Iron phosphate material and preparation method thereof, lithium iron phosphate material and preparation method and application thereof
Through the composite structure and carbon layer coating of large-particle hollow iron phosphate and small-particle solid iron phosphate, the problems of low electronic conductivity and lithium ion diffusion rate of lithium iron phosphate materials are solved, and the tap density and magnification rate of the material are improved. performance.
Patent Information
- Application Number
- CN202410907790.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-08
AI Technical Summary
Lithium iron phosphate material has low electronic conductivity and slow lithium ion diffusion rate due to its olivine structure, and the hollow structure is prone to "overburning" problems when increasing tap density.
It adopts a compound structure of large-particle hollow iron phosphate and small-particle solid iron phosphate. Through the combination of hollow template agent and solid template agent, an iron phosphate material with a carbon layer is formed, and is calcined with the addition of lithium source and carbon source. Lithium iron phosphate material is formed.
It improves the lithium ion diffusion rate and rate performance, alleviates the reduction in tap density caused by hollow materials, and optimizes the morphology and performance of lithium iron phosphate materials.
Smart Images

Figure CN118723957A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium battery materials, and in particular, relates to an iron phosphate material and a preparation method thereof, a lithium iron phosphate material and a preparation method and application thereof. Background Art
[0002] The main advantages of lithium iron phosphate (LiFePO4) materials include wide raw material sources, environmental friendliness, high theoretical capacity (170mAh / g) and stable discharge platform. However, due to its olivine structure, FeO6 does not form a continuous edge-sharing octahedral network, so it cannot form a good electronic conductive network, resulting in low electronic conductivity of LiFePO4; at the same time, PO4 tetrahedrons are located between FeO6 layers, which limits the change of crystal volume and hinders Li + The diffusion movement results in an extremely low lithium ion diffusion rate.
[0003] To address the shortcomings of lithium iron phosphate batteries, common improvement methods include preparing hollow structures, carbon coating, and material nano-scaling.
[0004] CN113540455A discloses a hollow carbon-coated lithium iron phosphate particle and its preparation method and application. Hollow lithium phosphate is prepared and then converted into hollow lithium iron phosphate precursor particles by adding iron salt and phosphorus source. The hollow carbon-coated lithium iron phosphate is obtained by mixing with a carbon source, spray drying and sintering under a protective atmosphere.
[0005] The hollow structure of lithium iron phosphate will affect the tap density of the material. In order to improve the tap density, the field adopts the method of large and small particle grading to improve the rate performance. However, large-particle hollow lithium iron phosphate makes lithium ion insertion / extraction difficult, and during the calcination process, the "overburning" problem will occur due to the large and small particle grading.
[0006] In view of this, the present invention is proposed. Summary of the invention
[0007] The purpose of the present invention includes providing an iron phosphate material and a preparation method thereof, a lithium iron phosphate material and a preparation method and application thereof, aiming to increase the lithium ion diffusion rate of the positive electrode material and improve the rate performance; at the same time, the large and small particle sizes are matched to alleviate the reduction in the tap density caused by the hollow lithium iron phosphate material.
[0008] In a first aspect, the present invention provides an iron phosphate material, which contains large hollow iron phosphate particles and small solid iron phosphate particles. The large hollow iron phosphate particles include an iron phosphate shell layer and a carbon layer on the inner surface of the iron phosphate shell layer.
[0009] In some embodiments of the present invention, the iron phosphate material has at least one of the following features 1 to 3:
[0010] Feature 1: The average particle size of large hollow iron phosphate particles ranges from 2.0μm to 4.0μm, and the average particle size of small solid iron phosphate particles ranges from 0.9μm to 2μm;
[0011] Feature 2: The thickness of the iron phosphate shell is 300nm-700nm;
[0012] Feature 3: The thickness of the carbon layer on the inner surface of the iron phosphate shell is 100nm-200nm.
[0013] In a second aspect, the present invention further provides a method for preparing an iron phosphate material, comprising the following steps:
[0014] The solid template is added to the dispersion of the hollow template to obtain a suspension, a second iron salt and a phosphorus source are added to the suspension to obtain a reaction solution, the mixture is stirred for reaction, and the obtained solid is calcined to obtain an iron phosphate material;
[0015] In some embodiments of the present invention, the preparation method of the hollow template agent dispersion is as follows: after mixing soy protein isolate, a surfactant and water to form a dispersion system, the dispersion system is mixed with an oil phase solvent and stirred to obtain an emulsion, and a first iron salt is further added to the emulsion to perform a gelation reaction, thereby obtaining a hollow template agent dispersion;
[0016] In some embodiments of the present invention, the suspension further includes ethanol, and the order of mixing the components is to first prepare a dispersion of the hollow template agent, then add the solid template agent to the dispersion and mix well, and finally add ethanol and stir evenly;
[0017] In some embodiments of the present invention, the method for preparing the iron phosphate material satisfies at least one of the following preparation conditions ① to ⑨:
[0018] Condition ①: The amount of ethanol added is 15%-20% of the volume of the dispersion;
[0019] Condition ②: The concentration of the phosphorus source in the reaction solution is 0.9-2 mol / L;
[0020] Condition ③: The molar ratio of iron to phosphorus in the reaction solution is 1:(1-1.03);
[0021] Condition ④: The solid template is a spherical nano-iron phosphate with an average diameter of 200-500 nm;
[0022] Condition ⑤: The amount of the solid template added is 5wt%-10wt% of the mass of the dispersion;
[0023] Condition ⑥: the second iron salt comprises at least one of ferric chloride or ferric nitrate;
[0024] Condition ⑦: The phosphorus source includes at least one of ammonium hydrogen phosphate, ammonium phosphate, ammonium dihydrogen phosphate, sodium hydrogen phosphate, sodium dihydrogen phosphate and sodium phosphate;
[0025] Condition ⑧: The stirring reaction has a stirring speed of 400-500 rpm, a reaction temperature of 60-90° C., and a reaction time of 8-12 h;
[0026] Condition ⑨: During the calcination process, the calcination temperature is controlled to be 400-700°C and the calcination time is 2-4h.
[0027] In some embodiments of the present invention, the method for preparing the dispersion of the hollow template agent satisfies at least one of the following conditions I to VII:
[0028] Condition I: The stirring speed of the mixing and stirring is 12000-16000 rpm, and the stirring time is 3-6 min;
[0029] Condition II: the surfactant includes at least one of polyoxyethylene fatty alcohol ether, alkyl glycoside compound, polyoxyethylene sorbitan monooleate, alkylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether, polyoxyethylene fatty amine, polyoxyethylene castor oil, and polyoxyethylene oleyl ether; the mass fraction of the surfactant in the dispersion is 1wt%-3wt%;
[0030] Condition III: the concentration of the soy protein isolate in the dispersion is 10-30 mg / ml;
[0031] Condition IV: The oil phase solvent includes at least one of kerosene, heptane, n-hexane, cyclohexane, vegetable oil, and liquid paraffin;
[0032] Condition V: The volume ratio of the dispersion system to the oil phase solvent is (3-8):2;
[0033] Condition VI: The gelation reaction is a reaction carried out under stirring at room temperature for 10-20 minutes;
[0034] Condition VII: The first iron salt includes at least one of ferric chloride and ferric nitrate; the feed ratio of the first iron salt to the dispersion is (0.1-0.3) mol:1L.
