Preparation method and application of flux-cored wire for double-wire electro-gas welding of large-heat-input thick ship plate steel

By adding calcium titanate and magnesium aluminum alloy to the welding wire, high melting point inclusions are formed, which solves the problems of poor toughness and risk of cracks in welded joints under high heat input, and significantly improves the performance and structure of welded joints.

CN118720522APending Publication Date: 2024-10-01CHINA-UKRAINE INST OF WELDING GUANGDONG ACAD OF SCI

Patent Information

Application Number
CN202410885072.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing welding technology causes the toughness of welded joints to deteriorate and the risk of cracks to increase under high heat input, especially in double-wire gas-electric vertical welding of thick ship plate steel above 600kJ/cm. Existing flux-cored welding wires cannot effectively solve this problem. question.

Method used

By adding calcium titanate and magnesium aluminum alloy to the flux-cored welding wire, elements such as oxygen and sulfur in the welding metal are reacted to form high melting point inclusions TiOx-CaO-Al2O3-MnS, TiOx-MnO-Al2O3-CaO and TiOx-MnS. It prevents grain coarsening, promotes the formation of acicular ferrite as a heterogeneous nucleation core, and improves the performance of welded joints.

Benefits of technology

It effectively prevents grain coarsening at high temperatures, optimizes the welding metal structure, significantly improves the toughness and mechanical properties of welded joints, and reduces the risk of cracks. It is suitable for double-wire gas-electric vertical welding with high heat input above 600kJ/cm.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118720522A_ABST
    Figure CN118720522A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a flux-cored wire for double-wire electro-gas welding of high-heat-input thick ship plate steel, calcium titanate is added into the flux-cored wire, so that elements such as oxygen and sulfur in welding metal are promoted to react to form Ti-Ca composite oxide with high melting point and hardness; the oxides serve as inclusions to prevent grain coarsening at high temperature and serve as heterogeneous nucleation cores to promote formation of acicular ferrite, the performance of a welded joint is improved, and a welded metal structure is optimized; under the condition of high heat input, the Ti-Ca composite oxide can effectively prevent Ti2O3 from being decomposed at high temperature, and the organization structure of welding metal is further optimized; the flux-cored wire disclosed by the invention can be used for ship plate steel for 580MPa and below grade structures in various industrial fields, and 400-600kJ / cm high heat input double-wire electro-gas welding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The invention belongs to the technical field of welding materials, and in particular relates to a preparation method and application of a flux-cored welding wire for double-wire gas-electric vertical welding of thick ship plate steel with large heat input. Background technology:

[0002] In order to promote the rapid construction process of domestic production of marine engineering equipment, it is urgent to develop independent and controllable high-efficiency marine engineering equipment construction technology. Ultra-large line energy welding technology (welding line energy ≥ 600kJ / cm) has extremely high welding efficiency and can greatly shorten the welding period. It has great application potential in the field of large-scale marine engineering equipment manufacturing. However, under such high welding heat input, the austenite grains in the welded joint will be significantly coarsened. At the same time, in the subsequent solid-state phase transformation process, brittle structures such as upper bainite, Widmanstatten structure, and polygonal ferrite are easily formed, resulting in a serious deterioration of the toughness of the welded joint, while increasing the risk of welding cracks, seriously affecting the safe use of marine engineering structural parts.

[0004] CN109128585B discloses a gas shielded flux-cored welding wire with high heat input gas electrostatic welding based on a homogenization mechanism, wherein the outer skin of the flux-cored welding wire is made of cold-rolled thin steel strip; the flux core formula is composed of one or two of titanium dioxide or rutile, feldspar, water glass, lithium oxide, low-carbon ferromanganese, ferrosilicon, aluminum powder, ferromolybdenum, nickel powder, rare earth silicon, boron powder, and the rest is reduced iron powder. It is suitable for high heat input gas electrostatic welding of medium and thick steel plates above 100kJ / cm, and meets the requirements of high heat input gas electrostatic welding of medium and thick plates of structural steel of 690MPa and below, but does not involve double-wire gas electrostatic welding applied to thick ship plate steel.

