relatively scarce and expensive copper resources. In fact, copper / aluminum has a wide range of application prospects in the fields of power transmission, electronic chips, etc., not only in the field of communications, and is expected to form a huge industry. The development of high-efficiency, low-energy composite technology suitable for industrial-scale production and the manufacture of new copper / aluminum composite belt materials will undoubtedly provide ideal new products for my country's rapidly developing electronics, power, machinery manufacturing and other industrial fields, and generate significant economic benefits.
[0004] Due to the large difference in melting points between copper and aluminum, the casting process is very demanding. At present, the explosion composite method or rolling composite method is mostly used. The working principle of the explosion composite method is to use the huge energy generated by the explosion of explosives to composite the plates, but it is dangerous, noisy, and difficult to store explosives. Secondly, the thickness of aluminum foil and copper foil is small. Using the explosion composite method for composite is not only difficult to complete the composite, but also easy to cause the foil to break. Therefore, the rolling composite method has become the only choice for manufacturing copper / aluminum composite foil.
[0005] Traditional rolling composite method can be divided into rolling composite method and hot rolling composite method. The rolling composite method needs to control the reduction rate to more than 50% to achieve effective bonding, which has high requirements for the rolling mill, and the foil strip is severely hardened, and subsequent heat treatment is required for practical engineering application. The hot rolling composite method requires the foil strip to be heated to above the recrystallization temperature for rolling, which not only consumes a lot of energy, but also has poor surface quality after hot rolling, and needs further rolling; Chinese invention patent 2017105726013 discloses a multi-layer rolling composite foil process and requires a deformation rate of more than 60% during the composite process. In order to ensure that the substrate and the covering material are mechanically interlocked with each other, the rolling force and reduction rate acting on them must be large enough and required to be completed at one time; at the same time, it is required to have a certain holding time during rolling, that is, the rolling speed shall not exceed 60 meters / minute, to avoid deformation rebound due to short interaction time, and reduce the bonding rate of the substrate and the covering material; the low rolling speed of this scheme is not conducive to large-scale production, and post-rolling heat treatment is required to further deepen the bonding degree of the materials. Chinese invention patent 2019113123587 discloses a method and device for pulse current assisted rolling of double-layer metal composite plates. This method uses a mechanical method to grind and fix the surface to achieve plate pre-treatment, which is not conducive to large-scale production of composite plates and strips. In addition, the use of pulse current for assisted rolling requires modification of the rollers and the installation of an insulating layer on the surface, which is difficult to implement and has a high risk factor.
[0006] Therefore, it is an urgent problem for technical personnel in this field to provide a dissimilar metal foil rolling device and method with high safety factor, high efficiency, simple operation and strong bonding surface. Summary of the invention
[0007] In view of this, the present invention provides a high-speed laser-assisted rolling device and method for manufacturing heterogeneous metal foil strips, which solves the problems of difficulty in composite double-layer metal foils, low bonding surface strength, low efficiency, and high energy consumption in traditional rolling processes.
[0008] In order to achieve the above-mentioned object, the present invention provides a high-speed laser-assisted rolling equipment for manufacturing heterogeneous metal foil strips, comprising: a heterogeneous metal foil strip pretreatment device, and a rolling mill and a coiler sequentially connected to the heterogeneous metal foil strip pretreatment device;
[0009] The heterogeneous metal foil strip pretreatment device comprises a plurality of single metal foil strip pretreatment devices arranged in parallel, and the function is to pretreatment different types of metal foils independently;
[0010] The single metal foil strip pretreatment device comprises: a metal foil strip coil, and a pickling tank, a water washing tank, a drying area, a high-speed laser etching device and a high-speed laser heating device which are sequentially connected to the metal foil strip coil;
[0011] The high-speed laser etching device and the high-speed laser heating device are arranged on one side of the surface to be combined with the metal foil strip.
[0012] Preferably, the number of the single metal foil strip pretreatment devices is two or three.
[0013] The pickling tank is sequentially provided with an acetone containing chamber and an acid containing chamber.
[0014] The pickling tank and the water washing tank are both made of double-layer materials, the inner layer is nylon material with a thickness of 10mm; the outer layer is stainless steel with a thickness of 3mm.
[0015] The beneficial effects are: the inner layer of nylon material has good corrosion resistance and hardly reacts with acid. At the same time, in order to prevent the nylon material from being damaged due to external force, a stainless steel shell is surrounded on the outer layer of the nylon material.
