Non-standard lead-antimony alloy electrode outer circle machining method for electroplating equipment and cutter

By using horizontal lathes and high-speed steel tools in electroplating equipment, combined with low rotational speed and low feed speed, and using petroleum and ethanol cutting fluids, the problem of difficulty in machining the outer circle of non-standard lead-antimony alloy electrodes and material deflection and tearing is solved , achieving efficient and stable processing processes and high-quality products.

CN118720184APending Publication Date: 2024-10-01SHAANXI WEIHE TOOLS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410780525.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

It is difficult to process the outer circle of non-standard lead-antimony alloy electrodes, and defects such as material deflection and tearing are prone to occur.

Method used

A horizontal lathe is used for processing, using a three-jaw chuck and a rotary top to support the workpiece at both ends, with low rotation speed and low feed speed, using high-speed steel 75° hand-grinding tools, and using liquids containing petroleum and ethanol as cutting fluids.

Benefits of technology

It improves processing accuracy and efficiency, avoids material deflection and tearing, reduces surface roughness and cutting force, and significantly improves product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118720184A_ABST
    Figure CN118720184A_ABST
Patent Text Reader

Abstract

The invention provides a non-standard lead-antimony alloy electrode outer circle machining method for electroplating equipment and a tool. A horizontal lathe is adopted in the machining method. Supporting the non-standard lead-antimony alloy electrode by using a three-jaw chuck of a lathe and double ends of a live center; the feeding speed is low through low rotating speed; a 75-degree hand sharpening cutter made of high-speed steel is used; the outer circle of the non-standard lead-antimony alloy electrode workpiece is processed by a method of selecting a liquid containing petroleum and ethanol as a basic liquid as a cutting fluid. The technical problems that in the prior art, the machining difficulty of the outer circle of a non-standard lead-antimony alloy electrode is large, and the defects of material deflection, tearing and the like occur in the machining process are solved; when the non-standard lead-antimony alloy electrode is machined, the conditions of rigid deformation, tearing and the like of a lead-antimony alloy workpiece can be effectively avoided, and the product quality of the non-standard lead-antimony alloy electrode is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of mechanical processing of operating and transporting rotary surfaces, and specifically relates to a processing method and a tool for processing the outer circle of a non-standard lead-antimony alloy electrode for electroplating equipment on a lathe. Background Art

[0002] Lead-antimony alloy is an alloy material made of lead and antimony, usually containing 70% to 85% lead and 15% to 30% antimony. This alloy has low melting point, high density, good corrosion resistance, electrical conductivity and unique physical properties. For example, the hardness of lead-antimony alloy is usually between 60 and 70 HB, and the melting point is usually between 183° and 327°. Lead-antimony alloy is mainly used in the manufacture of radiation protection materials, storage tanks in the chemical industry, aerospace, and positive and negative electrodes of electroplating equipment.

[0003] In electroplating equipment, due to the diversity of electroplating products and the special nature of the equipment, the external dimensions of lead-antimony alloy electrodes change. The production of lead-antimony alloy electrodes is mainly based on a variety of process methods such as casting, forging, rolling, and drawing. However, due to the limitations of molds and the high manufacturing cost, it is impossible to cover all lead-antimony alloy electrode products. Therefore, in order to produce non-standard lead-antimony alloy electrode products, the outer circle of the electrode can only be processed by casting the blank and using traditional mechanical processing methods. However, due to the special physical and chemical properties of non-standard lead-antimony alloy electrode materials, the processing difficulty increases; during the processing, problems such as material deflection and tearing will occur. In this regard, the following improved technical solutions are proposed. Summary of the invention

[0004] The technical problem solved by the present invention is: to provide a method and a tool for processing the outer circle of non-standard lead-antimony alloy electrodes for electroplating equipment, so as to solve the technical problem that the outer circle processing of non-standard lead-antimony alloy electrodes is difficult under the existing technology, and defects such as material deflection and tearing may occur during the processing.

