Medium-low speed magnetic levitation guide rail and welding method thereof

Through the welding method of curved rail cover plates and rib plates, the problem of difficulty in small batch rolling of medium and low-speed magnetic levitation guide rails is solved, the cost is reduced, the welding efficiency and quality are improved, and efficient guide rail production is achieved.

CN118720339APending Publication Date: 2024-10-01CHINA RAILWAY BAOJI BRIDGE GROUP CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410800893.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The cost of rolling F-shaped steel for medium and low-speed maglev guide rails is high and the level of market manufacturers is uneven, which makes rolling small batches of guide rails difficult, and the precision requirements for special-shaped sections are high, which increases the cost of steel mills.

Method used

The welding method of curve rail cover plate and rib plate is adopted, through CNC blanking, gantry cutting, penetration welding and carbon dioxide gas shielded welding, combined with electric heating or flame heating preheating, using asymmetric K-shaped groove welding, and Supports are set up during the welding process to reduce deformation, and finally the welding stress is eliminated by hammering.

Benefits of technology

It reduces the manufacturing cost of medium and low-speed magnetic levitation guide rails, solves the problem of difficulty in rolling small batch guide rails, improves welding efficiency and quality, reduces the workload of linear bending of curved rails, and reduces costs by 20% to 40%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118720339A_ABST
    Figure CN118720339A_ABST
Patent Text Reader

Abstract

The welding method comprises the following steps: blanking a curved rail cover plate by using a numerical control device, blanking a rib plate by using a gate-type cutting machine, finishing, processing a welding groove on a long side, and bending to form a curved line shape; the rib plate and the curve rail cover plate are welded through penetration welding, a welding groove of the rib plate is an asymmetric K-shaped groove, firstly, a deep groove is partially welded, then, a shallow groove is welded and filled, and then, the remaining deep groove is welded; in the welding process, the curved rail cover plate is supported, specifically, first supports are arranged between the two rib plates according to a first preset interval, and second supports are arranged on the outer side of the curved rail cover plate in the length direction according to a second preset interval; and after welding is completed, the support is dismantled. In the embodiment, the curve rail adopts a mode of firstly blanking and then welding, so that the workload of linear bending of the curve rail is reduced; guide rails are produced in a welding mode, and the problem that small-batch guide rails are difficult to roll is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The disclosed embodiments relate to the technical field of magnetic levitation guide rails, and in particular to a medium- and low-speed magnetic levitation guide rail and a welding method thereof. Background Art

[0002] Please refer to Figure 2 The medium and low speed maglev guide rails are made of special steel with an "F" shaped cross section for medium and low speed maglev tracks, which are produced by rolling. The normal service life of F-shaped steel should not be less than 30 years. The type of F-shaped steel should comply with the provisions of GB / T 700, GB / T1591, GB / T 699 or GB / T 4171. Carbon structural steel or weathering steel should be used, usually Q235D. The saturation magnetic flux density of the steel type selected for F-shaped steel should not be less than 1.4T, and the detection method should comply with the provisions of GB / T 13012. The cross-sectional dimensions, cross-sectional area, theoretical weight, and cross-sectional characteristic parameters of F-shaped steel should comply with relevant regulations. F-shaped steel needs to be fully processed and formed into rails to meet the requirements of line use.

[0003] In the related technology, CN106835865A (An "F" type guide rail fine-tuning frame for medium and low speed maglev tracks) discloses an "F" type guide rail fine-tuning frame for medium and low speed maglev tracks, which solves the problem that the accuracy of the F standard surface of the "F" type track sensor plate cannot be directly measured. It is suitable for cooperating with the fine-tuning construction requirements of medium and low speed maglev tracks, and is convenient for adjusting the elevation, mileage and center line of the track array of medium and low speed maglev tracks.

[0004] CN110983876A (rapidly adjustable medium and low speed maglev variable gauge track structure) discloses a rapidly adjustable medium and low speed maglev variable gauge track structure, which facilitates rapid adjustment of the track gauge, greatly reduces the cost of repetitive test line construction, and is conducive to ensuring the organization and implementation of various medium and low speed maglev train test work.

