Preparation method of graphite phase carbon nitride and catalyst for hydrogen production by photocatalytic decomposition of water
By using the SPS sintering method and discharge plasma treatment in the preparation process of graphite-phase carbon nitride, the problems of large energy band width and low crystallinity of graphite-phase carbon nitride are solved, and the efficiency of photocatalytic water splitting to produce hydrogen is improved. .
Patent Information
- Application Number
- CN202410803760.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-20
- Publication Date
- 2024-10-01
AI Technical Summary
The existing preparation method of graphitic phase carbon nitride results in a large energy band width and low crystallinity, which limits the efficiency of photocatalytic water splitting to produce hydrogen.
By calcining melamine and using SPS sintering method, applying pressure and discharge plasma, the formation time of graphite phase carbon nitride is shortened, its crystallinity and light absorption efficiency are improved, and highly crystalline graphite phase carbon nitride is formed.
The photocatalytic efficiency of graphite phase carbon nitride and the efficiency of photocatalytic water splitting to produce hydrogen are significantly improved, the recombination of carriers is reduced, and the light absorption and carrier separation capabilities are enhanced.
Smart Images

Figure CN118723942A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of catalyst technology, and in particular to a method for preparing graphite phase carbon nitride and a catalyst for photocatalytic decomposition of water to produce hydrogen. Background Art
[0002] Fossil energy, as the most widely used energy source, is consumed in large quantities and produces a large amount of pollutants. Clean energy, as a powerful alternative to fossil energy, is pollution-free and has high utilization rates. Hydrogen energy, as a representative of clean energy, does not produce pollutants and by-products when used, and has extensive resource storage. It is currently one of the most promising products to replace fossil energy. At present, the consumption required to extract hydrogen energy is large, resulting in low hydrogen energy production. Photocatalytic technology converts solar energy into chemical energy, transfers the energy of sunlight to catalytic products, and has high efficiency in theory. Photocatalytic hydrogen production can effectively obtain hydrogen energy from pure water, realizing the conversion of solar energy to clean energy.
[0003] As a non-metallic photocatalyst, graphite carbon nitride (g-C3N4) is a covalent crystal with a two-dimensional graphite-like structure. Graphite carbon nitride has a wide range of sources, a simple synthesis method, stable chemical properties, is non-toxic and harmless, has a suitable energy band structure to respond to sunlight, and is very suitable for photocatalytic water decomposition and catalytic hydrogen production.
[0004] However, the energy band width of graphite phase carbon nitride prepared by the existing graphite phase carbon nitride preparation method is relatively large, generally around 2.8eV, which makes the light absorption efficiency of graphite phase carbon nitride low. In addition, the degree of crystallization is low, and the recombination of electrons and holes is serious, which leads to a significant reduction in the number of carriers actually transmitted to the catalyst surface to participate in the reaction, limiting the efficiency of photocatalysis. Summary of the invention
[0005] The present application provides a method for preparing graphite phase carbon nitride and a catalyst for photocatalytic decomposition of water to produce hydrogen, so as to solve the problem that the graphite phase carbon nitride prepared by the method for preparing graphite phase carbon nitride in the related art has a large energy band width and a low degree of crystallinity.
[0006] In a first aspect, the present application provides a method for preparing graphite phase carbon nitride, comprising the following steps:
[0007] calcining melamine to obtain a first product;
[0008] Sintering the first product by SPS method to obtain a second product;
[0009] The second product is mixed with water and ball-milled, ultrasonicated, centrifuged, and freeze-dried to obtain graphite-phase carbon nitride;
[0010] The calcination temperature is 400-500°C.
[0011] The present application uses melamine as a reaction raw material and calcines it to obtain a first product. The calcination temperature is preferably 400-500°C. Within the above temperature range, it can ensure that melamine fully reacts to form the first product of the graphite phase carbon nitride structural unit, and avoid the formation of graphite phase carbon nitride in this step. The first product of the graphite phase carbon nitride structural unit can greatly shorten the formation time of graphite phase carbon nitride under SPS sintering and accelerate the reaction process; the pressure applied during SPS sintering can maintain the structure of the formed graphite phase carbon nitride and increase the crystallinity of the sample; the discharge plasma passed through during SPS sintering causes the graphite phase carbon nitride to produce a large number of carbon and nitrogen vacancies; after sintering, the natural cooling obtains a uniform high-crystalline defect-containing graphite phase carbon nitride material.
[0012] Under the SPS sintering treatment, the applied pressure can shorten the time required for the formation of graphite carbon nitride, while maintaining the structure of the formed graphite carbon nitride, increasing the crystallinity of the sample, improving the reaction area and contact sites of the catalyst, and reducing the recombination of photogenerated carriers; the discharge plasma passing through during SPS sintering causes the graphite carbon nitride to produce a large number of carbon and nitrogen vacancies, greatly shortening the energy band width of the graphite carbon nitride and improving the light absorption efficiency of the catalyst. The vacancies generated cause intermediate energy levels to appear in the energy band structure of the graphite carbon nitride, improving the separation efficiency of carriers, and greatly improving the photocatalytic efficiency of the graphite carbon nitride, and the efficiency of photocatalytic decomposition of water to produce hydrogen is significantly improved.