[0035] In a third aspect, the present invention further provides a method for preparing a lithium iron phosphate material, comprising mixing an iron phosphate material, a lithium source, a carbon source and ethanol to obtain a slurry, grinding and drying the slurry, and calcining the slurry in an inert atmosphere to obtain a lithium iron phosphate material; wherein the iron phosphate material is the iron phosphate material in any of the above embodiments or the iron phosphate material prepared by the preparation method in any of the above embodiments;
[0036] In some embodiments of the present invention, the method for preparing the lithium iron phosphate material satisfies at least one of the following conditions a to f:
[0037] Condition a: The lithium source is selected from at least one of lithium oxalate, lithium carbonate and lithium hydroxide;
[0038] Condition b: the carbon source is selected from at least one of glucose, sucrose, dopamine, cyclodextrin, citric acid, aniline, cellulose acetate, and polyvinyl pyrrolidone;
[0039] Condition c: the carbon source is 5%-10% of the total mass of the lithium source and the iron phosphate material;
[0040] Condition d: the slurry grinding time is 2-6h;
[0041] Condition e: the calcination temperature is 700-850°C, and the calcination time is 6-15h;
[0042] Condition f: The inert atmosphere is selected from at least one of nitrogen, helium and argon.
[0043] In a fourth aspect, the present invention also provides a lithium iron phosphate material, which includes large-particle hollow lithium iron phosphate and small-particle solid lithium iron phosphate; the large-particle hollow lithium iron phosphate includes a lithium iron phosphate shell, a first carbon coating layer on the outer surface of the lithium iron phosphate shell, and a carbon layer on the inner surface of the lithium iron phosphate shell; the small-particle solid lithium iron phosphate includes lithium iron phosphate and a second carbon coating layer on the outer surface of the lithium iron phosphate.
[0044] In a fifth aspect, the present invention further provides a positive electrode plate, the raw materials for preparing the positive electrode plate include the lithium iron phosphate material of the third aspect and / or the fourth aspect.
[0045] The beneficial effects of the present invention include:
[0046] The iron phosphate material provided by the present invention comprises large-particle hollow iron phosphate and small-particle solid iron phosphate, the inner surface of the shell of the large-particle hollow iron phosphate has a carbon layer, the prepared lithium iron phosphate material inherits the morphology of the above-mentioned iron phosphate material, and the outer surface of the lithium iron phosphate including solid and hollow is also coated with a carbon layer, and the uniform and diversely distributed carbon layer can improve the rate performance; at the same time, the compounding of large-particle hollow and small-particle solid lithium iron phosphate can effectively alleviate the reduction in tap density caused by the hollow material on the basis of shortening the lithium ion transmission path. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0048] Figure 1 A process flow chart of a method for preparing lithium iron phosphate provided in an embodiment of the present invention;
[0049] Figure 2 This is the TEM image of the iron phosphate material obtained in Example 1. DETAILED DESCRIPTION
[0050] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0051] The endpoints and any values of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be considered as specifically disclosed in this article.
[0052] The present invention provides an iron phosphate material, including large hollow iron phosphate particles and small solid iron phosphate particles. The large hollow iron phosphate particles include an iron phosphate shell layer and a carbon layer on the inner surface of the shell layer. The large hollow iron phosphate particles are formed by using a hollow template agent, and the small solid iron phosphate particles are formed by using a solid template agent as a seed. The combination of large and small particles can improve the tap density of the material.
[0053] In some embodiments, the solid template is spherical nano-iron phosphate with an average diameter of 200-500 nm (eg, 200 nm, 300 nm, 400 nm, 500 nm, etc.).
[0054] In some embodiments, the average particle size of the large-particle hollow ferric phosphate is in the range of 2.0 μm to 4 μm (eg, 2.0 μm, 2.5 μm, 3.0 μm, 3.5 μm, 4.0 μm, etc.).
[0055] In some embodiments, the thickness of the iron phosphate shell of the large hollow iron phosphate particle is in the range of 300-700 nm (eg, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, etc.).
[0056] In some embodiments, the thickness of the carbon layer on the inner surface of the shell layer of the large-particle hollow ferric phosphate material is in the range of 100 nm-200 nm (eg, 100 nm, 150 nm, 200 nm, etc.).
[0057] In some embodiments, the average particle size of the small-particle solid ferric phosphate is in the range of 0.9 μm to 2.0 μm (eg, 0.9 μm, 1.2 μm, 1.6 μm, 2.0 μm, etc.).
[0058] The present invention also provides a lithium iron phosphate material, including large-particle hollow lithium iron phosphate and small-particle solid lithium iron phosphate. The large-particle hollow lithium iron phosphate includes a lithium iron phosphate shell, a carbon layer on the inner surface of the lithium iron phosphate shell, and a first carbon-coated carbon layer on the outer surface of the lithium iron phosphate shell; the small-particle solid lithium iron phosphate includes lithium iron phosphate and a second carbon coating layer on the outer surface of the lithium iron phosphate.
[0059] Furthermore, an embodiment of the present invention also provides a positive electrode plate, comprising the above-mentioned lithium iron phosphate and a positive electrode current collector, wherein the lithium iron phosphate is distributed on the positive electrode current collector as a positive electrode active material.
[0060] The present invention provides a method for preparing lithium iron phosphate. Figure 1 , specifically including the following steps:
[0061] S1. Preparation of dispersion of hollow template agent
[0062] Soy protein isolate, surfactant and water form a dispersion system, the dispersion system is mixed with an oil phase solvent to obtain an emulsion, and the first iron salt is further added to the emulsion for gelation reaction to obtain a dispersion of the hollow template agent. The surfactant and the soybean protein isolate are compounded to obtain a mixed stabilizer. By adding iron ions, on the one hand, the soybean protein isolate in the emulsion is gelled, so that the soybean protein isolate is more tightly bound, and the stabilizing effect of the soybean protein isolate on the emulsion is improved; on the other hand, the surface of the hollow template is loaded with Fe 3+ Become the reaction center of iron phosphate.
[0063] In some embodiments, the surfactant is selected from at least one of polyoxyethylene fatty alcohol ether, alkyl glycoside compound, polyoxyethylene sorbitan monooleate, alkylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether, polyoxyethylene fatty amine, polyoxyethylene castor oil, and polyoxyethylene oleyl ether, and the surfactant can be any one or more of the above. The above surfactants can be well mixed with soy protein isolate, and after subsequent calcination, form a carbon layer together with the soy protein isolate.
[0064] In some embodiments, the concentration of soy protein isolate in the dispersion system is 10-30 mg / ml, and the mass fraction of the surfactant in the dispersion system is 1wt%-3wt%. By further controlling the concentration and content of soy protein isolate and surfactant, the emulsion microspheres are made more stable, and at the same time, the thickness of the carbon layer after calcination is controlled, which is beneficial to improving the rate performance and low-temperature stability of lithium iron phosphate.
[0065] Specifically, the concentration of soy protein isolate in the dispersion system can be 10 mg / ml, 15 mg / ml, 20 mg / ml, 25 mg / ml, 30 mg / ml, etc., and the mass fraction of the surfactant can be 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, etc.