[0016] The high-speed laser heating device is a multi-channel high-speed laser heating device, which is composed of a box, a strip-shaped laser head, a type I fine-tuning device, and a type II fine-tuning device.
[0017] The I-type fine-tuning device includes a laser head fixture, a fine-tuning screw, a bearing, and a fixed seat; the fixed seat is fixed on the inner wall of the box body, the fine-tuning screw and the fixed seat are matched by threads, the other end of the screw is connected to the bearing, the outer ring of the bearing is matched with the laser head fixture, and the laser head fixture is connected to the laser head.
[0018] The type II fine-tuning device includes a laser head fixture, a fine-tuning lead screw, a bearing, and a fixed seat. One end of the fixed seat is connected to the strip laser head, the fine-tuning lead screw and the fixed seat are threaded, the other end of the lead screw is connected to the bearing, the outer ring of the bearing is matched with the laser head fixture, and the laser head fixture is connected to the laser head.
[0019] The beneficial effects are: the type I fine-tuning device can adjust the distance between the laser head and the box by rotating the lead screw; the type II fine-tuning device can adjust the position relationship between the laser heads by rotating the lead screw
[0020] The metal foil strip pretreatment device also includes a second guide roller, a third guide roller, a fourth guide roller, a fifth guide roller, and a seventh guide roller;
[0021] The second guide roller is located between the metal strip coil and the pickling tank; the third guide roller is located between the pickling tank and the water washing tank; the fourth guide roller is located between the water washing tank and the drying area; the fifth guide roller is located between the drying area and the high-speed laser etching device; the seventh guide rail is located between the high-speed laser etching device and the high-speed laser heating device.
[0022] The metal foil strip pretreatment device also includes a first guide roller and a sixth guide roller;
[0023] The first guide roller is located between the metal strip coil and the second guide roller; the sixth guide roller is located between the fifth guide roller and the high-speed laser etching device.
[0024] The beneficial effect is that the foil strip is guided layer by layer by the guide rollers to approach and enter the rolling mill, thereby avoiding bending and breaking of the foil strip during the rolling process, which affects the product quality.
[0025] In addition, the present invention also provides a method for high-speed laser-assisted rolling of heterogeneous metal foil strips, using the above-mentioned equipment, specifically comprising the following steps:
[0026] S1, selecting heterogeneous metal foil strips to be compounded, and installing the heterogeneous metal foil strip rolls on different single metal foil strip pretreatment devices respectively;
[0027] S2, the parallel single metal foil strip pretreatment devices are started simultaneously, and the metal foil strips are independently put into the pickling tank from the metal foil strip coils, and are successively washed with acetone and pickled to remove oil stains and oxide scale on the surface of the metal foil strips;
[0028] S3, then enters the water washing tank to remove the acid residue on the surface of the metal foil;
[0029] S4, then enter the drying area to dry the surface moisture of the metal foil strip;
[0030] S5, then entering the high-speed laser etching device, etching the surfaces of the metal foil strips to be bonded by high-speed laser respectively;
[0031] The beneficial effect is that the high-speed laser etching device is used to etch the interface to be composited, so that the materials can be better mechanically bonded and the bonding strength of the bonding surface can be increased. The etching power can be selected according to the different metal foils to be composited. When the thickness of the foil is about 0.001-0.15mm, the power of the high-speed laser is generally between 1-100W to prevent the foil from being penetrated due to excessive laser power, resulting in a decrease in the yield rate of the foil.
[0032] S6, then entering the high-speed laser heating device, heating the surfaces of the metal foil strips to be bonded by high-speed laser respectively;
[0033] The beneficial effects are: the heating temperature can be selected according to the different metal foils to be composited, and the foils are heated by laser, with short heating time and high efficiency, which effectively inhibits the formation of oxide scale on the foil surface. At the same time, the high energy consumption of overall heating during hot rolling composite process is avoided, and by adjusting the power and relative position of the laser head, better metallurgical bonding is promoted during the composite process of dissimilar metals, and the bonding strength of the metal interface is improved.
[0034] S7, placing the surfaces of the dissimilar metal foil strips to be bonded opposite to each other, and rolling them in a rolling mill to achieve bonding of the dissimilar metal foil strips to obtain the dissimilar metal foil strips;
[0035] Asynchronous rolling is preferably used. During the rolling process of asynchronous rolling, the metal is subjected to significant friction and shearing, which intensifies the longitudinal flow of the material. It is widely used in difficult-to-deform metals and can also be used to manufacture ultrafine-grained metal materials, thereby improving the mechanical properties of the materials.