[0005] CN206127755 U (Tooling for connecting F-rail tracks of medium and low speed maglev tracks) discloses a tooling for connecting F-rail tracks of medium and low speed maglev tracks. The new tooling pre-installs a track connecting piece on one of the track ends to accurately position it, thereby accurately installing the connecting piece in the two connecting pieces to achieve two quick and accurate connections.

[0006] The above technical solutions have the following problems:

[0007] F-shaped steel can be rolled in blast furnaces and hot furnaces, but when the quantity is small, the rolling cost is too high, and the "F"-shaped special-shaped section requires high precision. The rolling levels of manufacturers on the market are uneven. For steel mills, necessary tests need to be conducted, which further increases costs.

[0008] Therefore, it is necessary to improve one or more problems existing in the above-mentioned related technical solutions.

[0009] It should be noted that this section is intended to provide background or context for the technical solutions of the present disclosure stated in the claims. The description herein is not admitted to be prior art by virtue of being included in this section. Summary of the invention

[0010] The purpose of the embodiments of the present disclosure is to provide a medium- and low-speed magnetic levitation guide rail and a welding method thereof, thereby overcoming one or more problems caused by the limitations and defects of the relevant technology at least to a certain extent.

[0011] The embodiment of the present disclosure first provides a method for welding a medium- and low-speed magnetic levitation guide rail, wherein the medium- and low-speed magnetic levitation guide rail comprises: a curved rail cover plate and two rib plates, wherein the two rib plates are arranged below the curved rail cover plate, and the cross section of the medium- and low-speed magnetic levitation guide rail is F-shaped; the welding method comprises:

[0012] The curved rail cover is cut by a numerical control device, the rib is cut by a gantry cutting machine, a welding groove is processed on one long side after trimming, and then a curved line is bent;

[0013] The rib plate and the curved rail cover plate are welded by penetration welding, wherein the welding groove of the rib plate adopts an asymmetric K-shaped groove: firstly, a deep groove is partially welded, then a shallow groove is filled by welding, and then the remaining deep groove is welded;

[0014] During the welding process, the curved rail cover plate is supported and arranged: a first support is arranged between the two ribs at a first preset interval, and a second support is arranged at a second preset interval along the length direction on the outer side of the curved rail cover plate;

[0015] After welding is completed, the support is removed.

[0016] In one embodiment of the present disclosure, the groove angles of the asymmetric K-shaped groove are: 45° on the deep groove side and 55° on the shallow groove side.

[0017] In one embodiment of the present disclosure, the joint area is preheated by electric heating or flame heating before welding.

[0018] In one embodiment of the present disclosure, the preheating range is 100 mm from each side of the joint, and the temperature in the thickness direction of the plate is made uniform, and the temperature measurement position is 30-50 mm away from the joint.

[0019] In one embodiment of the present disclosure, carbon dioxide gas shielded welding is used for welding, the welding wire is a solid welding wire or a flux-cored welding wire, the welding current is 220-280A, the voltage is 26-32V, and the welding speed is 30-40cm / min.

[0020] In one embodiment of the present disclosure, the welding sequence used during welding is: first weld the deep groove to a depth of 8-10 mm, then gouge and clean the shallow groove side, weld and fill the shallow groove, and then weld the deep groove side.

[0021] In one embodiment of the present disclosure, the welding direction used during welding is: welding from the middle to both sides along the length direction of the weld, and the welding direction of all welds is consistent.

[0022] In one embodiment of the present disclosure, the support is arranged as follows: a first support is added every 500 mm between two ribs; and a second support is arranged every 500 mm along the length direction on the outer side of the curved rail cover.

[0023] In one embodiment of the present disclosure, during the welding process, a hammering method is used to eliminate the stress of the middle welding layer.