[0013] It should be noted that the SPS sintering method is spark discharge plasma sintering, a high-end technology for material forming and sintering. The SPS technology is achieved by applying pressure on the powder particles and simultaneously passing a pulse current. When the current passes through, the plasma generated by the spark discharge is heated. This heating method uses thermal effects and field effects to complete sintering in a short time at a relatively low temperature. SPS has a fast sintering speed. Compared with traditional pressureless sintering (PLS), hot pressing sintering (HP) and hot isostatic pressing (HIP) processes, the sintering temperature of SPS can be reduced, and the energy consumption is lower than that of traditional hot pressing sintering. The SPS sintering container can be a graphite mold, preferably a tungsten carbide mold. The mass of the first product of the added intermediate product graphite phase carbon nitride structural element melem can be 2 to 8 g.
[0014] In some embodiments, the melamine is calcined to obtain the first product:
[0015] The calcination time is 4 to 6 hours. Within this range, the calcination time can ensure that the melamine is fully reacted to form the first product; and / or,
[0016] The heating rate of calcination is 2-5°C / min. Within this range, the calcination heating rate can ensure that melamine undergoes a rapid polymerization reaction; and / or,
[0017] The calcination condition is calcination under an inert gas atmosphere, which can reduce the introduction of other impurities. Preferably, the inert gas atmosphere is N2, and the flow rate of N2 is 10 to 50 sccm.
[0018] In some embodiments, the first product is sintered by SPS method to obtain the second product:
[0019] The sintering condition is vacuum sintering, which can reduce the introduction of other impurities; and / or,
[0020] The sintering pressure is 10-100 MPa. When the sintering pressure is within this range, the crystallinity of the second product can be increased.
[0021] In some embodiments, the first product is sintered by SPS method to obtain the second product:
[0022] The sintering temperature is 500-550° C. Within this range, the sintering temperature can ensure that the first product is converted into the second product; and / or,
[0023] The sintering time is 5 to 75 minutes. Within this range, the first product can be fully reacted to form the second product; and / or,
[0024] The heating rate of sintering is 20-50°C / min. When the heating rate of sintering is within this range, the first product can be ensured to undergo a rapid polymerization reaction.
[0025] In some embodiments, the second product is mixed with water, ball-milled, ultrasonicated, centrifuged, and freeze-dried to obtain graphite-phase carbon nitride:
[0026] The mass ratio of the second product to water is (2-5):100. When the mass ratio of the second product to water is within this range, a solution in which the second product is evenly dispersed can be obtained.
[0027] In some embodiments, the second product is mixed with water, ball-milled, ultrasonicated, centrifuged, and freeze-dried to obtain graphite-phase carbon nitride:
[0028] The ball milling speed is 200-500 rpm. The ball milling speed within this range can ensure that the second product is dispersed into a nanosheet structure; and / or,
[0029] The ball milling time is 12 to 24 hours. When the ball milling time is within this range, it can be ensured that the second product is completely converted into a nanosheet structure.
[0030] The ball mill container can be a steel ball mill jar or a zirconium oxide ball mill jar. The volume of the ball mill jar can be 100-150 ml.
[0031] In some embodiments, the second product is mixed with water, ball-milled, ultrasonicated, centrifuged, and freeze-dried to obtain graphite-phase carbon nitride:
[0032] The power of ultrasound is 600 to 1200 W. When the power of ultrasound is within this range, the nanosheets in the solution can be extracted; and / or,
[0033] The ultrasonic time is 4 to 8 hours. When the ultrasonic time is within this range, the nanosheets in the solution can be fully obtained.
[0034] In some embodiments, the second product is mixed with water, ball-milled, ultrasonicated, centrifuged, and freeze-dried to obtain graphite-phase carbon nitride:
[0035] The centrifugal speed is 3000-5000 rpm. Within this range, graphite phase carbon nitride nanosheets can be extracted; and / or,
[0036] The centrifugation time is 10 to 30 minutes. Within this range, graphite phase carbon nitride nanosheets can be fully obtained.
[0037] In some embodiments, the second product is mixed with water, ball-milled, ultrasonicated, centrifuged, and freeze-dried to obtain graphite-phase carbon nitride:
[0038] The freeze drying temperature is -50 to -30°C. Within this range, the water molecules in the solution can be separated; and / or,
[0039] The freeze-drying time is 10 to 48 hours. When the freeze-drying time is within this range, water molecules can be separated.
[0040] In a second aspect, the present application proposes a catalyst for photocatalytic decomposition of water to produce hydrogen, including graphite phase carbon nitride prepared by the preparation method of graphite phase carbon nitride.
[0041] In some embodiments, a method for photocatalytically decomposing water to produce hydrogen using the above-mentioned catalyst for photocatalytically decomposing water to produce hydrogen comprises the following steps:
[0042] S1, mixing the photocatalyst graphite phase carbon nitride, the co-catalyst Pt, the sacrificial agent (at least one of triethanolamine, lactic acid and methanol) and pure water by ultrasonication to obtain a suspension;
[0043] S2, depositing Pt on the surface of the photocatalyst by a photochemical reduction method to obtain a mixed solution;
[0044] S3, applying a light source to the mixed solution to perform photocatalytic hydrolysis to generate hydrogen;
[0045] The mass ratio of Pt to photocatalyst is (1-3):100. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0047] Figure 1 This is a SEM image of graphite phase carbon nitride prepared in Example 1 of the present application.