[0005] The technical solution adopted by the present invention is: a method for processing the outer circle of a non-standard lead-antimony alloy electrode for electroplating equipment, the processing method adopts a horizontal lathe; a three-jaw chuck of the lathe and a rotary center double-end support for the non-standard lead-antimony alloy electrode are selected; a low rotation speed and a low feed speed are used; a 75° hand-sharpened tool made of high-speed steel is used; and a base liquid containing petroleum and ethanol is selected as a cutting fluid to process the outer circle of the non-standard lead-antimony alloy electrode workpiece.

[0006] Among the above technical schemes, as the preferred technical scheme of the present invention: the diameter of the non-standard lead-antimony alloy electrode workpiece is between φ6mm and φ12mm; the lathe speed is 248 rpm for level I and 360 rpm for level II; the lathe feed speed is 0.08 to 0.1mm / min; the rough machining cutting depth is 0.2mm to 0.25mm, and the fine machining cutting depth is 0.1mm to 0.15mm.

[0007] Among the above technical solutions, as the preferred technical solution of the present invention: the petroleum content in the cutting fluid is 0.5% to 1%; the ethanol content is 10% to 15%.

[0008] Among the above technical solutions, as the preferred technical solution of the present invention: the lathe is a C616 horizontal lathe.

[0009] Among the above technical solutions, as the preferred technical solution of the present invention: the rotary center of the lathe is a 60° rotary center.

[0010] In the above technical solution, as a further improved technical solution of the present invention: when setting the tool, the tip of the tool is 0.01 mm lower than the center of the outer circle of the non-standard lead-antimony alloy electrode workpiece.

[0011] Among the above technical schemes, as the preferred technical scheme of the present invention: the rake angle γ of the tool is 13°~16°, and the rake angle is made with a rake angle arc of R0.2mm~R0.4mmmm; the main rake angle of the tool is 75°±10′, and the secondary rake angle is 15°±10′; the tool is also made with a circular arc chip groove; the depth of the circular arc chip groove is proportional to the cutting amount, and the circular arc chip groove is R3~R4mm.

[0012] The present invention also requests protection for a non-standard lead-antimony alloy electrode outer circle machining tool for electroplating equipment, the tool being a tool used for any machining method; the tool being a 75° hand-sharpened tool made of high-speed steel; the tool comprising a tool body and a tool head; at least the tool head being made of high-speed steel.

[0013] Among the above technical schemes, as the preferred technical scheme of the present invention: the tool head rake angle γ = 13°~16°, and the rake angle is made with a rake angle arc of R0.2mm~R0.4mmmm; the tool main rake angle is 75°±10′, and the secondary rake angle is 15°±10′; the tool is also made with an arc chip groove; the depth of the arc chip groove is proportional to the cutting amount, and the arc chip groove is R3mm~R4mm.

[0014] Among the above technical solutions, as a preferred technical solution of the present invention: the cutter head and the cutter body are welded and fixedly connected as one body.

[0015] The advantages of the present invention compared with the prior art are:

[0016] 1. The present invention adopts a horizontal lathe to process the outer circle, which has high precision, high efficiency, simple operation and good versatility.

[0017] 2. In the present invention, because the hardness of the lead-antimony alloy is low and the plastic deformation is large, the low rotation speed can avoid the workpiece from swaying, and the low feed speed can effectively avoid the workpiece from bending during the processing; therefore, the low rotation speed and low feed speed can effectively avoid the workpiece from bending during the processing, and can make the processing more stable, while improving and reducing the surface roughness.

[0018] 3. The 75° hand-ground tool made of high-speed steel of the present invention has high processing efficiency, stable cutting performance, wide application range and high cutting quality; the main material of high-speed steel is tungsten, which has poor affinity with lead-antimony alloy and can effectively avoid tearing.