[0024] The embodiment of the present disclosure provides a medium- and low-speed magnetic levitation guide rail, the guide rail comprising: a curved rail cover plate and two rib plates; the structure of the guide rail is one of the following three structures:

[0025] Structure 1: The curved rail cover and one of the ribs are L-shaped as a whole, and the other rib is connected to the curved rail cover by welding;

[0026] Structure 2: The curved rail cover and one of the ribs are L-shaped as a whole, the other rib is connected to the curved rail cover by welding, and the curved rail cover is also connected to a docking plate;

[0027] Structure three: the two ribs are connected to the curved rail cover by welding.

[0028] The technical solution provided by the embodiments of the present disclosure may have the following beneficial effects:

[0029] In the medium and low speed magnetic levitation guide rail welding method of the disclosed embodiment, the curved rail is cut first and then welded, which reduces the workload of bending the curved rail line; the guide rail is produced by welding, which solves the problem of difficulty in rolling small batches of guide rails. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The accompanying drawings herein are incorporated into the specification and constitute a part of the specification, illustrate embodiments consistent with the present disclosure, and together with the specification are used to explain the principles of the present disclosure. Obviously, the accompanying drawings described below are only some embodiments of the present disclosure, and for ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without creative work.

[0031] Figure 1A flow chart showing a medium and low speed magnetic levitation guide rail welding method in an exemplary embodiment of the present disclosure;

[0032] Figure 2 A schematic diagram of the cross-sectional structure of an F-type medium- and low-speed magnetic levitation guide rail rolled in the prior art is shown;

[0033] Figure 3 A schematic diagram showing the three-dimensional structure of an F-type medium- and low-speed magnetic levitation guide rail in an exemplary embodiment of the present disclosure is shown;

[0034] Figure 4 A schematic diagram showing welding of a F-type medium and low speed magnetic levitation guide rail blank in an exemplary embodiment of the present disclosure is shown;

[0035] Figure 5 A schematic diagram showing a rib weld of an F-type medium and low speed magnetic levitation guide rail in an exemplary embodiment of the present disclosure is shown;

[0036] Figure 6 A schematic cross-sectional view of a finished product of an F-type medium- and low-speed magnetic levitation guide rail in an exemplary embodiment of the present disclosure is shown;

[0037] Figure 7 An F-type guide rail adopting structure 1 in an exemplary embodiment of the present disclosure is shown;

[0038] Figure 8 An F-type guide rail adopting structure 2 in an exemplary embodiment of the present disclosure is shown;

[0039] Fig. 9 An F-type guide rail adopting structure three in an exemplary embodiment of the present disclosure is shown.

[0040] Reference numerals:

[0041] 100. Curved rail cover; 200. Rib plate. DETAILED DESCRIPTION

[0042] Example embodiments will now be described more fully with reference to the accompanying drawings. However, example embodiments can be implemented in a variety of forms and should not be construed as limited to the examples set forth herein; rather, these embodiments are provided so that the disclosure will be more comprehensive and complete and to fully convey the concepts of the example embodiments to those skilled in the art. The described features, structures, or characteristics may be combined in any suitable manner in one or more embodiments.

[0043] In addition, the accompanying drawings are only schematic illustrations of the embodiments of the present disclosure and are not necessarily drawn to scale. The same reference numerals in the figures represent the same or similar parts, and their repeated descriptions will be omitted. Some of the block diagrams shown in the accompanying drawings are functional entities and do not necessarily correspond to physically or logically independent entities.

[0044] This example embodiment provides a medium and low speed magnetic levitation guide rail welding method, please refer to Figure 3 and Fig. 9 The medium and low speed magnetic levitation guide rail comprises: a curved rail cover plate 100 and two ribs 200, wherein the two ribs 200 are arranged below the curved rail cover plate 100, and the cross section of the medium and low speed magnetic levitation guide rail is F-shaped.

[0045] Please refer to Figure 1 , the welding method comprises the following steps:

[0046] Step S101, use a numerical control device to cut the curved rail cover 100, use a gantry cutting machine to cut the rib 200, process the welding groove on one long side after trimming, and then bend it into a curved line. Among them, the groove angle of the asymmetric K-shaped groove is: 45° on the deep groove side and 55° on the shallow groove side, but it is not limited to this. For example, the deep groove side can also be 40-48° and the shallow groove side can be 50-58°. Among them, the thickness of the curved rail cover is 30mm; there are 2 ribs, with a thickness of 28mm, and the material is Q235D. When the F-rail blank rib 200 is assembled with the curved rail cover 100, it is precisely positioned. The curved rail cover 100 is CNC cut to ensure the linear size.