[0036] In addition, when rolling multiple layers of metal foil strips, due to the large differences in deformation resistance and elongation, the rolling composite is prone to deformation inconsistency, and the bonding layer is prone to produce residual shear stress, which destroys the bonding of the metal interface. Therefore, the diameter ratio or speed ratio of the rolling rollers is determined according to the properties of the composite material to be composited.
[0037] S8, finally the composited heterogeneous metal foil strip is rolled into a coil by a coiler and stored in a warehouse.
[0038] The heterogeneous metal foils in S1 are preferably copper foils and aluminum foils.
[0039] The etching depth in S5 cannot exceed 30% of the total thickness.
[0040] It can be seen from the above technical solution that compared with the prior art:
[0041] The present invention uses high-speed laser to etch and heat different metal foils respectively, thus avoiding the poor heating effect of the foils due to large difference in melting points of the foils, the sticking of the roller due to too high heating temperature, or the low strength of the bonding surface due to too low heating temperature.
[0042] The manufacturing process of the present invention has fewer steps, a short process, low energy consumption, good surface quality, smaller required rolling force, and low requirements on rolling mill performance. It can be directly applied to the composite production of foil strips in a workshop, and does not require large-scale changes to existing rolling mills. It has strong practicality and low modification cost, and can effectively improve production efficiency and reduce costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0044] Figure 1 Overall diagram of high-speed laser-assisted rolling equipment for double-layer metal foil strips
[0045] Dissimilar metal foil strip pretreatment device 1, single metal foil strip pretreatment device 1a, single metal foil strip pretreatment device 1b, rolling mill 2, coiler 3, metal foil strip roll 4, first guide roller 5, second guide roller 6, pickling tank 7, third guide roller 8, water washing tank 9, fourth guide roller 10, drying area 11, fifth guide roller 12, high-speed laser etching device 13, sixth guide roller 14, seventh guide roller 15, high-speed laser heating device 16.
[0046] Figure 2 Overall picture of high-speed laser-assisted rolling equipment for three-layer metal foil strips
[0047] Dissimilar metal foil strip pretreatment device 1, single metal foil strip pretreatment device 1a, single metal foil strip pretreatment device 1b, single metal foil strip pretreatment device 1c, rolling mill 2, coiler 3, metal foil strip roll 4, first guide roller 5, second guide roller 6, pickling tank 7, third guide roller 8, water washing tank 9, fourth guide roller 10, drying area 11, fifth guide roller 12, high-speed laser etching device 13, sixth guide roller 14, seventh guide roller 15, high-speed laser heating device 16.
[0048] Figure 3 Schematic diagram of pickling tank structure
[0049] Stainless steel layer 17 , nylon layer 18 , metal foil inlet 19 , metal foil outlet 20 , acetone containing chamber 21 , acid containing chamber 22 , first type I guide 23 , second type I guide roller 24 , third type I guide roller 25 .
[0050] Figure 4 Schematic diagram of the high-speed laser heating device
[0051] Box body 26, type I fine-tuning device 27, strip laser head 28, type II fine-tuning device 29.
[0052] Figure 5 Type I fine-tuning device
[0053] Laser head fixture 30 , fine-tuning screw 31 , bearing 32 , and fixing seat 33 .
[0054] Figure 6 Type II fine-tuning device
[0055] Laser head fixture 34 , fine-tuning screw 35 , bearing 36 , and fixing seat 37 .
[0056] Figure 7 Copper / aluminum foil composite process diagram
[0057] Figure 8 Flow chart of high-speed laser-assisted rolling of double-layer metal foil strip DETAILED DESCRIPTION
[0058] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0059] Example 1
[0060] High-speed laser-assisted rolling equipment for double-layer heterogeneous metal foil strips
[0061] like Figure 1 As shown, it includes: a heterogeneous metal foil strip pretreatment device 1, which is composed of a single metal foil strip pretreatment device 1a and a single metal foil strip pretreatment device 1b arranged in parallel; the ends of the heterogeneous metal foil strip pretreatment device are connected to a rolling mill and a coiler in sequence.
[0062] The single metal foil strip pretreatment device is composed of a metal foil strip roll 4, a first guide roller 5, a second guide roller 6, a pickling tank 7, a third guide roller 8, a water washing tank 9, a fourth guide roller 10, a drying area 11, a fifth guide roller 12, a high-speed laser etching device 13, a sixth guide roller 14, a seventh guide roller 15, and a high-speed laser heating device 16.