[0066] In some embodiments, an oil phase solvent is added to the dispersion system of soy protein isolate and surfactant to form a mixed system, and the volume ratio of the dispersion system to the oil phase solvent is (3-8):2. By further controlling the volume ratio of the dispersion system to the oil phase solvent, the sphericity of the emulsion microspheres can be higher and the stability can be better, thereby increasing the tap density of the final product.
[0067] Specifically, in the solution system of the dispersion system and the oil phase solvent, the volume ratio of the dispersion system and the oil phase solvent can be 3:2, 2:1, 7:3, 3:1, 4:1, etc.
[0068] In some embodiments, a first iron salt is further added to the emulsion to perform a gelation reaction, wherein the gelation reaction refers to a reaction performed under stirring at room temperature for 10-20 minutes; the feeding ratio of the first iron salt to the dispersion system is (0.1-0.3) mol:1L, and by controlling the concentration of the first iron salt, the soy protein isolate in the emulsion is gelled, so that the soy protein isolate is more tightly bound, thereby improving the stability of the emulsion; on the other hand, the surface of the soy protein isolate is loaded with Fe 3+ Become the reaction center of iron phosphate.
[0069] Specifically, the stirring time of the gelation reaction can be 10 min, 15 min, 20 min, etc.; the feeding ratio of the first iron salt to the dispersion system can be 0.1 mol:1L, 0.2 mol:1L, 0.3 mol:1L, etc.
[0070] In some embodiments, the first iron salt is selected from at least one of ferric chloride and ferric nitrate, and the first iron salt can be any one or more of the above.
[0071] In some embodiments, in the process of preparing the dispersion of the hollow template agent, the soy protein isolate and the surfactant can be first mixed with water to obtain a uniform dispersion system, a certain amount of oil phase solvent is added to the dispersion system, and then stirred at a high speed of 12000-16000 rpm for 3-6 minutes to obtain an emulsion, and the first iron salt is added to the above emulsion and stirred until it is completely dissolved and uniform to obtain gelled emulsion microspheres.
[0072] Specifically, after adding the oil phase solvent to the dispersion system, the mixing stirring speed can be 12000rpm, 13000rpm, 14000rpm, 15000rpm, 16000rpm, etc., and the controlled stirring time can be 3min, 4min, 5min, 6min, etc.
[0073] S2, forming large hollow iron phosphate particles and small solid iron phosphate particles
[0074] The solid template is added to the dispersion of the hollow template, and ethanol is further added to mix evenly to obtain a suspension of the hollow template and the solid template. The addition of ethanol to the solution improves the dispersibility of the nano-iron phosphate in the solution; Fe is loaded on the surface of the hollow template. 3+ It becomes the reaction center of iron phosphate, and the reaction forms large hollow iron phosphate particles; at the same time, the solid template nano-iron phosphate in the aqueous solution acts as a seed, causing the iron phosphate to further grow and form small solid iron phosphate particles.
[0075] Specifically, the solid template is spherical nano-iron phosphate with an average diameter of 200-500 nm (may be 200 nm, 300 nm, 400 nm, 500 nm, etc.).
[0076] In some embodiments, the solid template is added in an amount of 5wt%-10wt% of the mass of the dispersion, and the ethanol is added in an amount of 15%-20% of the volume of the dispersion, and the mixture is stirred well. By controlling the amount of ethanol added, the dispersion degree of the nano-ferric phosphate in the solution system is increased, and the agglomeration of the nano-ferric phosphate is reduced.
[0077] Specifically, the amount of solid template added can be 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt% etc. of the mass of the dispersion; the amount of ethanol added can be 15%, 16%, 17%, 18%, 19%, 20% etc. of the volume of the dispersion.
[0078] In some embodiments, a second iron salt and a phosphorus source are added to a suspension of a hollow template and a solid template to obtain a reaction solution, wherein the concentrations of the second iron salt and the phosphorus source in the reaction solution are both 0.9-2.0 mol / L, and then stirred for reaction. By controlling the concentrations of the second iron salt and the phosphorus source, the shell thickness of the large-particle hollow ferric phosphate and the thickness of the small-particle solid ferric phosphate are controlled.
[0079] Specifically, the second iron salt in the reaction solution is selected from at least one of ferric chloride and ferric nitrate, and the second iron salt can be any one or more of the above; the phosphorus source in the reaction solution is selected from at least one of ammonium hydrogen phosphate, ammonium phosphate, diammonium phosphate, sodium hydrogen phosphate, sodium dihydrogen phosphate and sodium phosphate, and the phosphorus source can be any one or more of the above.
[0080] Furthermore, the concentrations of the second iron salt and the phosphorus source in the reaction solution can be 0.9 mol / L, 1.2 mol / L, 1.4 mol / L, 1.6 mol / L, 1.8 mol / L, 2.0 mol / L, etc.; the molar ratio of the iron element of the second iron salt to the phosphorus element of the phosphorus source in the reaction solution is 1:(1-1.03), such as 1:1, 1:1.01, 1:1.02, 1:1.03, etc.
[0081] In some embodiments, after first controlling the pH of the suspension of the hollow template and the solid template to 1.5-2.2 using an acid and / or a base, a second iron salt and a phosphorus source are added to the suspension of the hollow template and the solid template to obtain a reaction solution, and then stirred for reaction at a stirring speed of 400-500 rpm, a reaction temperature of 60-90° C., and a reaction time of 8-12 h. By controlling the reaction pH value, the reaction stirring speed, the reaction temperature and time, iron phosphate can be uniformly deposited on the surface of the hollow template and the solid template. The acid is at least one of hydrochloric acid, nitric acid, and sulfuric acid; the base is at least one of ammonia water and sodium hydroxide.
[0082] Specifically, the pH of the hollow template and solid template suspensions can be 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.2, etc., the reaction stirring speed can be 400rpm, 500rpm, 600rpm, etc., and the reaction time can be 8h, 9h, 10h, 11h, 12h, etc.
[0083] In some embodiments, after the stirring reaction is completed, solid-liquid separation is performed, and hydrated iron phosphate is obtained through filtration, washing, and drying. The crystal water in the iron phosphate is removed by calcination, and the hollow template agent is carbonized. The calcined iron phosphate material is ground to obtain anhydrous iron phosphate material.
[0084] In some embodiments, the calcination process controls the calcination temperature to be 400-700° C. and the calcination time to be 2-4 hours. By controlling the calcination temperature and time, an ideal particle size and iron phosphate structure can be obtained.
[0085] Specifically, the calcination temperature of the calcination process can be 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, etc., and the calcination time can be 2h, 2.5h, 3h, 3.5h, 4h, etc.
[0086] S3. Calcination with lithium source and carbon source
[0087] The iron phosphate material, lithium source and carbon source obtained in step S2 are calcined, and by optimizing the process of the iron phosphate material, the prepared lithium iron phosphate positive electrode material can have excellent rate performance.
[0088] In some embodiments, the iron phosphate material, the lithium source, the carbon source and ethanol are mixed to obtain a slurry, the slurry is ground and then dried to obtain a lithium iron phosphate precursor powder, and the precursor powder is calcined. The grinding makes the precursor powder more uniform, and the calcination makes the carbon source coated on the surface of the lithium iron phosphate.