[0047] Step S102, please refer to Figure 4 The rib plate 200 and the curved rail cover plate 100 are welded by full penetration welding, wherein the welding groove of the rib plate 200 adopts an asymmetric K-shaped groove: firstly, the deep groove is partially welded, then the shallow groove is filled by welding, and then the remaining deep groove is welded. The full penetration welding can ensure the magnetic flux density of the F rail.

[0048] Step S103, during the welding process, supports are set for the curved rail cover 100: a first support is set between the two ribs 200 at a first preset interval, and a second support is set at a second preset interval along the length direction on the outer side of the curved rail cover.

[0049] Step S104, after welding is completed, the support is removed. Specifically, the support is removed after the welded part is completely cooled.

[0050] In this embodiment, the curved rail is produced by cutting first and then welding, which reduces the workload of bending the curved rail line; the guide rail is produced by welding, which solves the problem of difficulty in rolling small batches of guide rails.

[0051] It should be noted that the joint area is preheated by electric heating or flame heating before welding. A variety of preheating and heating methods are used to improve welding quality.

[0052] Furthermore, the preheating range is 100 mm from each side of the joint, and the temperature in the thickness direction of the plate is made uniform. The temperature measurement position is 30-50 mm from the joint, and the weld is positioned after preheating.

[0053] In one embodiment of the present disclosure, carbon dioxide gas shielded welding is used for welding, the welding wire is a solid welding wire (G49A3UC1S6) or a flux-cored welding wire (T492T1-1C1A), the welding current is 220-280A, the voltage is 26-32V, and the welding speed is 30-40cm / min.

[0054] In one embodiment of the present disclosure, please refer to Figure 5 The welding sequence used during welding is: first weld the deep groove to a depth of 8-10mm, then gouge the shallow groove side, weld and fill the shallow groove, and then weld the deep groove side. Control the temperature between welding layers not to exceed 150℃. According to this welding sequence, the welding qualification rate can be improved, the welding quality of the weld can be guaranteed, the weld position can withstand strong forces, and the safe operation of the vehicle can be guaranteed; in addition, the welding efficiency is improved.

[0055] In addition, cleaning and protection are required before welding: the surface to be welded and the impurities such as oxide scale, rust, grease, water, etc. within 30mm from the edge of the weld groove that affect normal welding and weld quality should be thoroughly removed.

[0056] In one embodiment of the present disclosure, the welding direction used during welding is: welding from the middle to both sides along the length direction of the weld, and the welding direction of all welds is consistent to prevent distortion.

[0057] In one embodiment of the present disclosure, the support is arranged as follows: a first support is added every 500mm between two ribs 200 to control the distance between the two ribs 200; a second support (20×150×350mm) is arranged every 500mm along the length direction on the outside of the curved rail cover 100 to reduce and offset welding deformation. The spacing distance may also adopt other values, such as 400mm, 450mm, etc.

[0058] After welding is completed, the welded parts need to be kept warm and cooled slowly. After welding is completed, the weld surface is immediately covered with asbestos for insulation for 1 hour, and then slowly cooled to room temperature after the insulation time is reached.

[0059] In one embodiment of the present disclosure, during the welding process, a hammering method is used to eliminate the stress of the middle welding layer. An air shovel, a chisel, etc. are used to clean and grind between welds to reduce welding stress.

[0060] Welding quality inspection requirements: The appearance quality of the weld should be free of defects such as cracks, lack of fusion, slag inclusions, and unfilled arc pits. After 24 hours of welding and passing the appearance inspection, the entire length of the weld shall be ultrasonically tested. The weld must meet GB / T 11345, GB / T 29712, B2 level.