[0048] Figure 2 This is a TEM image of graphite phase carbon nitride prepared in Example 1 of the present application.
[0049] Figure 3 This is the AMM diagram of the graphite phase carbon nitride prepared in Example 1 of the present application.
[0050] Figure 4 XRD diagram of graphite phase carbon nitride prepared in Comparative Example 1 and Example 1 of the present application.
[0051] Figure 5 This is the ESR graph of graphite phase carbon nitride prepared in Comparative Example 1 and Example 1 of the present application.
[0052] Figure 6 FTIR graph of graphite phase carbon nitride prepared in Comparative Example 1 and Example 1 of the present application.
[0053] Figure 7 This is a UV-visible diffuse reflection test graph of graphite phase carbon nitride prepared in Comparative Example 1 and Example 1 of the present application.
[0054] Figure 8 PL images of graphite phase carbon nitride prepared in Comparative Example 1 and Example 1 of the present application.
[0055] Fig. 9 This is the XPS graph of graphite phase carbon nitride prepared in Comparative Example 1 and Example 1 of the present application.
[0056] Fig.10 This is a diagram showing the catalytic effect of graphite phase carbon nitride prepared in Comparative Example 1 and Examples 1, 2 and 3 of the present application as a photocatalytic water decomposition to produce hydrogen. DETAILED DESCRIPTION
[0057] In order to make the purpose, technical solution and advantages of the present application clearer, the technical solution of the present application will be clearly and completely described below in combination with the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.
[0058] Fossil energy, as the most widely used energy source, is consumed in large quantities and produces a large amount of pollutants. Clean energy, as a powerful alternative to fossil energy, is pollution-free and has high utilization rates. Hydrogen energy, as a representative of clean energy, does not produce pollutants and by-products when used, and has extensive resource storage. It is currently one of the most promising products to replace fossil energy. At present, the consumption required to extract hydrogen energy is large, resulting in low hydrogen energy production. Photocatalytic technology converts solar energy into chemical energy, transfers the energy of sunlight to catalytic products, and has high efficiency in theory. Photocatalytic hydrogen production can effectively obtain hydrogen energy from pure water, realizing the conversion of solar energy to clean energy.
[0059] As a non-metallic photocatalyst, graphite carbon nitride (g-C3N4) is a covalent crystal with a two-dimensional graphite-like structure. Graphite carbon nitride has a wide range of sources, a simple synthesis method, stable chemical properties, is non-toxic and harmless, has a suitable energy band structure to respond to sunlight, and is very suitable for photocatalytic water decomposition and catalytic hydrogen production.
[0060] However, the energy band width of graphite phase carbon nitride prepared by the existing graphite phase carbon nitride preparation method is relatively large, generally around 2.8eV, which makes the light absorption efficiency of graphite phase carbon nitride low. In addition, the degree of crystallization is low, and the recombination of electrons and holes is serious, which leads to a significant reduction in the number of carriers actually transmitted to the catalyst surface to participate in the reaction, limiting the efficiency of photocatalysis.
[0061] In view of this, the present application provides a method for preparing graphite phase carbon nitride and a catalyst for photocatalytic decomposition of water to produce hydrogen, so as to solve the problem that the graphite phase carbon nitride prepared by the method for preparing graphite phase carbon nitride in the related art has a large energy band width and a low degree of crystallinity.
[0062] In a first aspect, the present application provides a method for preparing graphite phase carbon nitride, comprising the following steps:
[0063] S10, calcining melamine to obtain a first product;
[0064] S20, sintering the first product by SPS method to obtain a second product;
[0065] S30, mixing the second product with water, ball milling, ultrasonicating, centrifuging, and freeze-drying to obtain graphite phase carbon nitride;
[0066] The calcination temperature is 400-500°C.
[0067] The present application uses melamine as a reaction raw material and calcines it to obtain a first product. The calcination temperature is preferably 400-500°C. Within the above temperature range, it can ensure that melamine fully reacts to form the first product of the graphite phase carbon nitride structural unit, and avoid the formation of graphite phase carbon nitride in this step. The first product of the graphite phase carbon nitride structural unit can greatly shorten the formation time of graphite phase carbon nitride under SPS sintering and accelerate the reaction process; the pressure applied during SPS sintering can maintain the structure of the formed graphite phase carbon nitride and increase the crystallinity of the sample; the discharge plasma passed through during SPS sintering causes the graphite phase carbon nitride to produce a large number of carbon and nitrogen vacancies; after sintering, the natural cooling obtains a uniform high-crystalline defect-containing graphite phase carbon nitride material.
