Method for synthesizing lithium iron manganese phosphate from positive electrode material of retired lithium iron phosphate battery
Through MnO2 oxidation and hydrothermal synthesis technology, the high energy consumption and pollution problems in the recycling and processing of retired lithium iron phosphate battery cathode materials have been solved, and efficient and environmentally friendly recovery and regeneration of lithium iron manganese phosphate materials have been achieved, which has improved energy density and products. uniformity.
Patent Information
- Application Number
- CN202410909940.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-01
AI Technical Summary
The recycling of retired lithium iron phosphate battery cathode materials has problems of high energy consumption and pollution. It is difficult for existing technologies to effectively reduce energy consumption and increase the recycling rate. At the same time, the growth of the new energy vehicle market has led to an increase in the amount of retired materials, which requires an efficient and environmentally friendly recycling method. and regeneration methods.
Use MnO2 oxidation and sulfuric acid leaching technology to treat waste lithium iron phosphate battery cathode materials, combined with hydrothermal synthesis method, by introducing Mn ions and adjusting the proportion of leachate, to prepare lithium iron manganese phosphate (LiMnxFe(1-x)PO4) material, using MnO2 The oxidizing property and the reducing property of LiFePO4 realize the recovery of multiple elements, and control the particle size and structure through hydrothermal reaction and calcination steps.
It realizes the efficient recovery and regeneration of used lithium iron phosphate battery cathode materials, reduces energy consumption, improves the uniformity and energy density of the product, and avoids the release of harmful gases during high-temperature calcination, which has environmental protection and economic advantages.
Smart Images

Figure HDA0004933280130000011 
Figure HDA0004933280130000012
Abstract
Description
Technical Field
[0001] The invention belongs to the field of resource recycling and utilization, and mainly relates to a method for synthesizing lithium iron manganese phosphate from retired lithium iron phosphate battery positive electrode materials. Background Art
[0002] Lithium-ion battery is a secondary battery that charges and discharges the battery by the movement of lithium ions between two electrodes. It is usually used in power batteries, energy storage batteries, consumer batteries, etc. Lithium iron phosphate battery is a type of lithium-ion battery, and its positive electrode material is LiFePO4 (LFP). Lithium iron phosphate battery has the advantages of high stability and long cycle life, and is widely used in low-end and mid-range electric vehicles. With the rise of the energy storage market, lithium iron phosphate batteries with better safety and higher energy density are slowly replacing traditional lead-acid batteries. In addition, in the new energy vehicle industry, the market share of low-cost lithium iron phosphate batteries has exceeded that of expensive ternary batteries in 2022. With the rapid growth of new energy vehicle ownership, the number of retired power batteries is also increasing year by year. If these batteries are not properly handled, it will cause a waste of valuable metals and may also bring serious health and environmental problems. Taking 2022 as an example, the proportion of lithium iron phosphate batteries in power batteries has reached 60%. With the increase in market usage, the amount of lithium iron phosphate batteries retired in the future is bound to increase accordingly.
[0003] Lithium, as a precious metal, is an important industrial raw material. The positive electrode material is the core of the entire lithium battery. Researchers have tried a variety of technologies to recycle the positive electrode materials of waste lithium iron phosphate batteries, mainly divided into valuable metal recovery and battery recycling.
[0004] Pyrometallurgy can achieve the conversion and recovery of Li in waste LiFePO4 positive electrode materials through high-temperature roasting, but high energy consumption and high pollution are also problems that need to be solved. Compared with the pyrometallurgical process, wet recovery has the advantages of low energy consumption, high metal recovery rate, safety and environmental protection. The wet recovery technology of LFP batteries mainly adopts oxidative acid leaching technology. According to the type of leaching agent, it can be divided into organic acid leaching (such as acetic acid, citric acid, oxalic acid, etc.) and inorganic acid leaching (such as H2SO4, HCl, H3PO4, etc.). Inorganic acid has the advantages of low cost and fast leaching rate, and is usually the preferred solvent for hydrometallurgy. When using oxidizing agents and weak acid leaching, mechanical activation can be assisted to stimulate the leaching effect under weak acid or no acid. There are many oxidation methods for LiFePO4, and chemical oxidation (hydrogen peroxide, ozone, oxygen, air, persulfate, hypochlorite, etc.) and electrochemical oxidation have been reported. MnO2 is often used as a cheap oxidant in the leaching process, such as the oxidation and removal of iron in the hydrometallurgical zinc smelting process. The leaching of pyrolusite usually requires the addition of reducing agents, such as sulfur dioxide, ferrous sulfate, iron metal, pyrite, oxalic acid, hydrogen peroxide, and ascorbic acid.