[0089] In some embodiments, the lithium source is selected from at least one of lithium oxalate, lithium carbonate and lithium hydroxide, and may be any one or more of the above. By controlling the molar ratio of lithium in the lithium source and iron in iron phosphate during the mixing process, the molar ratio of lithium to iron is (1-1.04):1. By increasing the content of lithium, it is helpful to refine the grains, alleviate the sintering and fusion between the grains, and help improve the rate discharge performance of lithium iron phosphate.
[0090] Specifically, the molar ratio of the lithium element in the lithium source to the iron element in the iron phosphate during the mixing process can be 1.00:1, 1.01:1, 1.02:1, 1.03:1, 1.04:1, etc.
[0091] In some embodiments, the carbon source can be selected from at least one of glucose, sucrose, dopamine, cyclodextrin, citric acid, aniline, cellulose acetate, and polyvinyl pyrrolidone (PVP), and the carbon source is any one or more of the above. After calcination, the carbon source is coated on the surface of the lithium iron phosphate to form a coating layer, forming a carbon layer.
[0092] Specifically, the carbon source is 5%-10% of the total mass of the iron phosphate material and the lithium source, such as 5%, 6%, 7%, 8%, 9%, 10%, etc.
[0093] In some embodiments, ethanol is mixed as a dispersant to form a slurry, the slurry is ground for 2-6 hours, and then dried at 60-80° C. The dried lithium iron phosphate precursor powder is calcined at 700-850° C. for 6-15 hours in a nitrogen atmosphere to obtain lithium iron phosphate.
[0094] Specifically, the grinding time of the slurry can be 2h, 3h, 4h, 5h, 6h, etc., the drying temperature can be 60°C, 70°C, 80°C, etc., the calcination temperature can be 700°C, 750°C, 800°C, 850°C, etc., and the calcination time can be 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, etc.
[0095] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0096] Example 1
[0097] A method for preparing an iron phosphate material comprises the following steps:
[0098] (1) Adding soy protein isolate and polyoxyethylene sorbitan monooleate to deionized water and stirring to form a dispersion system, wherein the concentration of the soy protein isolate is 20 mg / ml, and the mass percentage of the polyoxyethylene sorbitan monooleate in the dispersion system is 2 wt%. The dispersion system is mixed with heptane at a volume ratio of 7:3, and stirred at a speed of 15000 rpm for 4 minutes; adding ferric chloride salt, the feeding ratio of ferric chloride to the dispersion system is 0.2 mol: 1 L, and stirring at room temperature for 15 minutes to obtain a dispersion of a hollow template agent.
[0099] (2) Spherical nano-iron phosphate with an average diameter of 350 nm, i.e., a solid template, is added to the above dispersion at a rate of 8 wt % of the mass of the dispersion, and 18 wt % of ethanol is added to the dispersion at the same time, and the mixture is stirred evenly. The pH of the solution is adjusted to 1.6 using hydrochloric acid or ammonia water, and then ammonium hydrogen phosphate and ferric chloride are added to obtain a reaction solution, wherein the concentration of the iron element in the reaction solution after the ferric chloride is added is 1 mol / L, and the concentration of the ammonium hydrogen phosphate in the reaction solution is 1.01 mol / L. The mixture is stirred at a speed of 400 rpm, and the reaction is stirred at a temperature of 70° C. for 9 h. After filtering, washing, and drying, a hydrated iron phosphate material is obtained, and the iron phosphate material is obtained after calcining at 500° C. in a nitrogen atmosphere for 3 h.
[0100] The TEM image of the iron phosphate material obtained in this example is as follows Figure 2 As shown by Figure 2 It can be seen that the iron phosphate material contains both large-particle hollow iron phosphate material and small-particle solid iron phosphate material, wherein the large-particle hollow iron phosphate material has a carbon layer on the inner surface of the shell, the average particle size corresponding to the large-particle hollow iron phosphate material is 3.4μm, the average shell thickness of the large-particle hollow iron phosphate material is 480nm, the average thickness of the carbon layer on the inner surface of the shell of the large-particle hollow iron phosphate material is 150nm, and the average particle size corresponding to the small-particle solid iron phosphate material is 1.5μm.
[0101] A method for preparing a lithium iron phosphate material comprises the following steps:
[0102] The above-mentioned iron phosphate material and lithium hydroxide are mixed in a ratio of iron to lithium of 1:1.02, glucose accounting for 8wt% of the total mass of the iron phosphate material and lithium hydroxide is added, and then ethanol is used as a dispersant to obtain a mixed material, wherein the amount of ethanol added is 2.5wt% of the total mass of the mixed material. The mixed material is placed in a grinder for grinding and stirring for 5 hours, and then placed in a 70°C drying oven for drying; the dried mixed material is placed in a tubular furnace and calcined at 850°C for 9 hours in a nitrogen atmosphere to obtain a lithium iron phosphate material.
[0103] The preparation steps of lithium iron phosphate refer to the instructions. Figure 1 .
[0104] Example 2
[0105] A method for preparing an iron phosphate material comprises the following steps:
[0106] (1) Adding soy protein isolate and polyoxyethylene fatty alcohol ether to deionized water and stirring to form a dispersion system, wherein the concentration of the soy protein isolate is 10 mg / ml, and the mass percentage of the polyoxyethylene fatty alcohol ether in the dispersion system is 1 wt%. The dispersion system is mixed with vegetable oil in a volume ratio of 3:2, and stirred at a speed of 12000 rpm for 4 minutes; adding ferric chloride salt, the feeding ratio of ferric chloride to the dispersion system is 0.1 mol: 1 L, and stirring at room temperature for 10 minutes to obtain a dispersion of a hollow template agent.
[0107] (2) Spherical nano-iron phosphate with an average diameter of 350 nm, i.e., a solid template, is added to the above dispersion at a rate of 5 wt % of the mass of the dispersion, and 15% of ethanol by volume of the dispersion is added, stirred evenly, and the pH of the solution is adjusted to 1.5 using hydrochloric acid or ammonia water, and then ammonium hydrogen phosphate and ferric chloride are added to obtain a reaction solution, wherein the concentration of iron element in the reaction solution after the addition of ferric chloride is 0.9 mol / L, and the concentration of ammonium hydrogen phosphate in the reaction solution is 0.92 mol / L, and the mixture is stirred at a speed of 400 rpm, and the reaction is stirred at a temperature of 70° C. for 9 hours, and then filtered, washed, and dried to obtain a hydrated iron phosphate material, which is calcined at 500° C. in a nitrogen atmosphere for 3 hours to obtain an iron phosphate material.
[0108] The obtained iron phosphate material was subjected to TEM testing, wherein the large-particle hollow iron phosphate material had a carbon layer on the inner surface of the shell, the average particle size corresponding to the large-particle hollow iron phosphate material was 3.8μm, the average shell thickness of the large-particle hollow iron phosphate material was 350nm, the average thickness of the carbon layer on the inner surface of the shell of the large-particle hollow iron phosphate material was 108nm, and the average particle size corresponding to the small-particle solid iron phosphate material was 2.0μm.
[0109] A method for preparing a lithium iron phosphate material comprises the following steps:
[0110] The above-mentioned iron phosphate material and lithium hydroxide are mixed in a ratio of iron to lithium of 1:1, sucrose accounting for 5wt% of the total mass of the iron phosphate material and the lithium hydroxide is added, and then ethanol is used as a dispersant to obtain a mixed material, wherein the amount of ethanol added is 2.5wt% of the total mass of the mixed material. The mixed material is placed in a grinder for grinding and stirring for 6 hours, and then placed in a 60°C drying oven for drying; the dried mixed material is placed in a tubular furnace and calcined at 700°C for 15 hours in a nitrogen atmosphere to obtain a lithium iron phosphate material.