[0068] Under the SPS sintering treatment, the applied pressure can shorten the time required for the formation of graphite carbon nitride, while maintaining the structure of the formed graphite carbon nitride, increasing the crystallinity of the sample, improving the reaction area and contact sites of the catalyst, and reducing the recombination of photogenerated carriers; the discharge plasma passing through during SPS sintering causes the graphite carbon nitride to produce a large number of carbon and nitrogen vacancies, greatly shortening the energy band width of the graphite carbon nitride and improving the light absorption efficiency of the catalyst. The vacancies generated cause intermediate energy levels to appear in the energy band structure of the graphite carbon nitride, improving the separation efficiency of carriers, and greatly improving the photocatalytic efficiency of the graphite carbon nitride, and the efficiency of photocatalytic decomposition of water to produce hydrogen is significantly improved.
[0069] It should be noted that the SPS sintering method is spark discharge plasma sintering, a high-end technology for material forming and sintering. The SPS technology is achieved by applying pressure on the powder particles and simultaneously passing a pulse current. When the current passes through, the plasma generated by the spark discharge is heated. This heating method uses thermal effects and field effects to complete sintering in a short time at a lower temperature. SPS has a fast sintering speed. Compared with traditional pressureless sintering (PLS), hot pressing sintering (HP) and hot isostatic pressing (HIP) processes, the sintering temperature of SPS can be reduced, and the energy consumption is lower than that of traditional hot pressing sintering. The SPS sintering container can be a graphite mold, preferably a tungsten carbide mold. The mass of the added intermediate product graphite phase carbon nitride structural element melem can be 2 to 8g.
[0070] It should be noted that the present application needs to generate the first product of the graphite phase carbon nitride structural unit in step S10, rather than graphite phase carbon nitride, so that the discharge plasma passed through by the first product during the SPS sintering process can generate a large number of carbon and nitrogen vacancies in the graphite phase carbon nitride, greatly shortening the energy band width of the graphite phase carbon nitride and improving the light absorption efficiency of the catalyst. If the graphite phase carbon nitride is directly sintered in the first step, a large number of carbon and nitrogen vacancies cannot be formed.
[0071] It should be noted that the first product is in the form of white blocks, the second product is in the form of brown blocks, and the graphite phase carbon nitride is in the form of brown nanosheets.
[0072] In combination with the first invention, in some embodiments of the present application, in the calcining of melamine to obtain the first product, the calcination time is 4 to 6 hours. The calcination time within this range can ensure that melamine fully reacts to form the first product.
[0073] In combination with the first invention, in some embodiments of the present application, melamine is calcined to obtain the first product at a heating rate of 2 to 5°C / min. Within this range, the calcination heating rate can ensure rapid polymerization of melamine.
[0074] In combination with the first invention, in some embodiments of the present application, in the calcination of melamine to obtain the first product: the calcination condition is calcination under an inert gas atmosphere, and calcination under an inert gas atmosphere can reduce the introduction of other impurities.
[0075] In combination with the first invention, in some embodiments of the present application, the first product is sintered by the SPS method to obtain the second product: the sintering condition is vacuum sintering, and vacuum sintering can reduce the introduction of other impurities.
[0076] In combination with the first invention, in some embodiments of the present application, the first product is sintered by SPS method to obtain the second product: the sintering pressure is 10-100 MPa. The sintering pressure is within this range, which can increase the crystallinity of the second product.
[0077] In combination with the first invention, in some embodiments of the present application, the first product is sintered by SPS method to obtain the second product: the sintering temperature is 500-550°C. The sintering temperature is within this range, which can ensure that the first product is converted into the second product.
[0078] In combination with the first invention, in some embodiments of the present application, the first product is sintered by SPS method to obtain the second product: the sintering time is 5 to 75 minutes. The sintering time within this range can ensure that the first product fully reacts to form the second product.
[0079] In combination with the first invention, in some embodiments of the present application, the first product is sintered by SPS method to obtain the second product: the sintering heating rate is 20-50°C / min. The sintering heating rate is within this range, which can ensure that the first product undergoes a rapid polymerization reaction.
[0080] In combination with the first invention, in some embodiments of the present application, the second product is mixed with water and ball-milled, ultrasonicated, centrifuged, and freeze-dried to obtain graphite phase carbon nitride: the mass ratio of the second product to water is (2 to 5): 100. Within this range, a solution in which the second product is evenly dispersed can be obtained.
[0081] In combination with the first invention, in some embodiments of the present application, the second product is mixed with water, ball-milled, ultrasonicated, centrifuged, and freeze-dried to obtain graphite phase carbon nitride: the ball milling speed is 200 to 500 rpm. Within this range, the ball milling speed can ensure that the second product is dispersed into a nanosheet structure.
[0082] In combination with the first invention, in some embodiments of the present application, the second product is mixed with water, ball-milled, ultrasonicated, centrifuged, and freeze-dried to obtain graphite phase carbon nitride: the ball milling time is 12 to 24 hours. The ball milling time within this range can ensure that the second product is completely converted into a nanosheet structure.
[0083] The ball mill container can be a steel or zirconium oxide ball mill jar. The volume of the ball mill jar can be 100-150 ml.
[0084] In combination with the first invention, in some embodiments of the present application, the second product is mixed with water, ball-milled, ultrasonicated, centrifuged, and freeze-dried to obtain graphite-phase carbon nitride: the power of the ultrasound is 600 to 1200 W. Within this range of ultrasound power, nanosheets in the solution can be extracted.