[0063] The pickling tank structure is as follows Figure 3 As shown, it is a double-layer box structure, the outer layer is a stainless steel layer 17, and the inner layer is a nylon layer 18; the box is provided with a metal foil inlet 19 and a metal foil outlet 20; an acetone containing chamber 21 and an acid containing chamber 22 are provided inside the box, which contain acetone and acid; a first type I guide roller 23, a second type I guide roller 24, and a third type I guide roller 25 are also provided to drive the metal foil to pass through the acetone containing chamber 21 and the acid containing chamber 22 in sequence.
[0064] The structure of high-speed laser etching device is as follows Figure 4 The device comprises a box 26 , a type I fine-tuning device 27 , a strip laser head 28 , and a type II fine-tuning device 29 .
[0065] like Figure 5 As shown, the I-type fine-tuning device includes a laser head fixture 30, a fine-tuning lead screw 31, a bearing 32, and a fixed seat 33. The fixed seat 33 is fixed on the inner wall of the box body 26. The fine-tuning lead screw 31 and the fixed seat 33 are matched by threads. The other end of the lead screw 31 is connected to the bearing 32. The outer ring of the bearing is matched with the laser head fixture 30. The laser head fixture 30 is connected to the laser head. The distance between the laser head and the box body 26 is adjusted by rotating the fine-tuning lead screw 31.
[0066] like Figure 6As shown, the type II fine-tuning device includes a laser head fixture 34, a fine-tuning screw 35, a bearing 36, and a fixed seat 37. One end of the fixed seat 37 is connected to the strip laser head, the fine-tuning screw 35 and the fixed seat 37 are matched with each other by threads, the other end of the fine-tuning screw 35 is connected to the bearing 36, the outer ring of the bearing 36 is matched with the laser head fixture 34, the laser head fixture 34 is connected to the laser head, and the positional relationship between the laser heads is adjusted by rotating the fine-tuning screw 35.
[0067] Example 2
[0068] High-speed laser-assisted rolling equipment for three-layer heterogeneous metal foil strips
[0069] like Figure 2 As shown, a metal foil pretreatment device 1c is added to the equipment described in Example 1, and the metal foil pretreatment device 1c is arranged in parallel with the metal foil pretreatment device 1a and the metal foil pretreatment device 1b; the metal foil pretreatment device 1c comprises in sequence: a metal foil roll 4, a second guide roller 6, a pickling tank 7, a third guide roller 8, a water washing tank 9, a fourth guide roller 10, a drying area 11, a fifth guide roller 12, two high-speed laser heating devices 13, a seventh guide roller 15, and two high-speed laser etching devices 16.
[0070] Example 3
[0071] A high-speed laser-assisted rolling method for copper-aluminum composite metal foil strip is carried out using the equipment in Example 1.
[0072] S1, installing the copper foil roll and the aluminum foil roll on different single metal foil pretreatment devices respectively;
[0073] S2, simultaneously starting the parallel single metal foil strip pretreatment devices, the copper foil strip and the aluminum foil strip are independently put into the pickling tank from the metal foil strip roll, and are successively washed with acetone and pickled to remove the oil stains and oxide scale on the surface of the copper foil strip and the aluminum foil strip;
[0074] The thickness ratio of the aluminum foil strip to the copper foil strip is 5:1, the aluminum foil strip is pickled using a hydrofluoric acid solution with a volume fraction of 15%, and the copper foil strip is pickled using a hydrochloric acid solution with a volume fraction of 12%;
[0075] S3, then enters the water washing tank to remove the acid residue on the surface of the copper foil and aluminum foil;
[0076] S4, then enter the drying area to dry the surface moisture of the copper foil and aluminum foil;
[0077] S5, then entering the high-speed laser etching device, etching the surfaces of the copper foil strip and the aluminum foil strip to be combined respectively by high-speed laser;
[0078] The high-speed laser etching power of the aluminum foil strip is 10W, and the high-speed laser etching power of the copper foil strip is 8W;
[0079] S6, then entering the high-speed laser heating device, heating the surfaces of the copper foil strip and the aluminum foil strip to be bonded respectively by high-speed laser;
[0080] The heating temperature of the copper foil strip is 450°C, and the heating temperature of the aluminum foil strip is 380°C.
[0081] S7, placing the surfaces of the copper foil strip and the aluminum foil strip to be bonded opposite to each other, and rolling them in a rolling mill to achieve bonding of the copper foil strip and the aluminum foil strip, thereby obtaining the copper-aluminum composite metal foil strip, i.e., the heterogeneous metal foil strip;
[0082] S8, finally the copper-aluminum composite metal foil strip is rolled into a coil by a coiler and stored in a warehouse.