[0005] CN104923989B discloses a high-efficiency flux-cored welding wire suitable for high-line energy forced forming and a method for preparing and using the same. The flux-cored welding wire comprises an outer steel strip and a filling flux, wherein the filling flux is composed of C, Si, Mn, Ni, Mo, Ti, B, Mg, Al, a slag-forming agent, and the rest is Fe and inevitable impurities. The flux-cored welding wire has strong adaptability, a wide range of welding processes that can be adopted, adjustable composition, and a fast melting speed; the welding process is smooth, the amount of smoke is small, the slag removal and fluidity are good, and the pores are less; the reasonable addition of iron powder improves the welding deposition efficiency, ensures the low-temperature toughness of the weld and obtains excellent comprehensive mechanical properties. However, the welding wire is only suitable for high-heat input gas-electrode welding greater than 100kJ / cm, and does not involve high-heat input double-wire gas-electrode welding greater than 600kJ / cm.

[0006] CN113001058A discloses a flux-cored welding wire for steel welding with high energy input and its application. The chemical composition of the welding wire powder is composed of C, Si, Mn, Ti, Ni, B, Cr, Mo, V, Cu, Al, calcium fluoride, quartz, rutile, strong deoxidizing element M, and the rest is Fe powder. The flux-cored welding wire is mainly used for single-wire gas-electric vertical welding with high energy input for strategic oil reserve tank steel plates.

[0007] Although the domestic market already has flux-cored wires suitable for gas-electric vertical welding with heat input of 100-300 kJ / cm, the existing patents and technologies are still insufficient in the face of the demand for ship plate steel with a thickness of more than 70 mm and a large heat input of more than 600 kJ / cm. Therefore, it is necessary to conduct research and develop flux-cored wires that are compatible with domestically manufactured ultra-large heat input welding steel. Such measures will not only help reduce the production cost of my country's marine engineering equipment manufacturing, but also improve the technical level and competitiveness of my country's marine engineering equipment.

[0008] In view of this, the present invention is proposed. Summary of the invention:

[0009] The present invention provides a method for preparing a flux-cored welding wire for double-wire gas-electric vertical welding of thick ship plate steel with large heat input and its application. By adding calcium titanate to the flux-cored welding wire, calcium titanate and magnesium-aluminum alloy synergistically promote the reaction of oxygen, sulfur and other elements in the weld metal to form inclusions TiO with high melting point and hardness. x -CaO-Al2O3-MnS, TiO x -MnO-Al2O3-CaO and TiO x -MnS effectively prevents the coarsening of grains at high temperatures and acts as a heterogeneous nucleation core to promote the formation of acicular ferrite, improves the performance of welded joints, optimizes the weld metal structure, and solves the problem of poor toughness of welded joints with high heat input above 600kJ / cm in the prior art.

[0010] The present invention is achieved through the following technical solutions:

[0011] The invention discloses a flux-cored welding wire for double-wire gas-electric vertical welding of thick ship plate steel with large heat input, which consists of an outer skin and powder. The powder filling rate (filling rate is the ratio of the powder mass to the sum of the powder mass and the outer skin) is 30-35%. The outer skin is a low-carbon cold-rolled steel strip H08A, and the inner skin contains powder. Based on the total mass percentage of 100%, the powder includes the following components: titanium dioxide: 1-5%, calcium fluoride: 2-6%, magnesium-aluminum alloy: 1-3%, nickel powder: 1-2%, ferromolybdenum: 1-2%, ferrosilicon: 1-2%, low-carbon ferromanganese: 10-15%, calcium titanate: 1-2%, and the balance is reduced iron powder.

[0012] The low carbon steel cold rolled steel strip comprises the following components based on a total mass percentage of 100%: C<0.06%, Si<0.3%, Mn<0.8%, P<0.02%, S<0.01%, and the balance is Fe and unavoidable impurities.

[0013] Preferably, the Mn content in the low carbon ferromanganese is ≥95%; the Si content in the ferrosilicon is ≥70%; the Al content in the magnesium aluminum alloy is ≥50%; the Mo content in the ferromolybdenum is ≥50%; and the Fe content in the reduced iron powder is ≥99%.