[0085] In combination with the first invention, in some embodiments of the present application, the second product is mixed with water, ball-milled, ultrasonicated, centrifuged, and freeze-dried to obtain graphite phase carbon nitride: the ultrasonic time is 4 to 8 hours. Within this range of the ultrasonic time, the nanosheets in the solution can be fully obtained.
[0086] In combination with the first invention, in some embodiments of the present application, the second product is mixed with water, ball-milled, ultrasonicated, centrifuged, and freeze-dried to obtain graphite-phase carbon nitride: the centrifugal speed is 3000-5000 rpm. Within this range of the centrifugal speed, graphite-phase carbon nitride nanosheets can be extracted.
[0087] In combination with the first invention, in some embodiments of the present application, the second product is mixed with water, ball-milled, ultrasonicated, centrifuged, and freeze-dried to obtain graphite-phase carbon nitride: the centrifugation time is 10 to 30 minutes. Within this range of centrifugation time, graphite-phase carbon nitride nanosheets can be fully obtained.
[0088] In combination with the first invention, in some embodiments of the present application, the second product is mixed with water, ball-milled, ultrasonicated, centrifuged, and freeze-dried to obtain graphite phase carbon nitride: the freeze-drying temperature is -50 to -30°C. Within this range of freeze-drying temperature, water molecules in the solution can be separated.
[0089] In combination with the first invention, in some embodiments of the present application, the second product is mixed with water, ball-milled, ultrasonicated, centrifuged, and freeze-dried to obtain graphite phase carbon nitride: the freeze-drying time is 10 to 48 hours. Within this range of freeze-drying time, water molecules can be separated.
[0090] The present application can produce two-dimensional sheet-like nanographite-phase carbon nitride, which contains a large number of carbon and nitrogen vacancies, improves the absorption efficiency of sunlight, increases the active sites of catalytic reactions, and has high photocatalytic performance for decomposing water to produce hydrogen.
[0091] In a second aspect, the present application proposes a catalyst for photocatalytic decomposition of water to produce hydrogen, including graphite phase carbon nitride prepared by the preparation method of graphite phase carbon nitride.
[0092] In conjunction with the second aspect, in some embodiments of the present application, a method for photocatalytically decomposing water to produce hydrogen using the above-mentioned catalyst for photocatalytically decomposing water to produce hydrogen comprises the following steps:
[0093] S1. Mix the photocatalyst graphite phase carbon nitride, the co-catalyst Pt, the sacrificial agent (at least one of triethanolamine, lactic acid and methanol) and pure water by ultrasonication to obtain a suspension; the mass ratio of Pt to the photocatalyst is (1-3):100, and the dosage ratio of the photocatalyst to water is preferably 10 mg of the photocatalyst corresponding to 40-80 ml of water;
[0094] S2. Depositing Pt on the surface of the photocatalyst by photochemical reduction to obtain a mixed solution; placing the suspension on a magnetic stirrer, preferably at a speed of 300 to 600 rpm; irradiating the suspension with a 300W xenon lamp with a 420nm long-wave pass filter for 1 hour, depositing Pt on the surface of the photocatalyst by photochemical reduction, evacuating the entire photocatalytic system, and removing air from the system;
[0095] S3. Applying a light source to the mixed liquid to perform photocatalytic hydrolysis to generate hydrogen.
[0096] The technical solution provided in this application is described in detail below with reference to the embodiments and drawings.
[0097] Example 1
[0098] Embodiment 1 of the present application provides a method for preparing graphite phase carbon nitride, comprising the following steps:
[0099] S1. Use melamine as the reaction raw material and a corundum boat as the reaction container, with the volume of melamine accounting for 2 / 3 of the volume of the corundum boat; move the corundum boat loaded with the raw materials into a tubular furnace for calcination, with a heating rate of 2.3°C / min, a calcination temperature of 400°C, a holding time of 4h, a calcination atmosphere of N2, and a flow rate of 20sccm; after natural cooling, a white first product is obtained.
[0100] S2. Take 2g of the white first product, place it in a tungsten carbide mold, and move it into the SPS sintering instrument after assembly. The parameters are set as follows: heating rate of 50℃ / min, sintering temperature of 550℃, applied pressure of 70MPa, holding time of 15min, and sintering atmosphere of vacuum; after natural cooling, a brown-yellow block-shaped second product is obtained.
[0101] S3. Take 2g of the brown-yellow second product, put it into a zirconia ball mill with a volume of 100ml, add 50g of zirconia balls, then add 50ml of deionized water to mix, and finally put it into a ball mill with the following parameters: ball mill speed of 400rpm and ball milling time of 24h; after ball milling, take out the mixed solution, dilute it five times with deionized water, ultrasonicate it at 900W for 4h, and then centrifuge the suspension after ultrasonication with the following parameters: centrifugal speed of 3000rpm and centrifugal time of 15min; then take the supernatant after centrifugation and freeze it for 10h, put the frozen solid into a vacuum freeze dryer with the freeze drying temperature of -50℃, and dry it to obtain brown-yellow graphite phase carbon nitride.