[0111] Example 3
[0112] A method for preparing an iron phosphate material comprises the following steps:
[0113] (1) Add soy protein isolate and fatty alcohol polyoxyethylene ether to deionized water and stir to form a dispersion system, wherein the concentration of the soy protein isolate is 30 mg / ml and the mass percentage of the fatty alcohol polyoxyethylene ether in the dispersion system is 3 wt %. The dispersion system is mixed with n-hexane at a volume ratio of 4:1, and stirred at a speed of 16000 rpm for 4 minutes; then add ferric chloride salt, and the feeding ratio of ferric chloride to the dispersion system is 0.3 mol: 1 L, and stir at room temperature for 20 minutes to obtain a dispersion of a hollow template agent.
[0114] (2) Spherical nano-iron phosphate with an average diameter of 350 nm, i.e., a solid template, is added to the above dispersion at a rate of 10 wt % of the mass of the dispersion, and 20% of ethanol by volume of the dispersion is added, stirred evenly, and the pH of the solution is adjusted to 2.2 using hydrochloric acid or ammonia water, and then ammonium hydrogen phosphate and ferric chloride are added to obtain a reaction solution, wherein the concentration of iron element in the reaction solution after the addition of ferric chloride is 1.98 mol / L, and the concentration of ammonium hydrogen phosphate in the reaction solution is 2.00 mol / L, and the mixture is stirred at a speed of 400 rpm, and the reaction is stirred at a temperature of 70° C. for 9 hours, and then filtered, washed, and dried to obtain a hydrated iron phosphate material, which is calcined at 700° C. in a nitrogen atmosphere for 2 hours to obtain an iron phosphate material.
[0115] The obtained iron phosphate material was subjected to TEM test, and the observation results were consistent with Figure 2 Similarly, there is a carbon layer on the inner surface of the shell of the large-particle hollow iron phosphate material. The average particle size corresponding to the large-particle hollow iron phosphate material is 2.6μm, the average shell thickness of the large-particle hollow iron phosphate material is 650nm, the average thickness of the carbon layer on the inner surface of the shell of the large-particle hollow iron phosphate material is 186nm, and the average particle size corresponding to the small-particle solid iron phosphate material is 1.2μm.
[0116] A method for preparing a lithium iron phosphate material comprises the following steps:
[0117] The above-mentioned iron phosphate material and lithium hydroxide are mixed in a ratio of iron to lithium of 1:1.04, cyclodextrin accounting for 10wt% of the total mass of the iron phosphate material and lithium hydroxide is added, and then ethanol is used as a dispersant to obtain a mixed material, wherein the amount of ethanol added is 2.5wt% of the total mass of the mixed material. The mixed material is placed in a grinder for grinding and stirring for 6 hours, and then placed in a drying oven at 80°C for drying; the dried mixed material is placed in a tubular furnace and calcined at 850°C for 9 hours in a nitrogen atmosphere to obtain a lithium iron phosphate material.
[0118] Example 4
[0119] The only difference between this embodiment and embodiment 1 is that the feeding ratio of ferric chloride to the dispersion system in step (1) is 0.1 mol:1 L, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0120] The obtained iron phosphate material was subjected to TEM testing, wherein the large-particle hollow iron phosphate material had a carbon layer on the inner surface of the shell, the average particle size corresponding to the large-particle hollow iron phosphate material was 3.6 μm, the average shell thickness of the large-particle hollow iron phosphate material was 450 nm, the average thickness of the carbon layer on the inner surface of the shell of the large-particle hollow iron phosphate material was 140 nm, and the average particle size corresponding to the small-particle solid iron phosphate material was 2.0 μm.
[0121] Example 5
[0122] The only difference between this embodiment and embodiment 1 is that the feeding ratio of ferric chloride to the dispersion system in step (1) is 0.3 mol:1 L, and the other conditions and parameters are exactly the same as those in embodiment 1.
[0123] The obtained iron phosphate material was subjected to TEM testing, wherein the large-particle hollow iron phosphate material had a carbon layer on the inner surface of the shell, the average particle size corresponding to the large-particle hollow iron phosphate material was 3.5 μm, the average shell thickness of the large-particle hollow iron phosphate material was 500 nm, the average thickness of the carbon layer on the inner surface of the shell of the large-particle hollow iron phosphate material was 130 nm, and the average particle size corresponding to the small-particle solid iron phosphate material was 1.6 μm.
[0124] Example 6
[0125] The only difference between this embodiment and embodiment 1 is that in step (2), spherical nano-iron phosphate with an average diameter of 350 nm is added to the above dispersion at 5 wt % of the mass of the dispersion, and other conditions and parameters are exactly the same as those in embodiment 1.
[0126] The obtained iron phosphate material was subjected to TEM testing, wherein the large-particle hollow iron phosphate material had a carbon layer on the inner surface of the shell, the average particle size corresponding to the large-particle hollow iron phosphate material was 3.5 μm, the average shell thickness of the large-particle hollow iron phosphate material was 490 nm, the average thickness of the carbon layer on the inner surface of the shell of the large-particle hollow iron phosphate material was 150 nm, and the average particle size corresponding to the small-particle solid iron phosphate material was 1.2 μm.
[0127] Example 7
[0128] The difference between this embodiment and embodiment 1 is that in step (2), spherical nano-iron phosphate with an average diameter of 350 nm is added to the above solution at 10 wt % of the mass of the dispersion, and other conditions and parameters are exactly the same as those in embodiment 1.
[0129] The obtained iron phosphate material was subjected to TEM testing, wherein the large-particle hollow iron phosphate material had a carbon layer on the inner surface of the shell, the average particle size corresponding to the large-particle hollow iron phosphate material was 3.4 μm, the average shell thickness of the large-particle hollow iron phosphate material was 460 nm, the average thickness of the carbon layer on the inner surface of the shell of the large-particle hollow iron phosphate material was 150 nm, and the average particle size corresponding to the small-particle solid iron phosphate material was 1.6 μm.
[0130] Example 8
[0131] The only difference between this embodiment and embodiment 1 is that 15% ethanol by volume of the dispersion is added in step (2), and the other conditions and parameters are exactly the same as those in embodiment 1.
[0132] The obtained iron phosphate material was subjected to TEM testing, wherein the large-particle hollow iron phosphate material had a carbon layer on the inner surface of the shell, the average particle size corresponding to the large-particle hollow iron phosphate material was 3.4 μm, the average shell thickness of the large-particle hollow iron phosphate material was 470 nm, the average thickness of the carbon layer on the inner surface of the shell of the large-particle hollow iron phosphate material was 150 nm, and the average particle size corresponding to the small-particle solid iron phosphate material was 1.6 μm.
[0133] Example 9
[0134] The only difference between this embodiment and embodiment 1 is that 20% ethanol by volume of the dispersion is added in step (2), and the other conditions and parameters are exactly the same as those in embodiment 1.