[0061] The F-rail cover plate and rib plate are cut with allowances for thickness and overall dimensions. After the rods are welded and corrected, mechanical processing is adopted to ensure the finished size requirements of the F-rail.

[0062] Use CNC machining center to weld the F rail from Figure 4 Processing to Figure 5 After processing is completed, check the surface quality and size, and sandblast and paint if qualified. Figure 6 This is a schematic diagram of the finished cross section of the welded F-type medium and low speed magnetic levitation guide rail. Figure 6 This is only a specific embodiment, and the guide rail structure size is not limited to this.

[0063] The present application adopts multiple welding to weld the groove in batches. After repeated tests, the welding wire, flux, welding current, voltage and welding speed that can guarantee the quality are adopted. The manufacturing cost of the welded guide rail of the present application is reduced by 20% to 40% compared with the small batch rolling process, and the cost reduction is obvious, which is suitable for large-scale promotion.

[0064] In addition, the present invention also provides a medium- and low-speed magnetic levitation guide rail, the guide rail comprising: a curved rail cover plate and two rib plates; the structure of the guide rail is one of the following three structures:

[0065] Structure 1: The curved rail cover and one of the ribs are L-shaped as a whole, and the other rib is connected to the curved rail cover by welding;

[0066] Structure 2: The curved rail cover and one of the ribs are L-shaped as a whole, the other rib is connected to the curved rail cover by welding, and the curved rail cover is also connected to a docking plate;

[0067] Structure three: the two ribs are connected to the curved rail cover by welding.

[0068] The guide rail of this application, namely the F-type guide rail, is produced using the above three structures according to the rolling batch and market conditions. Figure 7 For structure 1, you can use angle steel to weld a rib plate to form an F-type guide rail, and then process it to the designed size; please refer to Figure 8 For structure 2, an F-type guide rail is obtained by welding a rib plate and a butt plate by angle steel; please refer to Fig. 9 ,For structure three, both ribs are connected together by welding and the cover plate.

[0069] The beneficial effects of the above guide rail structure and welding method are as follows:

[0070] (1) Angle steel and steel plate are made by rolling. Compared with directly rolled F-shaped steel, these two materials are widely used, with more optional suppliers and improved component production efficiency.

[0071] (2) For curved F rails, Structure 1 and Structure 2 can use roll bending equipment to bend the angle steel to the required curve shape and then weld the ribs. During the roll bending process, monitor the verticality and top surface flatness of the angle steel at all times.

[0072] (3) For the curved F rail, the structure three can be cut according to the curve line shape, and then the rib plate can be bent to the line shape, and the relative position of the rib plate and the cover plate can be fixed with a tool before welding.

[0073] (4) For the curved F rail, Structure 1, Structure 2 and Structure 3 can be first welded (i.e. welded into an "F" shape) and then bent (top bending, roller bending, or hot bending can be used) into a curved shape. This process is difficult to control the flatness and linearity, and the secondary correction is difficult because the welding stress is released unevenly during the bending (top bending, roller bending, or hot bending) process, which affects the flatness and linearity.

[0074] (5) In the above scheme, since the lower part of the rib is the magnetic pole surface, the welding quality of the root of the rib is required to be high. Therefore, from the perspective of quality control, structure 1> structure 2> structure 3;

[0075] (6) Among the above schemes, since steel plates are the easiest to purchase, followed by small-size angle steels, and finally large-size angle steels, from the perspective of raw material sources and material procurement difficulty, Structure 3 > Structure 2 > Structure 1;

[0076] (7) The above three optimization schemes are selectable according to the production batch engineering quantity. Through the above three schemes, the manufacturing of various small batches of F guide rails can be met.

[0077] (8) Since the welding volume of the above-mentioned structure three is large and the weld requirements are the highest, this application mainly uses structure three as an example to discuss welding, and the welds of structures one and two are executed with reference to the process requirements of structure three.

[0078] It should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like in the above description indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the embodiments of the present disclosure and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the embodiments of the present disclosure.

[0079] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the embodiments of the present disclosure, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.

[0080] In the embodiments of the present disclosure, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present disclosure can be understood according to specific circumstances.