[0102] Example 2
[0103] Embodiment 2 of the present application provides a method for preparing graphite phase carbon nitride, comprising the following steps:
[0104] S1. Use melamine as the reaction raw material and a corundum boat as the reaction container, with the volume of melamine accounting for 2 / 3 of the volume of the corundum boat; move the corundum boat loaded with the raw materials into a tubular furnace for calcination, with a heating rate of 2°C / min, a calcination temperature of 450°C, a holding time of 5h, a calcination atmosphere of N2, and a flow rate of 20sccm; after natural cooling, a white first product is obtained.
[0105] S2. Take 2g of the white first product, place it in a tungsten carbide mold, and move it into the SPS sintering instrument after assembly. The parameters are set as follows: heating rate of 20℃ / min, sintering temperature of 500℃, applied pressure of 100MPa, holding time of 75min, and sintering atmosphere of vacuum; after natural cooling, a brown-yellow block-shaped second product is obtained.
[0106] S3. Take 2g of the brown-yellow second product, put it into a zirconia ball mill with a volume of 100ml, add 50g of zirconia balls, then add 50ml of deionized water to mix, and finally put it into a ball mill with the following parameters: ball mill speed is 200rpm, and ball milling time is 12h; after ball milling, take out the mixed solution, dilute it five times with deionized water, ultrasonicate it at 600W power for 8h, and then centrifuge the suspension after ultrasonication with the following parameters: centrifugal speed is 5000rpm, and centrifugal time is 10min; then take the supernatant after centrifugation and freeze it for 48h, and place the frozen solid into a vacuum freeze dryer with the freeze drying temperature of -30°C, and dry it to obtain brown-yellow graphite phase carbon nitride.
[0107] Example 3
[0108] Embodiment 3 of the present application provides a method for preparing graphite phase carbon nitride, comprising the following steps:
[0109] S1. Use melamine as the reaction raw material and a corundum boat as the reaction container, with the volume of melamine accounting for 2 / 3 of the volume of the corundum boat; move the corundum boat loaded with the raw materials into a tubular furnace for calcination, with a heating rate of 5°C / min, a calcination temperature of 500°C, a holding time of 6h, a calcination atmosphere of N2, and a flow rate of 20sccm; after natural cooling, a white first product is obtained.
[0110] S2. Take 2g of the white first product, place it in a tungsten carbide mold, and move it into the SPS sintering instrument after assembly. The parameters are set as follows: heating rate of 30℃ / min, sintering temperature of 525℃, applied pressure of 10MPa, holding time of 5min, and sintering atmosphere of vacuum; after natural cooling, a brown-yellow block-shaped second product is obtained.
[0111] S3. Take 2g of the brown-yellow second product, put it into a zirconia ball mill with a volume of 100ml, add 50g of zirconia balls, then add 50ml of deionized water to mix, and finally put it into a ball mill with the following parameters: ball mill speed of 500rpm and ball milling time of 18h; after ball milling, take out the mixed solution, dilute it five times with deionized water, ultrasonicate it at 1200W for 8h, and then centrifuge the suspension after ultrasonication with the following parameters: centrifugal speed of 4000rpm and centrifugal time of 30min; then take the supernatant after centrifugation and freeze it for 24h, put the frozen solid into a vacuum freeze dryer with the freeze drying temperature of -40℃, and dry it to obtain brown-yellow graphite phase carbon nitride.
[0112] Comparative Example 1
[0113] Comparative Example 1 of the present application provides a method for preparing graphite phase carbon nitride, comprising the following steps:
[0114] Melamine is used as the reaction raw material and a corundum boat is used as a reaction container, with the volume of melamine accounting for 2 / 3 of the volume of the corundum boat; the corundum boat loaded with the raw materials is moved into a tubular furnace for calcination, with a heating rate of 2.3°C / min, a calcination temperature of 550°C, a holding time of 4h, a calcination atmosphere of N2, and a flow rate of 20sccm; after natural cooling, graphite phase carbon nitride is obtained.
[0115] In the comparative example, since the calcination temperature is too high, graphite phase carbon nitride is directly formed, and therefore the pressure and pulse current applied by SPS sintering cannot be used to improve the crystallinity of the sample and increase the vacancies.
[0116] Comparative Example 2
[0117] Comparative Example 2 of the present application provides a method for preparing graphite phase carbon nitride, comprising the following steps:
[0118] S1. Use melamine as the reaction raw material and a corundum boat as the reaction container, with the volume of melamine accounting for 2 / 3 of the volume of the corundum boat; move the corundum boat loaded with the raw materials into a tubular furnace for calcination, with a heating rate of 2.3°C / min, a calcination temperature of 400°C, a holding time of 4h, a calcination atmosphere of N2, and a flow rate of 20sccm; after natural cooling, a white first product is obtained.
[0119] S2. Using a tubular furnace sintering method, the first product is sintered at a heating rate of 2.3°C / min, a calcination temperature of 550°C, a holding time of 4 hours, a calcination atmosphere of N2, and a flow rate of 20sccm; after natural cooling, graphite phase carbon nitride is obtained.
[0120] Since Comparative Example 2 did not use SPS sintering, the crystallinity of the sample was very low and the number of vacancies was very small.