[0083] The peeling test of the rolled composite foil showed an average bonding strength of 37.12N*mm. -1 The average bonding strength of conventional cold-rolled copper-aluminum composite foil is 30.08N*mm -1 Compared with the cold rolling composite method, the bonding strength of this application is increased by 25%.
[0084] Figure 7 This is a diagram of the copper / aluminum foil composite process. As can be seen from the figure, the present application first etches the pre-treated foil surface, and many etching pits appear on the surface. It is then heated again and rolled. When rolling begins, the etching pits on the surface of the foil to be combined begin to combine, and mechanical bonding occurs. Due to the high rolling temperature, metallurgical bonding occurs in the foil in the later stage of the rolling process, and the bonding strength is further increased, and the rolling is completed.
[0085] Example 4
[0086] A high-speed laser-assisted rolling method for copper-aluminum composite metal foil strip is carried out using the equipment in Example 1.
[0087] S1, installing the copper foil roll and the aluminum foil roll on different single metal foil pretreatment devices respectively;
[0088] S2, the parallel single metal foil strip pretreatment devices are started simultaneously, and the copper foil strip and the aluminum foil strip are independently put into the pickling tank from the metal foil strip roll, and are successively washed with acetone and pickled to remove the oil and oxide scale on the surface of the copper foil strip and the aluminum foil strip;
[0089] The thickness ratio of the aluminum foil strip to the copper foil strip is 5:1, the aluminum foil strip is pickled using a hydrofluoric acid solution with a volume fraction of 15%, and the copper foil strip is pickled using a hydrochloric acid solution with a volume fraction of 12%;
[0090] S3, then enters the water washing tank to remove the acid residue on the surface of the copper foil and aluminum foil;
[0091] S4, then enter the drying area to dry the surface moisture of the copper foil and aluminum foil;
[0092] S5, then entering the high-speed laser etching device, etching the surfaces of the copper foil strip and the aluminum foil strip to be combined respectively by high-speed laser;
[0093] The high-speed laser etching power of the aluminum foil strip is 0W, and the high-speed laser etching power of the copper foil strip is 8W;
[0094] S6, then entering the high-speed laser heating device, heating the surfaces of the copper foil strip and the aluminum foil strip to be bonded respectively by high-speed laser;
[0095] The heating temperature of the copper foil strip is 450°C, and the heating temperature of the aluminum foil strip is 380°C.
[0096] S7, placing the surfaces of the copper foil strip and the aluminum foil strip to be bonded opposite to each other, and rolling them in a rolling mill to achieve bonding of the copper foil strip and the aluminum foil strip, thereby obtaining the copper-aluminum composite metal foil strip, i.e., the heterogeneous metal foil strip;
[0097] S8, finally the copper-aluminum composite metal foil strip is rolled into a coil by a coiler and stored in a warehouse.
[0098] In this embodiment, only the copper foil is etched. Since copper is harder than aluminum, under the action of rolling force, the aluminum in the aluminum foil is squeezed into the etching pits of the copper foil to complete the mechanical bonding. Before rolling, the laser heats the foil surface to above the recrystallization temperature. As the rolling process continues, the composite layer enters the metallurgical composite stage until the rolling is completed.
[0099] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.
[0100] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A high-speed laser-assisted rolling equipment for manufacturing heterogeneous metal foil strips, It is characterized in that include: A heterogeneous metal foil strip pretreatment device, and a rolling mill and a coiler sequentially connected to the heterogeneous metal foil strip pretreatment device; The heterogeneous metal foil strip pretreatment device comprises a plurality of single metal foil strip pretreatment devices arranged in parallel, and the function is to pretreatment different types of metal foils independently; The single metal foil strip pretreatment device comprises: a metal foil strip coil, and a pickling tank, a water washing tank, a drying area, a high-speed laser etching device and a high-speed laser heating device which are sequentially connected to the metal foil strip coil; The high-speed laser etching device and the high-speed laser heating device are arranged on one side of the surface to be combined with the metal foil strip.
2. The high-speed laser-assisted rolling equipment for manufacturing heterogeneous metal foil strips according to claim 1, It is characterized in that The single metal foil strip pretreatment device is arranged in two or three.
3. The high-speed laser-assisted rolling equipment for manufacturing heterogeneous metal foil strips according to claim 1, It is characterized in that The pickling tank is sequentially provided with an acetone containing chamber and an acid containing chamber.