[0081] In the embodiments of the present disclosure, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include the first and second features being in direct contact, or may include the first and second features not being in direct contact but being in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes the first feature being directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes the first feature being directly below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature.

[0082] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present disclosure. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification.

[0083] Those skilled in the art will readily appreciate other embodiments of the present disclosure after considering the specification and practicing the invention disclosed herein. This application is intended to cover any modification, use or adaptation of the present disclosure, which follows the general principles of the present disclosure and includes common knowledge or customary techniques in the art that are not disclosed in the present disclosure. The specification and examples are intended to be exemplary only, and the true scope and spirit of the present disclosure are indicated by the appended claims.

Claims

1. A medium and low speed magnetic levitation guide rail welding method, the medium and low speed magnetic levitation guide rail comprising: A curved rail cover plate and two rib plates, wherein the two rib plates are arranged below the curved rail cover plate, and the cross section of the medium and low speed magnetic levitation guide rail is F-shaped; characterized in that the welding method includes: The curved rail cover is cut by a numerical control device, the rib is cut by a gantry cutting machine, a welding groove is processed on one long side after trimming, and then a curved line is bent; The rib plate and the curved rail cover plate are welded by penetration welding, wherein the welding groove of the rib plate adopts an asymmetric K-shaped groove: firstly, a deep groove is partially welded, then a shallow groove is filled by welding, and then the remaining deep groove is welded; During the welding process, the curved rail cover plate is supported and arranged: a first support is arranged between the two ribs at a first preset interval, and a second support is arranged at a second preset interval along the length direction on the outer side of the curved rail cover plate; After welding is completed, the support is removed.

2. The medium and low speed magnetic levitation guide rail welding method according to claim 1, characterized in that: The groove angles of the asymmetric K-shaped groove are: 45° on the deep groove side and 55° on the shallow groove side.

3. The medium and low speed magnetic levitation guide rail welding method according to claim 1, characterized in that: Before welding, the joint area is preheated by electric heating or flame heating.

4. The medium and low speed magnetic levitation guide rail welding method according to claim 3 is characterized in that: The preheating range is 100mm on each side of the joint, and the temperature in the thickness direction of the plate is uniform. The temperature measurement position is 30-50mm away from the joint.

5. The medium and low speed magnetic levitation guide rail welding method according to claim 1, characterized in that: Carbon dioxide gas shielded welding is used for welding, the welding wire is solid wire or flux-cored wire, the welding current is 220-280A, the voltage is 26-32V, and the welding speed is 30-40cm / min.

6. The medium and low speed magnetic levitation guide rail welding method according to claim 4, characterized in that: The welding sequence used during welding is: first weld the deep groove to a depth of 8-10mm, then gouge and clean the shallow groove side, weld and fill the shallow groove, and then weld the deep groove side.

7. The medium and low speed magnetic levitation guide rail welding method according to claim 1, characterized in that: The welding direction used during welding is: along the length of the weld, welding from the middle to both sides, and the welding direction of all welds is consistent.

8. The medium and low speed magnetic levitation guide rail welding method according to claim 1, characterized in that: The support is arranged in a method that a first support is added every 500 mm between two ribs; and a second support is arranged every 500 mm along the length direction on the outer side of the curved rail cover.

9. The medium and low speed magnetic levitation guide rail welding method according to any one of claims 1 to 8, characterized in that: During the welding process, the hammering method is used to eliminate the stress in the middle weld layer.

10. A medium and low speed magnetic levitation guide rail, characterized in that: The guide rail comprises: a curved rail cover plate and two rib plates; the structure of the guide rail is one of the following three structures: Structure 1: The curved rail cover plate and one of the rib plates are L-shaped as a whole, and the other rib plate is connected to the curved rail cover plate by welding; Structure 2: The curved rail cover and one of the ribs are L-shaped as a whole, the other rib is connected to the curved rail cover by welding, and the curved rail cover is also connected to a docking plate; Structure three: the two ribs are connected to the curved rail cover by welding.

Citation Information

Cited By

  • Fabricated F-shaped rail

    CN224063202U