[0121] Performance Testing
[0122] The graphite phase carbon nitride prepared in Example 1 was subjected to product characterization, wherein:
[0123] Figure 1 The SEM image (scanning electron microscope image) of the graphite phase carbon nitride obtained in Example 1 is shown in FIG. Figure 2 TEM image (transmission electron microscope image) of the graphite phase carbon nitride obtained in Example 1, Figure 3 This is an AFM image (atomic force microscope image) of the graphite phase carbon nitride obtained in Example 1. Figure 1 and Figure 2 It can be seen that the product is formed by stacking of flake structures, and the size of graphite phase carbon nitride nanosheets is about hundreds of nanometers. Figure 2 The (100) and (002) crystal planes of graphite carbon nitride can also be seen, with interplanar spacings of 0.67 and 0.32 nm, respectively.
[0124] Figure 4 The XRD patterns (X-ray diffraction patterns) of the graphite phase carbon nitride obtained in Comparative Example 1 and Example 1 are as follows: Figure 5 The ESR diagram (electron spin resonance diagram) of the graphite phase carbon nitride obtained in Comparative Example 1 and Example 1, Figure 6 The FTIR graph (Fourier infrared spectrum) of the graphite phase carbon nitride obtained in Comparative Example 1 and Example 1. The XRD graph shows that the structure of the graphite phase carbon nitride obtained in Example 1 is graphite phase carbon nitride, and has higher crystallinity. The ESR graph shows that the product has a large number of vacancies, which improves the catalytic efficiency of the photocatalyst. The FTIR graph shows the presence of the characteristic triazine ring structure of the product, and the overall structure of the graphite phase carbon nitride is maintained.
[0125] Figure 7 The UV-visible diffuse reflection test diagram of the graphite phase carbon nitride obtained in Comparative Example 1 and Example 1 is shown in FIG. Figure 8 This is the PL graph (fluorescence spectrum graph) of the graphite phase carbon nitride obtained in Example 1. The UV-visible diffuse reflectance graph proves that the graphite phase carbon nitride product obtained in Example 1 has strong absorption under ultraviolet and visible light and has stronger absorption efficiency of sunlight. The PL graph shows that the carrier recombination of the product is weak, which is conducive to the carrier transmission to the surface of the sample to participate in the photocatalytic reaction.
[0126] Fig. 9 The XPS graphs (X-ray photoelectron spectroscopy) of the graphite phase carbon nitride obtained in Comparative Example 1 and Example 1 show that the C1s spectrum shows that the graphite phase carbon nitride obtained in Example 1 has a high carbon vacancy, and the N1s spectrum shows that a large number of nitrogen vacancies are generated, and the vacancy type is mainly N 2C and N 3CThe composition and high dose of carbon and nitrogen vacancies not only narrow the band gap of graphitic carbon nitride, but also generate intermediate energy levels, which are beneficial to the separation and transmission of photogenerated carriers and inhibit the recombination of carriers, thereby greatly improving the rate of photocatalytic water decomposition to produce hydrogen.
[0127] Under ultrasonic conditions, 10 mg of the graphite phase carbon nitride prepared in Example 1, Example 2 and Example 3 was dispersed in 36 ml of deionized water, the ultrasonic power was 75 W, and the ultrasonic time was 30 min; then 4 ml of triethanolamine was added, and the ultrasonic was continued for 10 min; finally, 150 μl of 2% H2PtC l6 Solution. Pt was deposited on the catalyst surface by photochemical reduction; the reaction system was then evacuated to remove air. A 300W xenon lamp with a 420nm long-wave filter was used as a simulated light source to illuminate the reaction system for photocatalytic water decomposition to produce hydrogen. Finally, the amount of hydrogen produced was analyzed using a Shimadzu GC-2014C gas chromatograph.
[0128] Using Comparative Example 1 as a control catalyst, photocatalytic water decomposition to produce hydrogen was carried out according to the above experimental process, and the amount of hydrogen produced was analyzed.
[0129] Fig.10 The graphs show the effects of graphite phase carbon nitride as photocatalytic water decomposition to produce hydrogen in comparative example 1, examples 1, 2 and 3. The hydrogen production rate of the SPS sintered sample is significantly higher than that of the CNN sample, and the hydrogen production rate of example 1 is the highest and is 8.8 times that of CNN. This shows that the graphite phase carbon nitride photocatalyst prepared by the present invention can greatly improve the efficiency of photocatalytic water decomposition to produce hydrogen.
[0130] The rates of photocatalytic water decomposition and hydrogen production by the graphite phase carbon nitride in Examples 2 and 3 are much higher than that of CNN, which proves that the graphite phase carbon nitride photocatalyst prepared in the present invention can greatly improve the efficiency of photocatalytic water decomposition and hydrogen production.
[0131] In summary, by using melamine as a reaction raw material and calcining it, a first product is obtained. The calcination temperature is preferably 400-500°C. Within the above temperature range, melamine can be fully reacted to form the first product of the graphite phase carbon nitride structural unit, and the formation of graphite phase carbon nitride in this step can be avoided. The first product of the graphite phase carbon nitride structural unit can greatly shorten the formation time of graphite phase carbon nitride under SPS sintering and accelerate the reaction process; the pressure applied during SPS sintering can maintain the structure of the formed graphite phase carbon nitride and increase the crystallinity of the sample; the discharge plasma passed through during SPS sintering causes the graphite phase carbon nitride to produce a large number of carbon and nitrogen vacancies; after sintering, the natural cooling obtains a uniform high-crystalline defect-containing graphite phase carbon nitride material.