[0014] The preparation method of the medicinal powder comprises the following steps:

[0015] (1) ball milling 60-80 mesh iron powder and calcium titanate with a particle size of 200 nm under the protection of argon atmosphere to obtain iron powder / calcium titanate composite powder; ball milling parameters: ball-to-material ratio of 5-6:1, ball milling time of 1-2 hours, and rotation speed of 300-350 r / min;

[0016] (2) The iron powder / calcium titanate composite powder prepared in step (1) and titanium dioxide, calcium fluoride, magnesium aluminum alloy, nickel powder, ferromolybdenum, ferrosilicon, and low-carbon ferromanganese are sieved through a 60-mesh sieve respectively, and then placed in a V-type powder mixer and mixed for 20 to 40 minutes to obtain a uniformly mixed core powder.

[0017] Preferably, the low carbon steel cold-rolled steel strip has a thickness of 0.4-0.5 mm and a width of 14-16 mm.

[0018] Preferably, the particle size of the calcium titanate is 200-300 nm, and the purity is >99%.

[0019] The present invention also provides a method for preparing a flux-cored welding wire for double-wire gas-electric vertical welding of thick ship plate steel with large heat input, which specifically comprises the following steps: an H08A steel strip is ultrasonically cleaned and then rolled into a U-shaped groove, the prepared powder is filled into the U-shaped groove, and after the U-shaped groove is closed, it is rolled into shape and continuously drawn to reduce the diameter to prepare the welding wire; the surface of the welding wire is mechanically cleaned to obtain the flux-cored welding wire.

[0020] The present invention also protects the application of the flux-cored welding wire in 600 kJ / cm high heat input double-wire gas-electric vertical welding of ship plate steel with a thickness of more than 70 mm.

[0021] Preferably, the flux-cored welding wire is used for 80mm wall thickness EH40 grade shipbuilding steel 600kJ / cm heat input double-wire gas-electrode welding test, and the process parameters are: the groove form is designed as a single-sided V-shape, the angle is 20°, the gap is 6-8mm, the blunt edge is 0-1mm, there is no preheating before welding, and no heat treatment after welding; the front wire adopts the DC reverse connection method, and the rear wire adopts the DC positive connection method; the front wire current is 460-557A, and the voltage is 44-50V; the rear wire current is 470-579A, the voltage is 45-53V, the swing width is 15-20mm, the inner dwell time is 0s, and the outer dwell time is 0.5s; the dry extension length of the front and rear two welding wires is 32mm, the welding speed is 30-60mm / min, the welding gun angle is 8-12°, the distance from the rear wire to the pad is 20mm, and the spacing between the two welding wires is 15mm.

[0022] The weld deposited metal of the above-mentioned flux-cored welding wire for double-wire gas-electric vertical welding of thick ship plate steel with high heat input after welding under 100% CO2 gas protection conditions has the following components, based on the total mass percentage as 100%,: C: 0.10~0.20%, Si: 0.30~0.70%, Mn: 1.0~1.8%, Ni: 0.5~1.5%, Ti: 0.02~0.05%, Al: 0.01~0.03%, Mg: 0.01~0.03%, Mo: 0.5~1.0%, O: 0.03~0.10%, and the remainder is Fe and unavoidable impurities.

[0023] Different from the Ti-containing oxide generated by the traditional flux-cored welding wire with added Ti powder, the Ti-containing oxide of the present invention is covered by a layer of CaO or MnS. The thermal expansion coefficient between this type of inclusion and the matrix is ​​large, which will generate large stress and strain around the inclusion, thereby providing a greater driving force for the transformation of austenite to acicular ferrite, promoting the nucleation of acicular ferrite in the crystal, thereby exerting the synergistic effect of Ti and Ca to obtain a welding joint with better performance.