[0135] The obtained iron phosphate material was subjected to TEM testing, wherein the large-particle hollow iron phosphate material had a carbon layer on the inner surface of the shell, the average particle size corresponding to the large-particle hollow iron phosphate material was 3.4 μm, the average shell thickness of the large-particle hollow iron phosphate material was 490 nm, the average thickness of the carbon layer on the inner surface of the shell of the large-particle hollow iron phosphate material was 150 nm, and the average particle size corresponding to the small-particle solid iron phosphate material was 1.4 μm.
[0136] Comparative Example 1
[0137] The main difference from Example 1 is that the dispersed system in step (1) does not add soy protein isolate, and the specific steps are as follows:
[0138] (1) Add polyoxyethylene sorbitan monooleate to deionized water and stir to form a dispersion system, wherein the mass percentage of polyoxyethylene sorbitan monooleate in the dispersion system is 3wt%. The dispersion system is mixed with heptane at a volume ratio of 7:3, and stirred at a speed of 15000 rpm for 4 minutes; then ferric chloride is added, and the feeding ratio of ferric chloride to the dispersion system is 0.2 mol: 1 L, and stirred at room temperature for 15 minutes to obtain an emulsion dispersion.
[0139] (2) Spherical nano-iron phosphate with an average diameter of 350 nm, i.e., a solid template, is added to the above dispersion at a rate of 8 wt % of the mass of the dispersion, and 18 wt % of ethanol by volume of the above dispersion is added, stirred evenly, and the pH of the solution is adjusted to 1.6 using hydrochloric acid or ammonia water, and then sodium hydrogen phosphate and ferric chloride are added to obtain a reaction solution, wherein the concentration of iron element in the reaction solution after the addition of ferric chloride is 1 mol / L, and the concentration of sodium hydrogen phosphate in the reaction solution is 1.01 mol / L. The mixture is stirred at a speed of 400 rpm, and the reaction is stirred at a temperature of 70° C. for 9 h. After filtering, washing, and drying, a hydrated iron phosphate material is obtained, which is calcined at 500° C. in a nitrogen atmosphere for 3 h to obtain an iron phosphate material.
[0140] The iron phosphate material obtained in this embodiment includes hollow iron phosphate and solid iron phosphate material, wherein the hollow iron phosphate is irregular in shape.
[0141] A method for preparing a lithium iron phosphate material comprises the following steps:
[0142] The above-mentioned iron phosphate material and lithium hydroxide are mixed in a ratio of iron to lithium of 1:1.02, glucose accounting for 8wt% of the total mass of the iron phosphate material and lithium hydroxide is added, and then ethanol is used as a dispersant to obtain a mixed material, wherein the amount of ethanol added is 2.5wt% of the total mass of the mixed material. The mixed material is placed in a grinder for grinding and stirring for 5 hours, and then placed in a 70°C drying oven for drying; the dried mixed material is placed in a tubular furnace, and kept warm at 850°C for 9 hours under a nitrogen atmosphere to obtain a lithium iron phosphate material.
[0143] Comparative Example 2
[0144] The main difference from Example 1 is that no surfactant is added to the dispersion system in step (1). The specific steps are as follows:
[0145] (1) Add soy protein isolate to deionized water and stir to form a dispersion system, wherein the concentration of the soy protein isolate is 20 mg / ml. The dispersion system solution is mixed with heptane in a volume ratio of 7:3, and the mixture is stirred at a speed of 15000 rpm for 4 minutes; ferric chloride is added, and the feeding ratio of ferric chloride to the dispersion system is 0.2 mol: 1 L, and the mixture is stirred at room temperature for 15 minutes to obtain a dispersion liquid of a gelled soy protein isolate emulsion.
[0146] (2) Spherical nano-iron phosphate with an average diameter of 350 nm, i.e., a solid template, is added to the above dispersion at a rate of 8 wt % of the mass of the dispersion, and 18 wt % of ethanol is added to the dispersion at the same time, and the mixture is stirred evenly. The pH of the solution is adjusted to 1.6 using hydrochloric acid or ammonia water, and then sodium hydrogen phosphate and ferric chloride are added to obtain a reaction solution, wherein the concentration of the iron element in the reaction solution after the ferric chloride is added is 1 mol / L, and the concentration of the sodium hydrogen phosphate in the reaction solution is 1.01 mol / L. The mixture is stirred at a speed of 400 rpm, and the reaction is stirred at a temperature of 70° C. for 9 h. After filtering, washing, and drying, a hydrated iron phosphate material is obtained, and the iron phosphate material is obtained after calcining at 500° C. in a nitrogen atmosphere for 3 h.
[0147] The iron phosphate material obtained in this comparative example includes hollow iron phosphate and solid iron phosphate materials, wherein the hollow iron phosphate is irregular in shape.
[0148] A method for preparing a lithium iron phosphate material comprises the following steps:
[0149] The above-mentioned iron phosphate material and lithium hydroxide are mixed in a ratio of iron to lithium of 1:1.02, glucose accounting for 8wt% of the total mass of the iron phosphate material and lithium hydroxide is added, and then ethanol is used as a dispersant to obtain a mixed material, wherein the amount of ethanol added is 2.5wt% of the total mass of the mixed material. The mixed material is placed in a grinder for grinding and stirring for 5 hours, and then placed in a 70°C drying oven for drying; the dried mixed material is placed in a tubular furnace, and kept warm at 850°C for 9 hours under a nitrogen atmosphere to obtain a lithium iron phosphate material.
[0150] Comparative Example 3:
[0151] A method for preparing an iron phosphate material, comprising the following steps:
[0152] (1) Adding soy protein isolate and polyoxyethylene sorbitan monooleate to deionized water, stirring evenly to form a dispersion system, wherein the concentration of the soy protein isolate is 20 mg / ml, and the mass percentage of polyoxyethylene sorbitan monooleate in the dispersion system is 2 wt %; then adding ferric chloride to a concentration of 0.2 mol / L in the dispersion system, and stirring at room temperature for 15 min.
[0153] (2) The above dispersion system was mixed with heptane in a volume ratio of 7:3, and the mixture was stirred at a speed of 15,000 rpm for 4 minutes to obtain a dispersion liquid; the dispersion liquid was a flocculent suspension of soybean protein and could not form a stable emulsion.
[0154] Spherical nano-iron phosphate with an average diameter of 350 nm, i.e., a solid template, is added to the above dispersion at 8wt% of the mass of the dispersion, and 18% of ethanol by volume of the dispersion is added, stirred evenly, and the pH of the solution is adjusted to 1.6 using hydrochloric acid or ammonia water, and then sodium hydrogen phosphate and ferric chloride are added to obtain a reaction solution, wherein the concentration of the iron element in the reaction solution after the addition of ferric chloride is 1 mol / L, and the concentration of the sodium hydrogen phosphate solution is 1.01 mol / L. The reaction is stirred at a speed of 400 rpm, and the reaction is stirred at a temperature of 70°C for 9 hours. After filtering, washing, and drying, a hydrated iron phosphate material is obtained, and the iron phosphate material is obtained after calcining at 500°C in a nitrogen atmosphere for 3 hours.
[0155] The iron phosphate material obtained in this comparative example consists of irregular iron phosphate particles and solid iron phosphate.