[0132] Under the SPS sintering treatment, the applied pressure can shorten the time required for the formation of graphite carbon nitride, while maintaining the structure of the formed graphite carbon nitride, increasing the crystallinity of the sample, improving the reaction area and contact sites of the catalyst, and reducing the recombination of photogenerated carriers; the discharge plasma passing through during SPS sintering causes the graphite carbon nitride to produce a large number of carbon and nitrogen vacancies, greatly shortening the energy band width of the graphite carbon nitride and improving the light absorption efficiency of the catalyst. The vacancies generated cause intermediate energy levels to appear in the energy band structure of the graphite carbon nitride, improving the separation efficiency of carriers, and greatly improving the photocatalytic efficiency of the graphite carbon nitride, and the efficiency of photocatalytic decomposition of water to produce hydrogen is significantly improved.
[0133] In the description of this specification, the description with reference to the terms "one embodiment / method", "some embodiments / methods", "example", "specific example" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment / method or example are included in at least one embodiment / method or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment / method or example. Moreover, the specific features, structures, materials or characteristics described may be combined in a suitable manner in any one or more embodiments / methods or examples. In addition, those skilled in the art may combine and combine the different embodiments / methods or examples described in this specification and the features of the different embodiments / methods or examples, unless they are contradictory.
[0134] It should be noted that, in the present application, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment. In the absence of more restrictions, the elements defined by the sentence "comprise one..." do not exclude the existence of other identical elements in the process, method, article or equipment including the elements. In the present application, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically stipulated.
[0135] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A method for preparing graphite phase carbon nitride, It is characterized in that The following steps are involved: calcining melamine to obtain a first product; Sintering the first product by SPS method to obtain a second product; The second product is mixed with water and ball-milled, ultrasonicated, centrifuged, and freeze-dried to obtain graphite-phase carbon nitride; The calcination temperature is 400-500°C.
2. The method for preparing graphite phase carbon nitride according to claim 1, It is characterized in that The melamine is calcined to obtain the first product: The calcination time is 4 to 6 hours; and / or, The heating rate of calcination is 2 to 5°C / min; and / or, The calcination condition is calcination under an inert gas atmosphere.
3. The method for preparing graphite phase carbon nitride according to claim 1, It is characterized in that The first product is sintered by SPS method to obtain the second product: The sintering condition is vacuum sintering; and / or, The sintering pressure is 10-100 MPa.
4. The method for preparing graphite phase carbon nitride according to claim 1, It is characterized in that The first product is sintered by SPS method to obtain the second product: The sintering temperature is 500-550°C; and / or, The sintering time is 5 to 75 minutes; and / or, The heating rate of sintering is 20-50°C / min.
5. The method for preparing graphite phase carbon nitride according to claim 1, It is characterized in that The second product is mixed with water and ball-milled, ultrasonicated, centrifuged, and freeze-dried to obtain graphite phase carbon nitride: The mass ratio of the second product to water is (2-5):
100.
6. The method for preparing graphite phase carbon nitride according to claim 1, It is characterized in that The second product is mixed with water and ball-milled, ultrasonicated, centrifuged, and freeze-dried to obtain graphite phase carbon nitride: The ball milling speed is 200 to 500 rpm; and / or, The ball milling time is 12 to 24 hours.
7. The method for preparing graphite phase carbon nitride according to claim 1, It is characterized in that The second product is mixed with water and ball-milled, ultrasonicated, centrifuged, and freeze-dried to obtain graphite phase carbon nitride: The power of ultrasound is 600 to 1200 W; and / or, The ultrasound time is 4 to 8 hours.
8. The method for preparing graphite phase carbon nitride according to claim 1, It is characterized in that The second product is mixed with water and ball-milled, ultrasonicated, centrifuged, and freeze-dried to obtain graphite phase carbon nitride: The centrifugal speed is 3000-5000 rpm; and / or, The centrifugation time is 10 to 30 minutes.
9. The method for preparing graphite phase carbon nitride according to claim 1, It is characterized in that The second product is mixed with water and ball-milled, ultrasonicated, centrifuged, and freeze-dried to obtain graphite phase carbon nitride: The freeze drying temperature is -50 to -30°C; and / or, The freeze-drying time is 10 to 48 hours.
10. A catalyst for photocatalytic decomposition of water to produce hydrogen, It is characterized in that The invention relates to graphite phase carbon nitride prepared by the method for preparing graphite phase carbon nitride according to any one of claims 1 to 9.
Citation Information
Patent Citations
Preparation method of g-C3N4-based p-n homojunction photocatalyst and preparation method of hydrogen
CN112354553A
Preparation method and application of Ti4O7 doped C3N4 electrode material
CN117756232A
Parts of apparatus for plasma treatment and method for manufacture thereof, and apparatus for plasma treatment
WO2002067312A1