[0024] The beneficial effects of the present invention are as follows:

[0025] 1. In the present invention, calcium titanate is added to the powder, and calcium titanate and magnesium-aluminum alloy work synergistically to promote the reaction of oxygen, sulfur and other elements in the welding metal to form a composite oxide TiO x -CaO-Al2O3-MnS, TiO x -MnO-Al2O3-CaO and TiO x-MnS, etc. These inclusions have high melting points and hardness, which can effectively prevent the coarsening of grains at high temperatures, and can serve as heterogeneous nucleation cores to promote the formation of acicular ferrite; the addition of Ca not only refines the Ti-containing oxides, increases the number density of fine inclusions, and improves the pinning effect; in addition, the addition of Ca changes the composition of the inclusions, turning the Ti oxides into Ti-Ca oxysulfides with smaller particle sizes, which better induces the nucleation of acicular ferrite; in addition, under high heat input conditions, Ti-Ca composite oxides can effectively prevent the decomposition of Ti2O3 at high temperatures, and the presence of a large number of fine nano-scale inclusions can effectively inhibit the growth of grains, further optimizing the organizational structure of the weld metal.

[0026] 2. The present invention adopts 0.4-0.5 mm thin steel strip and high filling rate (35%) flux-cored welding wire, which effectively reduces the molten pool temperature and material loss under high heat input, promotes the addition of more alloy elements, and significantly improves the microstructure and forming quality of the weld.

[0027] 3. The Ti-containing oxide of the present invention is covered by a layer of CaO or MnS. The thermal expansion coefficient between this type of inclusion and the matrix is ​​large, which will generate greater stress and strain around the inclusion, thereby providing a greater driving force for the transformation of austenite to acicular ferrite, promoting the nucleation of acicular ferrite in the crystal, thereby exerting the synergistic effect of Ti and Ca to obtain a welded joint with better performance.

[0028] 4. The present invention adopts ball milling process to evenly disperse calcium titanate in iron powder, give full play to the in-situ strengthening effect of calcium titanate, introduce effective and fine Ti-Ca oxide particles to promote AF formation and improve impact performance. Description of the drawings:

[0029] Figure 1 This is the microstructure diagram of the weld metal after welding with the flux-cored wire prepared in Example 2.

[0030] Figure 2 This is the microstructure diagram of the weld metal after welding with the flux-cored wire prepared in Comparative Example 1. Specific implementation method:

[0031] It will be appreciated by those skilled in the art that the disclosed techniques in the following examples represent techniques that the inventors have found to work well in the practice of the present invention. However, many changes may be made in the disclosed specific embodiments and still achieve the same or similar results without departing from the spirit and scope of the present invention.

[0032] Examples 1-5

[0033] The flux-cored welding wire of Examples 1-5 consists of two parts: an outer skin and powder. The powder filling rate is 35%. The outer skin is a low-carbon cold-rolled steel strip H08A with a thickness of 0.4 mm and a width of 16 mm (see Table 1 for details of the composition). The powder components are shown in Table 2 based on the total mass percentage of 100%.

[0034] Table 1 Chemical composition of steel strip in flux-cored welding wire of Examples 1-5 (wt.%)

[0035]

[0036] Table 2 Composition of powder in flux-cored welding wire (wt.%)

[0037]

[0038]

[0039] The components of the flux-cored welding wire powder of Examples 1-5 include low-carbon ferromanganese containing ≥95% Mn; ferrosilicon containing ≥70% Si; magnesium-aluminum alloy containing ≥50% Al; ferromolybdenum containing ≥50% Mo; and reduced iron powder containing ≥99% Fe.

[0040] The specific preparation steps of the medicinal powder are as follows: 60-mesh iron powder and calcium titanate with a particle size of 200 nm are ball-milled and mixed under the protection of an argon atmosphere, and the ball-milling parameters are as follows: a ball-to-material ratio of 5:1, a ball-milling time of 1 h, and a rotation speed of 300 r / min; an iron powder / calcium titanate composite alloy powder is obtained; the composite alloy powder and titanium dioxide, calcium fluoride, magnesium-aluminum alloy, nickel powder, ferromolybdenum, ferrosilicon, and low-carbon ferromanganese are sieved through a 60-mesh sieve respectively, and the sieved powders are placed in a V-type powder mixer and mixed for 30 min according to the mass percentage in Table 2 to obtain a uniformly mixed medicinal powder.