[0019] 4. The rake angle γ of the cutter head of the present invention is 13°~16°, which can keep the cutting edge in a relatively sharp state, thereby reducing the generation of cutting force and cutting heat, improving cutting efficiency, and at the same time reducing the deformation of chips and avoiding the accumulation of chips during the cutting process; the rake angle arc of R0.2mm~R0.4mmmm helps to reduce the rigid deformation and cutting force generated by the metal during the cutting process, thereby reducing the wear and heat of the front cutting edge; the main rake angle of 75°±10′ and the secondary rake angle of 15°±10′ help to improve the cutting force and vibration, and improve the processing accuracy and surface quality; the high-speed steel main component tungsten has a poor affinity with the lead-antimony alloy, which can effectively avoid tearing.

[0020] 5. The present invention contains 0.5% to 1% petroleum and 10% to 15% ethanol-like liquid as the base liquid, which mainly functions to quickly remove heat through the volatilization of ethanol during the processing process, and the petroleum is used to form an oil film on the processed surface of the workpiece to reduce the oxidation of the workpiece.

[0021] 6. The present invention uses the three-jaw chuck of the lathe and the rotary center to support the non-standard lead-antimony alloy electrodes at both ends; compared with the tool rest, it can effectively avoid scratches on the workpiece surface; the 60° rotary center has high positioning accuracy, wide application range, repairability, high processing efficiency and stable structure.

[0022] 7. When aligning the tool in the present invention, the tool tip is 0.01 mm lower than the center of the workpiece, which can improve processing stability, reduce cutting force and tool wear, and reduce rigid deformation of long workpieces.

[0023] 8. The present invention can effectively avoid rigid deformation, tearing and the like of lead-antimony alloy, thus greatly improving the product quality of non-standard lead-antimony alloy electrodes. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 A top view of the processing of the outer circle of a non-standard lead-antimony alloy electrode by a C616 horizontal lathe of the present invention;

[0025] Figure 2 This is a front view of an embodiment of the outer circle of a φ9×65×210 non-standard lead-antimony alloy electrode of the present invention;

[0026] Figure 3 A three-dimensional diagram of a high-speed steel 75° hand-sharpened tool according to the present invention;

[0027] Figure 4 For the present invention Figure 3 Enlarged detail of the tool head with R0.8 rake angle arc;

[0028] In the figure: 1-front angle arc, 2-arc chip groove, 3-tool body, 4-tool head, 5-center, 6-tool holder, 7-tool, 8-three-jaw chuck, 9-workpiece, 10-lathe. DETAILED DESCRIPTION

[0029] The following will be combined with the attached embodiment of the present invention Figure 1-4 , the technical solutions in the embodiments of the present invention are clearly and completely described. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] A method for machining the outer circle of a non-standard lead-antimony alloy electrode for electroplating equipment (such as Figure 1 (As shown) The processing method adopts a horizontal lathe 10. The horizontal lathe 10 adopts advanced processing technology and can process the outer circle of the workpiece 9 very accurately; this high-precision processing can meet various high-precision mechanical processing needs and ensure the processing quality and performance of the workpiece 9. The horizontal lathe 10 has the characteristics of high speed and high efficiency, and can complete the outer circle processing of the workpiece 9 in a shorter time; this efficient processing method helps to improve production efficiency and reduce production costs. Furthermore, the operation of the horizontal lathe 10 is relatively simple and easy to master, which allows operators to become familiar with the equipment more quickly and improve processing efficiency, while also reducing the difficulty of operation and the error rate. Furthermore, the horizontal lathe 10 has good machine versatility and can process the outer circle in one clamping.

[0031] In the above embodiment, as a preferred embodiment of the present invention: the lathe 10 is a C616 horizontal lathe. The present invention adopts a C616 horizontal lathe to undertake the turning of external cylindrical processing. The guide rails, gears and other important parts of the lathe 10 are all subjected to medium and high quenching and fine grinding, so they have the characteristics of higher precision and good rigidity, thereby ensuring the precision and quality of the processed workpiece 9. The C616 horizontal lathe 10 is easy to operate, safe and reliable; its design takes into account the convenience of the operator, making the operation and processing simpler and more intuitive. The lathe 10 is equipped with a foot-operated brake device and other safety devices, such as a cone clutch safety device, which are helpful to prevent accidents during operation and improve operational safety. The bed, bed feet, oil pan, etc. of the C616 horizontal lathe 10 adopt an integral casting structure with high rigidity and good shock resistance. The lubrication system of the C616 horizontal lathe 10 is reasonably and reliably designed, adopts internal splash lubrication, and performs automatic forced lubrication on special parts, ensuring the stability and durability of the equipment. The C616 horizontal lathe 10 is equipped with a variety of feeding and adjustment mechanisms, such as a four-station automatic feeding mechanical stop device and a speed change device, which makes the processing process more flexible and can meet complex processing requirements. In summary, the C616 horizontal lathe 10 has advantages in processing range, accuracy, operability, safety, structural durability, versatility and flexibility, and has excellent application value.