[0156] A method for preparing a lithium iron phosphate material comprises the following steps:
[0157] The above-mentioned iron phosphate material and lithium hydroxide are mixed in a ratio of iron to lithium of 1:1.02, glucose accounting for 8wt% of the total mass of the iron phosphate material and lithium hydroxide is added, and then ethanol is used as a dispersant to obtain a mixed material, wherein the amount of ethanol added is 2.5wt% of the total mass of the mixed material. The mixed material is placed in a grinder for grinding and stirring for 5 hours, and then placed in a 60°C drying oven for drying; the dried mixed material is placed in a tubular furnace, and kept warm at 850°C for 9 hours under a nitrogen atmosphere to obtain a lithium iron phosphate material.
[0158] Effect Example 1
[0159] In order to verify the product of the present invention and the use effect of the product, the lithium iron phosphate material prepared in each embodiment and comparative example was used to prepare a simulated battery, and the preparation method was as follows:
[0160] A uniform slurry was prepared by mixing lithium iron phosphate, acetylene black and binder PVDF in a mass ratio of 75:15:10 and evenly coated on an aluminum foil substrate as the positive electrode of the simulated battery. The negative electrode of the simulated battery used a lithium sheet, a polypropylene porous membrane was used as a diaphragm, and the electrolyte was 1 mol LiPF6 dissolved in 1L of a mixed solvent of ethylene carbonate and dimethyl carbonate (volume ratio 1:1). The positive electrode, negative electrode, electrolyte and diaphragm were assembled into a battery in an argon-protected glove box.
[0161] The obtained simulated battery was subjected to rate performance test at a voltage of 2.0V-4.2V. The specific test steps are as follows:
[0162] First, charge to 4.2V with constant current, then discharge to 2.0V with rate current, the released capacity is the discharge capacity at this rate, after discharge, discharge to 2.0V with constant current again; then test at the next rate. The test results are shown in Table 1.
[0163] Effect Example 2
[0164] In order to verify the performance of the lithium iron phosphate product of the present invention, the lithium iron phosphate materials prepared in each embodiment and comparative example were subjected to a tap density test, and the specific steps were as follows:
[0165] Weigh the mass of the dry measuring cylinder m1 (g) and add a certain amount of solid sample (about 5 ml) into the measuring cylinder. Block the mouth of the measuring cylinder and vibrate the measuring cylinder vertically until the volume of the sample in the cylinder stops decreasing. Record the sample volume V (ml). Weigh the mass of the measuring cylinder + sample m2 (g); use the formula ρ = (m2-m1) / V to get ρ (g / cm 3 ) is the tap density of the sample to be tested. The results are shown in Table 1.
[0166] Effect Example 3
[0167] In order to verify the performance of the lithium iron phosphate product of the present invention, the lithium iron phosphate materials prepared in each embodiment and comparative example were subjected to specific surface area testing, specifically using a BETA201A fully automatic static capacity method specific surface and pore size analysis tester. The results are shown in Table 1.
[0168] Table 1 Performance test results of positive electrode materials in embodiments and comparative examples
[0169]
[0170] As can be seen from Table 1, the lithium iron phosphate products prepared by Examples 1-3 and Comparative Examples 1-3 have ideal physical and chemical properties, and the specific surface area of each product can reach 20.12 m 2 / g or more, the tap density of each product can reach 1.20g / cm 3 In the rate performance test, the 0.2C discharge specific capacity can reach more than 161mAh / g, the 2C discharge specific capacity can reach more than 146mAh / g, and the 5C discharge specific capacity can reach more than 141mAh / g. Even if the rate performance reaches 10C, the discharge specific capacity of the products in each embodiment can reach more than 130mAh / g.
[0171] In comparative example 1, no soy protein isolate is added during the preparation of the hollow template agent. The iron phosphate material obtained under this embodiment includes hollow iron phosphate and solid iron phosphate material. Only using a surfactant will reduce the stability of the hollow template agent. In the reaction solution containing the solid template agent, the hollow template agent is easily deformed or even destroyed, and the hollow iron phosphate formed is finally irregular in shape; in comparative example 2, no surfactant is added during the preparation of the hollow template agent. The iron phosphate material obtained under this embodiment includes hollow iron phosphate and solid iron phosphate material. Since only soy protein isolate is used, the soy protein isolate in the hollow template agent has a certain degree of aggregation during the gelation process, causing the hollow template to deform or even break, and finally causing the hollow iron phosphate to be mostly irregular in shape; in comparative example 3, iron salt is first added during the preparation of the hollow template agent and then the emulsion is prepared. In the iron phosphate material obtained under this embodiment, since the iron salt and soy protein isolate are first added for gelation reaction, it can no longer form a hollow template agent, and finally irregular solid iron phosphate particles and spherical solid iron phosphate are formed. Therefore, the specific surface area, tap density and rate performance of the lithium iron phosphate materials prepared by Comparative Examples 1-3 are all affected. As shown in Table 1, the performance parameters corresponding to the products of Examples 1-3 are significantly better than the performance parameters of the products of Comparative Examples 1-3.
[0172] By comparing Example 1 with Examples 4-5, it can be seen that in the preparation process of the iron phosphate of the present invention, the first iron salt is added to the gelation treatment of the emulsion, and the feeding ratio of the first iron salt to the dispersion system in step (1) is controlled at (0.1-0.3) mol: 1L. If the proportion of the first iron salt in the dispersion system is too low, the gelation degree will be too low, the stability of the hollow template agent will be poor, and the morphology of the iron phosphate material prepared by the hollow template agent will be affected, and further the rate performance of the lithium iron phosphate positive electrode material inheriting the morphology of the iron phosphate material will be reduced, and the tap density and specific surface area will be reduced; if the proportion of the first iron salt in the dispersion system is too high, the gelation degree of the soy protein isolate of the hollow template agent will be too high, and the stability and sphericity of the hollow template agent will be destroyed. Similarly, the rate performance of the lithium iron phosphate positive electrode material will be reduced, and the tap density and specific surface area of the lithium iron phosphate positive electrode material will be reduced. Therefore, the feeding ratio of the first iron salt to the dispersion system is controlled at (0.1-0.3) mol:1L, and the performance of the lithium iron phosphate positive electrode material made from the iron phosphate obtained within this range is better.
[0173] By comparing Example 1 with Example 6-7, it can be obtained that in the preparation process of iron phosphate of the present invention, the amount of solid template agent added affects the proportion of small-particle solid iron phosphate material in the product, and the amount of solid template agent added in step (2) is controlled to be 5wt%-10wt% of the mass of the dispersion. If the content of the solid template agent added is too low, the proportion of small-particle solid iron phosphate material is reduced, further resulting in a decrease in the tap density of the lithium iron phosphate positive electrode material inheriting the morphology of the iron phosphate material; if the content of the solid template agent added is too much, it will affect the stability of the hollow template agent, reduce the sphericity of the hollow template agent, and increase the proportion of small-particle solid iron phosphate in the iron phosphate product, further resulting in a decrease in the tap density and specific surface area of the lithium iron phosphate positive electrode material inheriting the morphology of the iron phosphate material, and a decrease in rate performance. Therefore, the amount of solid template agent added is controlled to be 5wt%-10wt% of the mass of the dispersion, and the iron phosphate material prepared within this range has better performance in preparing the lithium iron phosphate positive electrode material.