[0041] The preparation steps of the flux-cored welding wire are as follows: the H08A steel strip is ultrasonically cleaned and then rolled into a U-shaped groove, the above-prepared powder is filled into the U-shaped groove, and after the U-shaped groove is closed, it is rolled into shape and continuously drawn to reduce the diameter to prepare the welding wire; the surface of the welding wire is mechanically cleaned to obtain the flux-cored welding wire of Examples 1-5.

[0042] Comparative Example 1

[0043] Refer to Example 2, the difference is that the powder component does not contain calcium titanate, and the other steps are the same as Example 2.

[0044] Comparative Example 2

[0045] Refer to Example 2, the difference is that the powder component does not contain magnesium-aluminum alloy, and the other steps are the same as Example 2.

[0046] Comparative Example 3:

[0047] Refer to Example 2, the difference is that the powder component does not contain calcium titanate or magnesium-aluminum alloy, and the other steps are the same as Example 2.

[0048] Comparative Example 4:

[0049] Referring to Example 1, the difference is that in the preparation method of the powder, the iron powder and calcium titanate are not ball-milled, and the specific steps are as follows:

[0050] (1) 60-80 mesh iron powder, calcium titanate with a particle size of 200 nm, titanium dioxide, calcium fluoride, magnesium aluminum alloy, nickel powder, ferromolybdenum, ferrosilicon, and low-carbon ferromanganese are sieved through a 60-mesh sieve respectively, and then placed in a V-type powder mixer and mixed for 20-40 minutes to obtain a uniformly mixed core powder.

[0051] The flux-cored welding wire prepared by Examples 1-5 and Comparative Examples 1-4 was selected and applied to a double-wire gas-electrode welding test of 80mm thick EH40 grade shipbuilding steel with a heat input of 600kJ / cm. The groove form is designed to be a single-sided V-shape with an angle of 20°, a gap of 6mm, a blunt edge of 1mm, no preheating before welding, and no heat treatment after welding. The front wire adopts the DC reverse connection method, and the rear wire adopts the DC positive connection method. The current of the front wire is 460A, the voltage is 44V, the current of the rear wire is 470A, the voltage is 45V, the swing width is 15mm, the inner dwell time is 0s, and the outer dwell time is 0.5s. The dry extension of the front and rear two welding wires is 32mm, the welding speed is 30mm / min, and the welding gun angle is 8°. The distance from the rear wire to the pad is 20mm, and the spacing between the two welding wires is 15mm. Before welding, the welding groove and the area within 30mm on both sides need to be polished and cleaned to remove visible oil and rust on the surface to avoid welding defects. No heat treatment is required before welding. The chemical composition of the deposited metal after welding is shown in Table 3, and the performance of the welded joint is shown in Table 4.

[0052] Table 3 Chemical composition of cladding metal after welding (wt.%)

[0053]

[0054]

[0055] Table 4 Welding joint performance test results

[0056]

[0057]

[0058] It can be seen from Table 4 that under the above high heat input twin-wire gas-electrode welding conditions, the welding wires of Examples 1-5 have significantly improved weld performance after welding compared to Comparative Example 1. Among them, the weld metal of Example 2 shows more stable and excellent comprehensive mechanical properties. Figure 1 and Figure 2 The microstructures of the weld metals of Example 2 and Comparative Example 1 are shown respectively. The weld metal of Example 2 exhibits a fine acicular ferrite structure, and its impact energy reaches 70 J. In contrast, Comparative Example 1 forms an upper bainite structure that is easy to crack through under high heat input conditions, resulting in a significant reduction in impact energy to 35 J. This shows that under high heat input welding conditions, the microstructure and impact properties of the weld metal can be effectively controlled by adding an appropriate amount of calcium titanate.