[0032] In the processing method of the present invention, the three-jaw chuck 8 of the lathe 10 and the rotary center 5 are used to support the non-standard lead-antimony alloy electrode at both ends. Figure 1 Choose a processing method that clamps one end and supports the other end, which can avoid scratching the surface of the workpiece 9 compared to the tool holder.

[0033] In the above embodiment, as a preferred embodiment of the present invention: the rotary top 5 of the lathe 10 is a 60° rotary top. The present invention adopts a 60° rotary top 5 to locate with the help of the center hole, which can ensure that the workpiece 9 obtains a high dimensional accuracy, which is a crucial advantage for high-precision processing. In addition, during use, although the top 5 may be damaged by scratches or surface wear of the tool 7, as long as the bearing in the top 5 is not damaged, the 60° cone surface can be repaired on the cylindrical grinder, so that the 60° rotary top 5 can continue to be used normally. This repairability extends the service life of the top 5 and reduces the cost of use. The 60° rotary top 5 can ensure stable rotation performance during the processing, thereby improving the processing efficiency. The 60° angle design of the top 5 makes the top 5 have better stability during the processing, can reduce vibration and jumping, and further improve and ensure the processing accuracy. In summary, the 60° rotary top 5 has the advantages of high positioning accuracy, wide application range, excellent repairability, high processing efficiency and stable structure.

[0034] In the processing method of the present invention, the outer circle is processed by low rotation speed and low feed speed. Because the hardness of the lead-antimony alloy is low and the plastic deformation is large, the low rotation speed will avoid the workpiece 9 from swinging; and the low feed speed can effectively prevent the workpiece 9 from bending during the processing.

[0035] In the above embodiment, as a preferred embodiment of the present invention: the diameter of the non-standard lead-antimony alloy electrode workpiece 9 is between φ6mm and φ12mm; and the diameter range value refers to the sum of the large end diameter and the small end diameter of the non-standard lead-antimony alloy electrode workpiece 9 is between φ6mm and φ12mm (combined with Figure 2 The rotation speed of the lathe 10 is 248 rpm for level I and 360 rpm for level II; the feed speed of the lathe 10 is 0.08-0.1 mm / min, the cutting depth for rough machining is 0.2 mm-0.25 mm, and the cutting depth for fine machining is 0.1 mm-0.15 mm.

[0036] Embodiment 1: When machining a workpiece 9 of φ6, the rotation speed of the lathe 10 is 248 rpm at level I; the feed speed of the lathe 10 is 0.09 mm / min, the rough machining cutting depth is 0.2 mm, and the fine machining cutting depth is 0.1 mm.

[0037] Embodiment 2: Figure 2 The embodiment is a front view of a φ9×65×210 workpiece; when processing a φ9×65×210 workpiece 9, the rotation speed is level II 360 rpm; the feed rate is 0.09 mm / min, the rough machining cutting depth is 0.2 mm, and the fine machining cutting depth is 0.1 mm.

[0038] Embodiment 3: When machining a φ12 workpiece 9, the rotation speed of the lathe 10 is 360 rpm at level II; the feed speed of the lathe 10 is 0.09 mm / min, the rough machining cutting depth is 0.2 mm, and the fine machining cutting depth is 0.1 mm.

[0039] In summary, the use of low vehicle speed and feed speed can effectively avoid the bending of the workpiece 9 during the processing, and effectively solve the surface roughness problem caused by the tool tip being lower than the center of the workpiece 9. Therefore, low rotation speed and low feed speed can make the processing process more stable and reduce surface roughness.