[0005] Regeneration is the process of using waste LFP as one of the raw materials and combining it with other lithium, iron, phosphorus or carbon sources to synthesize LFP. In other words, the synthesis process of LFP is also applicable to its regeneration process. The high-temperature solid-phase method is a method of using solid substances for chemical reactions. By mixing other materials of waste positive electrode materials and then co-baking them, a solid-phase reaction occurs between the materials to regenerate new positive electrode materials. The high-temperature solid-phase method has a short process, but the treatment of original waste LFP with different degrees of lithium loss, the unevenness of the products and the high energy consumption are all limitations of high-temperature multiphase reactions. In order to reduce energy consumption and obtain more uniform products, some researchers have proposed to regenerate positive electrode materials by a hydrothermal route. This strategy is more suitable for treating original waste LFP with different degrees of lithium loss. Hydrothermal synthesis can significantly reduce the subsequent calcination temperature, while avoiding the release of harmful gases during the high-temperature calcination process. It is a green and environmentally friendly regeneration process.
[0006] Lithium iron manganese phosphate (LiMnxFe(1-x)PO4) is a material obtained by doping LFP with manganese ions. The embedding of manganese does not change the original olivine structure of LFP, so LiMnxFe(1-x)PO4 retains the high safety advantage of LFP. At the same time, compared with Fe2+, Mn2+ has a higher redox potential. Therefore, doping LFP with Mn can effectively improve the energy density of LFP.
[0007] The nano-sizing of LiMnxFe(1-x)PO4 materials can reduce the diffusion path of lithium ions inside them and improve the efficiency of lithium ion extraction and extraction. Therefore, controlling the particle size of LiMnxFe(1-x)PO4 is the key in its preparation process. In terms of particle size control, the liquid phase method has a natural advantage. The use of a wet process to recover LFP provides a good prerequisite for the subsequent synthesis of LiMnxFe(1-x)PO4 materials. Hydrothermal synthesis can further ensure that LiMnxFe(1-x)PO4 products with uniform particle size distribution and good grain development are obtained.
[0008] In summary, the method adopted by the present invention is: using MnO2 oxidation and sulfuric acid leaching to treat waste lithium iron phosphate positive electrode materials, coupling the oxidizing property of Mn in MnO2 with the reducibility of Fe in LiFePO4, and realizing the recovery of multiple elements in waste positive electrode materials. Mn ions are introduced during the leaching process, and the leaching solution is subsequently used for hydrothermal synthesis to prepare the positive electrode material LiMnxFe(1-x)PO4. Summary of the invention
[0009] The present invention aims at the problem of recycling the positive electrode materials of retired lithium iron phosphate batteries and provides a method for synthesizing lithium iron manganese phosphate from the positive electrode materials of retired lithium iron phosphate batteries.
[0010] The method for synthesizing lithium iron manganese phosphate from retired lithium iron phosphate battery positive electrode materials of the present invention comprises the following process steps:
[0011] 1. Leaching of lithium iron phosphate
[0012] The waste lithium iron phosphate battery is discharged, roasted, disassembled and ground to obtain lithium iron phosphate positive electrode material; lithium iron phosphate and manganese dioxide (MnO2) are mixed in a certain molar ratio and then subjected to acid leaching reaction with dilute sulfuric acid of a certain concentration to obtain a leachate;
[0013] 2. Adjustment of leachate and hydrothermal synthesis
[0014] The leaching solution obtained in step 1 is added with lithium source, manganese source and phosphorus source under the protection of nitrogen to adjust the ratio of each element in the solution, and then the reducing agent is added. After adjusting the pH (5.5-9) with ammonia water, the sample is quickly transferred to the reactor for hydrothermal reaction, the temperature is controlled at 160-250°C, and the hydrothermal time is 8-24h.
[0015] 3. Calcination of hydrothermal products
[0016] The hydrothermal product obtained in step 2 is washed several times and dried for 8 hours; the ground sample is sent to a tube furnace for calcination; under the protection of nitrogen, the product obtained by calcining at 400-700°C for 3-8 hours is LiMnxFe(1-x)PO4. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.
[0018] Figure 1 This is a flow chart of an embodiment of the present invention;
[0019] Figure 2 The XRD diagrams of the products obtained under different examples of the present invention are shown in FIG. DETAILED DESCRIPTION
[0020] The present invention is described in detail below in conjunction with the embodiments, but the protection scope of the present invention is not limited to the following embodiments.
[0021] like Figure 1 and Figure 2 As shown, Example 1
[0022] (1) After discharging, calcining, disassembling and grinding, lithium iron phosphate positive electrode material and MnO2 are mixed; the molar ratio of lithium iron phosphate to MnO2 is controlled to be 2.6:1, the liquid-solid ratio is 35 ml / g, the sulfuric acid concentration is 0.5 mol / L, and leaching is carried out at 25° C. for 60 min to obtain a mixed slurry;
[0023] (2) vacuum filtering the mixed slurry obtained in step 1, and obtaining a leachate after separating the filter residue; adding Li2SO4, MnSO4·H2O, and NH4H2PO4 to the leachate to control Li:Fe:Mn:P=2:0.8:0.2:1; adding malic acid to reduce trivalent iron under the protection of nitrogen, and adjusting the pH to 8.5; transferring the sample into a reactor and reacting at 250°C for 8h;
[0024] (3) The product after the hydrothermal reaction was washed three times with deionized water and dried in an oven at 80°C for 8 h. After drying, the sample was ground and placed in a tubular furnace and calcined at 700°C for 3 h under the protection of nitrogen.