[0059] Compared with Comparative Example 2, Example 2 effectively reduces the oxygen content in the weld metal (down to 0.5wt.%) by adding magnesium-aluminum alloy. Magnesium-aluminum alloy and calcium titanate work together to deoxidize during welding, forming a more stable TiO x -MnO-Al2O3-CaO inclusions. Among them, Al2O3, as the heterogeneous nucleation core of intracrystalline acicular ferrite, helps to improve the microstructure of the weld metal, making it more uniform and fine, thereby significantly improving the performance. In contrast, the high oxygen content in comparative example 2 causes a large amount of oxides in the weld metal, resulting in a significant reduction in impact energy to 28J.

[0060] Compared with Example 2, Comparative Example 3 does not contain calcium titanate and magnesium aluminum alloy, and the inclusions formed during welding are different, thereby reducing the mechanical properties. Its performance is manifested in lower yield strength (400MPa) and tensile strength (505MPa), as well as poor impact toughness (26J). The absence of calcium titanate and magnesium aluminum alloy significantly changes the microstructure and mechanical properties of the weld metal.

[0061] From the comparison between Example 2 and Comparative Examples 1 to 3 in Table 4, it can be seen that calcium titanate and magnesium aluminum alloy work synergistically to significantly enhance the mechanical properties and impact toughness of the weld metal.

[0062] In addition, compared with Comparative Example 4, Example 2 adopts a ball milling method. By subjecting the powder to ball milling, not only is the particle size more uniform and fine, but also the nano calcium titanate can be evenly dispersed in the powder, avoiding local agglomeration of nano particles, giving full play to the synergistic effect of calcium titanate, thereby forming a more uniform weld metal structure during the welding process. The experimental results show that Example 2 prepared by the ball milling method has a significant improvement in tensile strength and yield strength, and the elongation and impact toughness are also significantly improved.

[0063] In summary, the present invention focuses on high-efficiency marine engineering equipment welding technology, especially flux-cored welding wire used in a high heat input twin-wire gas-electrode welding environment. By using a cold-rolled thin steel strip of a specific composition system as the outer skin of the flux-cored welding wire, and combining a specific proportion of powder components, the welding wire of the present invention utilizes the synergistic effect of Ti and Ca during the welding process. This design can inhibit grain growth during the reaction stage between the molten droplet and the molten pool and the subsequent solid-state phase transformation process, and promote the uniform distribution of Ti-Ca composite oxides. In addition, the present technology effectively solves the problem of Ti2O3 decomposition under high heat input conditions, thereby ensuring that the weld metal exhibits excellent welding process performance and comprehensive mechanical properties of the joint after twin-wire gas-electrode welding. The flux-cored welding wire of the present invention can be used in various industrial fields for ship plate steel with a grade of 580MPa and below, and twin-wire gas-electrode welding with a high heat input of 400kJ / cm to 600kJ / cm.

Claims

1. A flux-cored welding wire for double-wire gas-electrode vertical welding of thick ship plate steel with high heat input, characterized in that: The invention consists of an outer skin and powder. The powder filling rate is 30-35%. The outer skin is a low-carbon cold-rolled steel strip H08A, and the inner skin contains powder. Based on the total mass percentage of 100%, the powder includes the following components: titanium dioxide: 1-5%, calcium fluoride: 2-6%, magnesium-aluminum alloy: 1-3%, nickel powder: 1-2%, ferromolybdenum: 1-2%, ferrosilicon: 1-2%, low-carbon ferromanganese: 10-15%, calcium titanate: 1-2%, and the balance is reduced iron powder.

2. The flux-cored welding wire according to claim 1, characterized in that: Based on the total mass percentage of 100%, the low carbon steel cold rolled steel strip includes the following components: C<0.06%, Si<0.3%, Mn<0.8%, P<0.02%, S<0.01%, and the balance is Fe.

3. The flux-cored welding wire according to claim 1, characterized in that: The low carbon ferromanganese contains ≥95% Mn; the ferrosilicon contains ≥70% Si; the magnesium aluminum alloy contains ≥50% Al; the ferromolybdenum contains ≥50% Mo; and the reduced iron powder contains ≥99% Fe.