[0040] In the processing method of the present invention, a 75° hand-sharpened tool 7 made of high-speed steel is used; because the processed material is lead-antimony alloy, the hardness is relatively low, and the alloy turning tool will generate a large impact force perpendicular to the axial direction when contacting the workpiece 9, and the workpiece 9 will be torn and bent during the processing. Therefore, the present invention selects a 75° hand-sharpened tool 7 made of high-speed steel to avoid axial impact force and ensure processing quality. In addition, the 75° hand-sharpened tool has a moderate tip angle, so that the contact area between the tool head and the workpiece 9 is large, and the cutting force is evenly distributed, which helps to improve the processing efficiency, so that the workpiece 9 has a higher processing speed when processing compared to other tools 7. The tool head 4 of the 75° hand-sharpened tool 7 is relatively wide, and the tool head 4 is more stable during the processing, and is not easy to vibrate and jump. This stability helps to obtain higher processing accuracy and surface quality, thereby improving product quality and consistency. Due to the design of its cutting angle, the 75° hand-sharpened tool 7 can provide better cutting quality and surface accuracy. Therefore, the 75° hand-grinded tool 7 made of high-speed steel of the present invention has high processing efficiency, stable cutting performance, wide application range and high cutting quality.

[0041] In the processing method of the present invention, the present invention selects a base liquid containing petroleum and ethanol as a cutting fluid to process the outer circle of the non-standard lead-antimony alloy electrode workpiece 9. Its main function is to quickly take away heat through ethanol volatilization during the processing, and form an oil film on the processed surface of the workpiece 9 to reduce the oxidation of the workpiece 9.

[0042] In the above embodiment, as a preferred embodiment of the present invention, the petroleum content in the cutting fluid is 0.5% to 1% and the ethanol content is 10% to 15%. This ratio can achieve excellent processing surface quality and stable processing quality.

[0043] Example 1: Processing a φ6 workpiece 9, the petroleum content is 1%; the ethanol content is 10%.

[0044] Example 2: Processing a φ9 workpiece 9, the petroleum content is 1%; the ethanol content is 15%.

[0045] Example 3: Processing a φ12 workpiece 9, the petroleum content is 1%; the ethanol content is 15%.

[0046] In the above embodiment, as a further improved technical solution of the present invention: when setting the tool, the tip of the tool 7 is 0.01 mm lower than the center of the non-standard lead-antimony alloy electrode outer circle workpiece 9. When the tip of the tool is lower than the center of the workpiece 9, the processing stability can be improved, the cutting force and tool wear can be reduced, and the rigid deformation of the long workpiece 9 can be reduced.

[0047] In the above embodiment, as a preferred embodiment of the present invention: the rake angle γ of the tool 7 is 13°~16°, and the rake angle γ=13°~16° can keep the cutting edge in a relatively sharp state, thereby reducing the generation of cutting force and cutting heat, and improving cutting efficiency; at the same time, it can reduce the deformation of chips and avoid the accumulation of chips during the cutting process. The rake angle is made with a rake angle arc 1 of R0.2mm~R0.4mmmm; this helps to reduce the rigid deformation and cutting force generated by the metal during the cutting process, thereby reducing the wear and heat of the front cutting surface. The main rake angle of the tool 7 is 75°±10′, and the secondary rake angle is 15°±10′; it helps to improve the cutting force and vibration, and improve the processing accuracy and surface quality. The tool 7 is also made with a circular arc chip groove 2; the depth of the circular arc chip groove 2 is proportional to the cutting amount, and the larger the cutting amount, the larger the chip groove R, and vice versa. The circular arc chip groove 2 is R3~R4mm. When the cutting depth is large, in order to more effectively discharge the chips and prevent them from interfering with the machining process, the chip groove R may be designed to be slightly larger. On the contrary, when the cutting depth is small, the chip groove R may be reduced accordingly. The chip groove design mainly takes into account the discharge, flow direction and chip breaking effect of the chips. A reasonable arc chip groove 2 can ensure that the chips are naturally broken into small fragments during the machining process and are smoothly discharged to other places, thereby avoiding interference or scratching the surface of the workpiece 9, reducing the wear of the tool 7, and improving the machining efficiency.