[0025] Embodiment 2
[0026] (1) After discharge, roasting, disassembly and grinding, lithium iron phosphate positive electrode material and MnO2 are mixed. The molar ratio of lithium iron phosphate to MnO2 is controlled to be 2.6:1; the liquid-solid ratio is 35ml / g; the sulfuric acid concentration is 0.5mol / L, and leaching is carried out at 25°C for 60min to obtain a mixed slurry;
[0027] (2) The mixed slurry obtained in step 1 is vacuum filtered to separate the filter residue to obtain a metal solution. Li2SO4, MnSO4·H2O, and NH4H2PO4 are added to the leaching solution to control Li:Fe:Mn:P=2:0.5:0.5:1; ascorbic acid is added under the protection of nitrogen to reduce trivalent iron, and the pH is adjusted to 5.5; the sample is transferred to a reactor and reacted at 200°C for 15 hours;
[0028] (3) The product after the hydrothermal reaction was washed three times with deionized water and dried in an oven at 80°C for 10 h. After drying, the sample was ground and placed in a tubular furnace and calcined at 650°C for 5 h under the protection of nitrogen.
[0029] Embodiment 3
[0030] (1) After discharge, roasting, disassembly and grinding, lithium iron phosphate positive electrode material and MnO2 are mixed. The molar ratio of lithium iron phosphate to MnO2 is controlled to be 2.6:1; the liquid-solid ratio is 35ml / g; the sulfuric acid concentration is 0.5mol / L, and leaching is carried out at 25°C for 60min to obtain a mixed slurry;
[0031] (2) The mixed slurry obtained in step 1 is vacuum filtered to obtain a metal solution after separating the filter residue. Li2SO4, MnSO4·H2O, and NH4H2PO4 are added to the leaching solution to control Li:Fe:Mn:P=2:0.2:0.81. After adding hydrazine hydrate to reduce trivalent iron under the protection of nitrogen, the pH is adjusted to 9.0. The sample is transferred to a reactor and reacted at 160°C for 24 hours;
[0032] (3) The product after the hydrothermal reaction was washed three times with deionized water and dried in an oven at 80°C for 8 h. After drying, the sample was ground and placed in a tubular furnace and calcined at 400°C for 8 h under the protection of nitrogen.
Claims
1. A method for synthesizing lithium iron manganese phosphate from retired lithium iron phosphate battery positive electrode materials, It is characterized in that The steps include: Step 1: Discharge, roast and disassemble the waste lithium iron phosphate battery to obtain lithium iron phosphate positive electrode material, and mix it with manganese dioxide (MnO2) at a certain molar ratio. After mixing, acid leaching reaction is carried out with a certain concentration of dilute sulfuric acid to obtain a leachate; Step 2: Under the protection of nitrogen, lithium source, manganese source and phosphorus source are added to the leaching solution obtained in step 1 to adjust the ratio of each element in the solution, and then a reducing agent is added; after adjusting the pH with ammonia water, the sample is quickly transferred to a reactor for hydrothermal reaction; Step 3: After washing and drying the hydrothermal product of step 2 for multiple times, the product is calcined at high temperature under a nitrogen atmosphere to obtain lithium iron manganese phosphate.
2. The method for synthesizing lithium iron manganese phosphate from retired lithium iron phosphate battery positive electrode materials according to claim 1, Features The molar ratio of manganese to iron in the solution of step 2 is 1:4 to 0.
25.
3. The method for synthesizing lithium iron manganese phosphate from retired lithium iron phosphate battery positive electrode materials according to claim 1, Features The reducing agent in step 2 is one or more of ascorbic acid, hydrazine hydrate, malic acid and ammonium sulfite.
4. The method for synthesizing lithium iron manganese phosphate from retired lithium iron phosphate battery positive electrode materials according to claim 1, Features The pH after adjustment with ammonia water in step 2 is controlled at 5.5 to 9.
0.
5. The method for synthesizing lithium iron manganese phosphate from retired lithium iron phosphate battery positive electrode material according to claim 1, Features The hydrothermal synthesis temperature in step 2 is 160-250° C., and the hydrothermal synthesis time is 8-24 hours.
6. The method for synthesizing lithium iron manganese phosphate from retired lithium iron phosphate battery positive electrode material according to claim 1, Features The material in step 3 is calcined at a temperature of 400 to 700° C. and for a time of 3 to 8 hours.
Citation Information
Patent Citations
Method for recycling and preparing lithium iron manganese phosphate from positive electrode materials of waste lithium iron phosphate batteries
CN104609385A
Regeneration method of positive electrode material of waste lithium iron phosphate battery
CN116119636A
Cited By
Recovery and regeneration method of retired electrode material
CN119208800A