4. The high-speed laser-assisted rolling equipment for manufacturing heterogeneous metal foil strips according to claim 1, It is characterized in that The pickling tank and the water washing tank are both made of double-layer materials; the inner layer is nylon material with a thickness of 10 mm; the outer layer is a stainless steel layer with a thickness of 3 mm.
5. The high-speed laser-assisted rolling equipment for manufacturing heterogeneous metal foil strips according to claim 1, It is characterized in that The high-speed laser heating device is a multi-channel high-speed laser heating device, which is composed of a box, a strip-shaped laser head, a type I fine-tuning device, and a type II fine-tuning device. The I-type fine-tuning device includes a laser head fixture, a fine-tuning screw, a bearing, and a fixed seat; the fixed seat is fixed on the inner wall of the box body, the fine-tuning screw and the fixed seat are matched by threads, the other end of the screw is connected to the bearing, the outer ring of the bearing is matched with the laser head fixture, and the laser head fixture is connected to the laser head. The type II fine-tuning device includes a laser head fixture, a fine-tuning lead screw, a bearing, and a fixed seat. One end of the fixed seat is connected to the strip laser head, the fine-tuning lead screw and the fixed seat are threaded, the other end of the lead screw is connected to the bearing, the outer ring of the bearing is matched with the laser head fixture, and the laser head fixture is connected to the laser head.
6. The high-speed laser-assisted rolling equipment for manufacturing heterogeneous metal foil strips according to claim 1, It is characterized in that The single metal foil strip pretreatment device further comprises a second guide roller, a third guide roller, a fourth guide roller, a fifth guide roller, and a seventh guide roller; The second guide roller is located between the metal strip coil and the pickling tank; the third guide roller is located between the pickling tank and the water washing tank; the fourth guide roller is located between the water washing tank and the drying area; the fifth guide roller is located between the drying area and the high-speed laser etching device; the seventh guide rail is located between the high-speed laser etching device and the high-speed laser heating device.
7. The high-speed laser-assisted rolling equipment for manufacturing heterogeneous metal foil strips according to claim 6, It is characterized in that The single metal foil strip pretreatment device also includes a first guide roller and a sixth guide roller; The first guide roller is located between the metal strip coil and the second guide roller; the sixth guide roller is located between the fifth guide roller and the high-speed laser etching device.
8. A high-speed laser-assisted rolling method for manufacturing heterogeneous metal foil strips, It is characterized in that The device according to any one of claims 1 to 7 is used, and specifically comprises the following steps: S1, selecting heterogeneous metal foil strips to be compounded, and installing the heterogeneous metal foil strip rolls on different single metal foil strip pretreatment devices respectively; S2, the parallel single metal foil strip pretreatment devices are started simultaneously, and the metal foil strips are independently put into the pickling tank from the metal foil strip coils, and are successively washed with acetone and pickled to remove oil stains and oxide scale on the surface of the metal foil strips; S3, then enters the water washing tank to remove the acid residue on the surface of the metal foil; S4, then enter the drying area to dry the surface moisture of the metal foil strip; S5, then entering the high-speed laser etching device, etching the surfaces of the metal foil strips to be bonded by high-speed laser respectively; S6, then entering the high-speed laser heating device, heating the surfaces of the metal foil strips to be bonded by high-speed laser respectively; S7, placing the surfaces of the dissimilar metal foil strips to be bonded opposite to each other, and rolling them in a rolling mill to achieve bonding of the dissimilar metal foil strips to obtain the dissimilar metal foil strips; S8, finally the composited heterogeneous metal foil strip is rolled into a coil by a coiler and stored in a warehouse.
9. A method for high-speed laser-assisted rolling of heterogeneous metal foil strips according to claim 8, It is characterized in that S1 The heterogeneous metal foil strips are preferably copper foil strips and aluminum foil strips.
10. A method for high-speed laser-assisted rolling of heterogeneous metal foil strips according to claim 8, It is characterized in that The etching depth in S5 cannot exceed 30% of the total thickness.
Citation Information
Patent Citations
Method for preparing dry bonded structure surface through direct metal laser ablation
CN108620740A
Method of adopting multi-roll mill to roll three-layer composite extremely thin belt
CN111702008A
Device and method for synergistically preparing dissimilar metal composite plate strip through composite energy field
CN117680487A
Laser-assisted dissimilar metal cast rolling device and method based on bionic interlocking
CN117943400A
Ultrasonic cleaning device for magnesium alloy foil strip surface treatment
CN118268393A