[0048] Embodiment 1: Processing a φ6 workpiece 9, γ=14°; the rake angle is formed with an arc 1 of R0.2; the arc chip groove 2 is R3.0 mm.

[0049] Embodiment 2: Processing a φ9 workpiece 9, γ=14°; the rake angle is formed with an R0.2 rake angle arc 1; the arc chip groove 2 is R3.5mm.

[0050] Embodiment 3: Processing a φ12 workpiece 9, γ=14°; the rake angle is formed with an arc 1 of R0.4; the arc chip groove 2 is R4.0mm.

[0051] The present invention also claims protection for a non-standard lead-antimony alloy electrode outer circle machining tool for electroplating equipment (such as Figure 3 , Figure 4 As shown in the figure, the tool 7 is a tool used in any of the processing methods; the tool 7 is a 75° hand-sharpened tool made of high-speed steel; the tool 7 has a tool body 3 and a tool head 4; at least the tool head 4 is made of high-speed steel. That is, the tool head material 4 can be different from the tool body 3 material to reduce the manufacturing cost of the tool 7.

[0052] In the above embodiment, as a preferred embodiment of the present invention: the rake angle γ of the cutter head 4 is 13°~16°, and the rake angle is formed with a rake angle arc 1 of R0.2mm~R0.4mm; the main deflection angle of the tool 7 is 75°±10′, and the secondary deflection angle is 15°±10′; the tool 7 is also formed with a circular arc chip groove 2; the depth of the circular arc chip groove 2 is proportional to the cutting amount, and the circular arc chip groove 2 is R3mm~R4mm. The technical advantages of these structural features of the tool 7 have been described above and will not be repeated.

[0053] In the above embodiment, as a preferred embodiment of the present invention, when the cutter head and the cutter body are made of different materials, the cutter head 4 and the cutter body 3 are welded and fixedly connected as one. The welding method is used for the fixed connection, and the structural strength is high and the processing stability is excellent.

[0054] It can be found from the above description that: firstly, the present invention adopts the horizontal lathe 10 to process the outer circle, which has high precision, high efficiency, simple operation and good versatility.

[0055] In the present invention, since the hardness of the lead-antimony alloy is low and the plastic deformation is large, the low rotation speed can avoid the workpiece 9 from swinging; and the low feed speed can effectively avoid the workpiece 9 from bending during the processing; therefore, the low rotation speed and low feed speed can effectively avoid the workpiece 9 from bending during the processing, which can make the processing process more stable and improve and reduce the surface roughness.

[0056] The 75° hand-grinded cutter 7 made of high-speed steel has high processing efficiency, stable cutting performance, wide application range and high cutting quality. The main material of high-speed steel is tungsten, which has poor affinity with lead-antimony alloy and can effectively avoid tearing.

[0057] The rake angle γ of the cutter head of the present invention is 13°~16°, which can keep the cutting edge in a relatively sharp state, thereby reducing the generation of cutting force and cutting heat, improving cutting efficiency, and at the same time reducing the deformation of chips and avoiding the accumulation of chips during the cutting process. The rake angle arc 1 of R0.2mm~R0.4mm helps to reduce the rigid deformation and cutting force generated by the metal during the cutting process, thereby reducing the wear and heat of the front cutting edge. The main rake angle of 75°±10′ and the secondary rake angle of 15°±10′ also help to improve the cutting force and vibration, and improve the processing accuracy and surface quality. The main component of the high-speed steel, tungsten, has a poor affinity with lead-antimony alloys, which can effectively avoid tearing.

[0058] The present invention contains 0.5% to 1% petroleum and 10% to 15% ethanol-like liquid as the base liquid. During the processing, the heat can be quickly removed by the volatilization of the ethanol, and the oxidation of the workpiece 9 can be reduced by the oil film formed on the processed surface of the workpiece 9 by the petroleum.