4. The flux-cored welding wire according to claim 1, characterized in that: The preparation method of the medicinal powder comprises the following steps: (1) ball milling 60-80 mesh iron powder and calcium titanate with a particle size of 200 nm under the protection of argon atmosphere to obtain iron powder / calcium titanate composite powder; ball milling parameters: ball-to-material ratio of 5-6:1, ball milling time of 1-2 hours, and rotation speed of 300-350 r / min; (2) The iron powder / calcium titanate composite powder prepared in step (1) and titanium dioxide, calcium fluoride, magnesium aluminum alloy, nickel powder, ferromolybdenum, ferrosilicon, and low-carbon ferromanganese are sieved through a 60-mesh sieve respectively, and then placed in a V-type powder mixer and mixed for 20 to 40 minutes to obtain a uniformly mixed core powder.

5. The flux-cored welding wire according to claim 1, characterized in that: The low carbon steel cold rolled steel strip H08A has a thickness of 0.4-0.5 mm and a width of 14-16 mm.

6. The flux-cored welding wire according to claim 1, characterized in that: The particle size of the calcium titanate is 200-300 nm, and the purity is >99%.

7. A method for preparing a flux-cored welding wire for double-wire gas-electrode vertical welding of thick ship plate steel with high heat input as claimed in claim 1, characterized in that: The following steps are involved: (1) ball milling 60-80 mesh iron powder and calcium titanate with a particle size of 200 nm under the protection of argon atmosphere to obtain iron powder / calcium titanate composite powder; ball milling parameters: ball-to-material ratio of 5-6:1, ball milling time of 1-2 hours, and rotation speed of 300-350 r / min; (2) The iron powder / calcium titanate composite powder prepared in step (1) and titanium dioxide, calcium fluoride, magnesium aluminum alloy, nickel powder, ferromolybdenum, ferrosilicon, and low-carbon ferromanganese are sieved through a 60-mesh sieve respectively, and then placed in a V-type powder mixer and mixed for 20 to 40 minutes to obtain a uniformly mixed core powder; (3) The H08A steel strip is ultrasonically cleaned and then rolled into a U-shaped groove, and the powder prepared in step (2) is filled into the U-shaped groove. After the U-shaped groove is closed, it is rolled into shape and continuously drawn to reduce the diameter to prepare a welding wire; the surface of the welding wire is mechanically cleaned to obtain a flux-cored welding wire.

8. The use of the flux-cored welding wire according to claim 1, characterized in that: Used for 600kJ / cm high heat input twin-wire gas-electric vertical welding of ship plate steel with a thickness of 70mm or more.

9. The use according to claim 8, characterized in that: The flux-cored welding wire is used for double-wire gas-electrode welding test with heat input of 600 kJ / cm for EH40 grade shipbuilding steel with 80 mm wall thickness. The process parameters are as follows: the groove form is designed as a single-sided V-shape with an angle of 20°, a gap of 6-8 mm, a blunt edge of 0-1 mm, no preheating before welding, and no heat treatment after welding; the front wire adopts the DC reverse connection method, and the rear wire adopts the DC positive connection method; the front wire current is 460-557A, and the voltage is 44-50V; the rear wire current is 470-579A, the voltage is 45-53V, the swing width is 15-20mm, the inner dwell time is 0s, and the outer dwell time is 0.5s; the dry extension length of the front and rear two welding wires is 32mm, the welding speed is 30-60mm / min, and the welding gun angle is 8-12°; the distance from the rear wire to the pad is 20mm, and the spacing between the two welding wires is 15mm.

Citation Information

Patent Citations

  • Flux-cored and gas-shielded wire for gas-electric vertical welding with high heat input

    CN104923989B

  • A gas-shielded flux-cored welding wire for high heat input vertical welding based on microstructure homogenization mechanism

    CN109128585B

  • Flux-cored wire matched with steel for high heat input welding and application thereof

    CN113001058A

Cited By

  • Flux-cored wire containing fluorine-titanium smelting flux as well as preparation method and application of flux-cored wire

    CN120080063A