[0174] By comparing Example 1 with Example 8-9, it can be seen that in the preparation process of the iron phosphate material of the present invention, the addition of ethanol affects the dispersibility of the solid template agent, and the amount of ethanol added in step (2) is controlled to be 15wt%-20wt% of the volume of the dispersion. If the ethanol content added is too little, the agglomeration of the solid template agent is increased, and the average particle size of the small solid iron phosphate particles in the iron phosphate product becomes larger, which further leads to a decrease in the tap density and specific surface area of the lithium iron phosphate positive electrode material inheriting the morphology of the iron phosphate material; if the ethanol content added is too much, on the basis of causing an increase in economic costs, the lithium iron phosphate positive electrode material prepared from the iron phosphate cannot be substantially improved in physical and chemical properties. Therefore, the amount of ethanol added is controlled to be 15wt%-20wt% of the volume of the dispersion, and the performance of the lithium iron phosphate positive electrode material prepared from the iron phosphate material prepared within this range is better.
[0175] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. An iron phosphate material, It is characterized in that The iron phosphate material comprises large hollow iron phosphate particles and small solid iron phosphate particles. The large hollow iron phosphate particles comprise an iron phosphate shell layer and a carbon layer on the inner surface of the iron phosphate shell layer.
2. The iron phosphate material according to claim 1, It is characterized in that The iron phosphate material has at least one of the following features 1 to 3: Feature 1: The average particle size of the large-particle hollow iron phosphate is in the range of 2.0 μm to 4.0 μm, and the average particle size of the small-particle solid iron phosphate is in the range of 0.9 μm to 2 μm; Feature 2: The thickness of the iron phosphate shell layer is 300nm-700nm; Feature 3: The thickness of the carbon layer on the inner surface of the iron phosphate shell layer is 100nm-200nm.
3. A method for preparing the iron phosphate material according to any one of claims 1 to 2, It is characterized in that The following steps are involved: The solid template is added to the dispersion of the hollow template to obtain a suspension, a second iron salt and a phosphorus source are added to the suspension to obtain a reaction solution, the reaction is stirred, and the obtained solid is calcined to obtain the iron phosphate material.
4. A method for preparing an iron phosphate material according to claim 3, It is characterized in that The preparation steps of the dispersion of the hollow template agent include: After the soy protein isolate, surfactant and water are mixed to form a dispersion system, the dispersion system is mixed and stirred with an oil phase solvent to obtain an emulsion, and a first iron salt is added to the emulsion for gelation reaction to obtain a dispersion of the hollow template agent.
5. A method for preparing an iron phosphate material according to claim 3, It is characterized in that The suspension also includes ethanol, and the mixing order of the components is to first prepare a dispersion of the hollow template agent, then add the solid template agent to the dispersion and mix evenly, and finally add ethanol and stir evenly; the preparation method of the iron phosphate material satisfies at least one of the following preparation conditions ① to ⑨: Condition ①: The amount of ethanol added is 15%-20% of the volume of the dispersion; Condition ②: The concentration of the phosphorus source in the reaction solution is 0.9-2 mol / L; Condition ③: The molar ratio of iron to phosphorus in the reaction solution is 1:(1-1.03); Condition ④: The solid template is a spherical nano-iron phosphate with an average diameter of 200-500 nm; Condition ⑤: The amount of the solid template added is 5wt%-10wt% of the mass of the dispersion; Condition ⑥: the second iron salt comprises at least one of ferric chloride or ferric nitrate; Condition ⑦: The phosphorus source includes at least one of ammonium hydrogen phosphate, ammonium phosphate, ammonium dihydrogen phosphate, sodium hydrogen phosphate, sodium dihydrogen phosphate and sodium phosphate; Condition ⑧: The stirring reaction has a stirring speed of 400-500 rpm, a reaction temperature of 60-90° C., and a reaction time of 8-12 h; Condition ⑨: During the calcination process, the calcination temperature is controlled to be 400-700°C and the calcination time is 2-4h.
6. A method for preparing an iron phosphate material according to claim 4, It is characterized in that The preparation of the dispersion of the hollow template agent satisfies at least one of the following conditions I to VII: Condition I: The stirring speed of the mixing and stirring is 12000-16000 rpm, and the stirring time is 3-6 min; Condition II: the surfactant includes at least one of polyoxyethylene fatty alcohol ether, alkyl glycoside compound, polyoxyethylene sorbitan monooleate, alkylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether, polyoxyethylene fatty amine, polyoxyethylene castor oil, and polyoxyethylene oleyl ether; the mass fraction of the surfactant in the dispersion is 1wt%-3wt%; Condition III: the concentration of the soy protein isolate in the dispersion is 10-30 mg / ml; Condition IV: The oil phase solvent includes at least one of kerosene, heptane, n-hexane, cyclohexane, vegetable oil, and liquid paraffin; Condition V: The volume ratio of the dispersion system to the oil phase solvent is (3-8):2; Condition VI: The gelation reaction is a reaction carried out under stirring at room temperature for 10-20 minutes; Condition VII: The first iron salt includes at least one of ferric chloride and ferric nitrate; the feed ratio of the first iron salt to the dispersion is (0.1-0.3) mol:1L.
7. A method for preparing lithium iron phosphate material, It is characterized in that The iron phosphate material, lithium source, carbon source and ethanol are mixed to obtain a slurry, and the slurry is ground and dried, and then calcined in an inert atmosphere to obtain a lithium iron phosphate material; the iron phosphate material is the iron phosphate material according to any one of claims 1-2.
8. A method for preparing a lithium iron phosphate material according to claim 7, It is characterized in that The preparation method satisfies at least one of the following conditions a to f: Condition a: The lithium source is selected from at least one of lithium oxalate, lithium carbonate and lithium hydroxide; Condition b: the carbon source is selected from at least one of glucose, sucrose, dopamine, cyclodextrin, citric acid, aniline, cellulose acetate, and polyvinyl pyrrolidone; Condition c: the carbon source is 5%-10% of the total mass of the lithium source and the iron phosphate material; Condition d: the slurry grinding time is 2-6h; Condition e: the calcination temperature is 700-850°C, and the calcination time is 6-15h; Condition f: The inert atmosphere is selected from at least one of nitrogen, helium and argon.
9. A lithium iron phosphate material obtained according to any one of the preparation methods of claims 7-8, It is characterized in that The lithium iron phosphate material includes large-particle hollow lithium iron phosphate and small-particle solid lithium iron phosphate; The large-particle hollow lithium iron phosphate comprises a lithium iron phosphate shell layer, a first carbon coating layer on the outer surface of the lithium iron phosphate shell layer, and a carbon layer on the inner surface of the lithium iron phosphate shell layer; The small-particle solid lithium iron phosphate comprises lithium iron phosphate and a second carbon coating layer on the outer surface of the lithium iron phosphate.
10. A positive electrode sheet, It is characterized in that The positive electrode plate comprises the lithium iron phosphate material according to claim 9.
Citation Information
Patent Citations
Hollow carbon-coated lithium iron phosphate particles as well as preparation method and application thereof
CN113540455A
Lithium iron phosphate material, preparation method thereof and battery
CN114725374A
Method for promoting soybean to enhance nodulation and increase yield by applying iron-based nano material on leaves
CN115885800A
Multi-channel iron phosphate precursor, lithium iron phosphate material and preparation method of multi-channel iron phosphate precursor and lithium iron phosphate material
CN117916196A
Composite iron phosphate as well as preparation method and application thereof
CN118183666A