[0059] The present invention uses a three-jaw chuck 8 of a lathe 10 and a rotary center 5 to support non-standard lead-antimony alloy electrodes at both ends; compared with a tool holder, it avoids scratches on the surface of a workpiece 9; the 60° rotary center 5 has high positioning accuracy, a wide range of applications, excellent repairability, high processing efficiency, and a stable structure.

[0060] When aligning the tool in the present invention, the tool tip is 0.01 mm lower than the center of the workpiece 9 , which can improve processing stability, reduce cutting force and tool wear, and reduce rigid deformation of the long workpiece 9 .

[0061] In summary, the present invention can effectively avoid problems such as rigid deformation and tearing of lead-antimony alloy, and greatly improve the product quality of non-standard lead-antimony alloy electrodes.

[0062] Each embodiment in this specification is described in a related manner, and the same or similar parts between the embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.

[0063] The above description is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention. Any modification and equivalent replacement made within the spirit and principle of the present invention are included in the protection scope of the present invention.

Claims

1. A method for machining the outer circle of a non-standard lead-antimony alloy electrode for electroplating equipment, characterized in that: The processing method adopts a horizontal lathe (10); selects a three-jaw chuck (8) of the lathe (10) and a rotary center (5) to support the non-standard lead-antimony alloy electrode at both ends; uses a low rotation speed and a low feed speed; uses a 75° hand-sharpened tool (7) made of high-speed steel; and selects a base liquid containing petroleum and ethanol as a cutting fluid to process the outer circle of the non-standard lead-antimony alloy electrode workpiece (9).

2. The processing method according to claim 1, characterized in that: The diameter of the workpiece (9) is between φ6 mm and φ12 mm; the rotation speed of the lathe (10) is 248 rpm for level I and 360 rpm for level II; the feed speed of the lathe (10) is 0.08 to 0.1 mm / min, the cutting depth for rough machining is 0.2 mm to 0.25 mm, and the cutting depth for fine machining is 0.1 mm to 0.15 mm.

3. The processing method according to claim 1, characterized in that: The cutting fluid contains 0.5% to 1% petroleum and 10% to 15% ethanol.

4. The processing method according to claim 1, characterized in that: The lathe (10) is a C616 horizontal lathe.

5. The processing method according to claim 1, characterized in that: The rotary center (5) of the lathe (10) is a 60° rotary center.

6. The processing method according to claim 1, characterized in that: When aligning the tool, the tip of the tool (7) is 0.01 mm lower than the center of the non-standard lead-antimony alloy electrode outer circle workpiece (9).

7. The processing method according to claim 1, characterized in that: The rake angle γ of the tool (7) is 13° to 16°, and the rake angle is provided with a rake angle arc (1) of R0.2mm to R0.4mm; the main rake angle of the tool is 75°±10′, and the secondary rake angle is 15°±10′; the tool (7) is also provided with an arc chip groove (2); the depth of the arc chip groove (2) is proportional to the cutting depth; the arc chip groove (2) is R3mm to R4mm.

8. A non-standard lead-antimony alloy electrode outer circle machining tool for electroplating equipment, characterized in that: The tool is a tool used in any one of the processing methods described in claims 1-7; the tool is a 75° hand-sharpened tool made of high-speed steel; the tool (7) comprises a tool body (3) and a tool head (4); at least the tool head (4) is made of high-speed steel.

9. The tool according to claim 8, characterized in that: The tool head (4) has a rake angle γ of 13° to 16°, and the rake angle is provided with a rake angle arc (1) of R0.2mm to R0.4mm; the tool (7) has a main deflection angle of 75°±10′ and a secondary deflection angle of 15°±10′; the tool is also provided with an arc chip groove (2); the depth of the arc chip groove (2) is proportional to the cutting depth; the arc chip groove (2) is R3mm to R4mm.

10. The tool according to claim 8 or 9, characterized in that: The cutter head (4) and the cutter body (3) are welded and fixedly connected as one body.