Polyferric chloride and production method thereof

By adding iron oxide powder and silicon-based cleaning waste phosphoric acid to the steel pickling waste liquid, combined with oxidant treatment, the problems of unstable polyferric chloride flocculant and high acidity of iron salt were solved, and an efficient, economical and mild The water treatment agent improves the flocculation effect and phosphorus removal capacity, while reducing environmental risks and resource consumption.

CN118724074APending Publication Date: 2024-10-01LANBAO (XIAMEN) WATER TREATMENT SCI & TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310321811.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-03-29
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Among the existing water treatment agents, the flocculation effect of polyferric chloride is unstable and easy to gel. The iron salt has strong phosphorus removal ability but is highly acidic and is highly corrosive. There is a lack of an agent with good flocculation effect, strong bridging ability and low price. , polyferric chloride products with strong phosphorus removal ability and mildness.

Method used

Polyferric chloride is produced by heating and dissolving iron oxide powder in steel pickling waste liquid containing ferrous ions and free acids, adding silicon-based cleaning waste phosphoric acid as a stabilizer, and optimizing the process formula to improve its performance. stability and performance.

Benefits of technology

The polyferric chloride with good flocculation effect, strong bridge capacity, strong phosphorus removal ability, low price and stable non-gelling has been realized, which reduces the cost of hazardous waste disposal and environmental risks, and promotes the comprehensive utilization of resources.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses polyferric chloride and a production method thereof, and belongs to the technical field of water treatment.The production method of the polyferric chloride comprises the following steps that S1, ferric oxide powder is added into steel pickling waste liquid containing ferrous ions and free acid to be heated and dissolved, and mixed liquid is obtained; and S3, slowly adding an oxidizing agent into the mixed solution which is uniformly stirred in the step S2, and continuously stirring after the oxidizing agent is added, so as to obtain polyferric chloride. According to the polyferric chloride and the production method thereof disclosed by the invention, the produced polyferric chloride is good in flocculation effect, high in bridging capability, low in price, high in phosphorus removal capability, relatively mild and capable of achieving long-term stability without gelling.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of water treatment, and in particular relates to polyferric chloride and a production method thereof. Background Art

[0002] At present, the inorganic water treatment agents widely used in China are aluminum salts represented by aluminum chloride, aluminum sulfate, and polyaluminum chloride (PAC), and iron salts represented by ferric chloride, ferric sulfate, polyferric chloride, and polyferric sulfate. Both are excellent water treatment agents with good flocculation effect, strong bridging ability, and low price. However, both have their own defects. For example, aluminum salts have insufficient phosphorus removal ability but weak acidity and relatively mild, while iron salts have strong phosphorus removal ability but their high acidity leads to strong corrosiveness.

[0003] At present, domestic sewage and phosphorus-containing industrial sewage are dephosphorized with iron salts. The scientific and technical personnel engaged in the research and development of water treatment agents know that polyferric chloride flocculants are very unstable and easily gel.

[0004] Therefore, the water treatment market is in urgent need of a polyferric chloride that has good flocculation effect, strong bridging ability, low price, strong phosphorus removal ability, is relatively mild, and can achieve long-term stability without gelling. Summary of the invention

[0005] The object of the present invention is to provide a polyferric chloride and a production method thereof to overcome at least one of the above-mentioned defects in the prior art.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] The invention provides a method for producing polyferric chloride, comprising the following steps: S1: adding iron oxide powder to steel pickling waste liquid containing ferrous ions and free acid, heating and dissolving the mixture to obtain a mixed solution; S2: adding a stabilizer to the mixed solution of step S1, and stirring the mixture evenly; S3: slowly adding an oxidant to the mixed solution stirred evenly in step S2, and continuing stirring after adding the oxidant, to obtain polyferric chloride.

[0008] Preferably, step S2 specifically includes: sampling the mixed solution of step S1 to detect the total iron ion content, and calculating the amount of stabilizer to be added according to the detection result.

[0009] Preferably, the stabilizer is silicon-based waste phosphoric acid for cleaning, and the mass ratio of the phosphoric acid in the stabilizer to the total iron in the mixed solution of step S1 is ≥0.30.

[0010] Preferably, before adding the oxidant, the mixed solution in step S1 is sampled to detect the ferrous ion and free acid content, and the amount of oxidant added is calculated based on the detection results.

[0011] Preferably, the total iron content of the polyferric chloride is 9.85-11.20wt / %, the basicity is 4.5-7%, and the yield is ≥99.6%.

[0012] Preferably, the steel pickling waste liquid has a ferrous chloride content of 19.6-25 wt / %, and a free acid content calculated as HCl of 2-8 wt / %.

[0013] Preferably, the phosphoric acid content in the silicon-based cleaning waste phosphoric acid is 65-75 wt / %, and the sulfuric acid content is 6-7 wt / %.

[0014] Preferably, the purity of the iron oxide powder is ≥90%, and the oxidant is sodium chlorate with a purity of ≥99%.

[0015] Preferably, in step S3, after the oxidant is added, stirring is continued at room temperature and pressure for 0.8-1.2 h.

[0016] The invention also provides polyferric chloride, which is prepared by adopting the polyferric chloride production method.

[0017] The beneficial effects of the present invention are:

[0018] Establish a comprehensive utilization model of multiple different multi-component mixed waste acids to reduce the cost of hazardous waste disposal, reduce environmental risks, and reduce the consumption of land resources and chemical resources. Polyferric chloride is produced using silicon-based cleaning waste phosphoric acid and steel pickling waste liquid. The steel pickling waste liquid contains a large amount of ferrous ions and some free hydrochloric acid. The excess free acid is consumed by adding an appropriate amount of iron oxide powder, and then silicon-based cleaning waste phosphoric acid is used as a stabilizer. By optimizing the process formula, an economical and efficient water treatment polymer flocculant polyferric chloride (PFC) is synthesized. Polyferric chloride flocculant is very unstable and easy to gel. The innovation of the present invention is to find suitable process conditions to improve the stability of polyferric chloride flocculant, so that the polyferric chloride flocculant is stable for a long time without gelling. The produced polyferric chloride has good flocculation effect, strong bridging ability, low price, strong phosphorus removal ability, and is relatively mild, and can achieve long-term stability without gelling. DETAILED DESCRIPTION

[0019] The present invention will now be further described in conjunction with specific implementation methods.

[0020] Embodiment 1:

[0021] A method for producing polyferric chloride provided in this embodiment comprises the following steps:

[0022] S1: Pretreatment of steel pickling waste liquid: Add 4.0g of iron oxide powder (purity = 90%) to 150g of steel pickling waste liquid containing ferrous ions (24.1wt / %) and free acid (3.0wt / %, calculated as HCl) and heat to dissolve to obtain a mixed solution. Samples were taken and tested according to the method of HG / T4672-2014 "Water Treatment Agent Polyferric Chloride": the total iron content was 12.00wt / %, the ferrous chloride content was 17.1wt / %, and the free acid (calculated as HCl) content was 1.0wt / %.

[0023] S2: Add 10.5g of silicon-based waste phosphoric acid (phosphoric acid content is 70wt / %, sulfuric acid content is 6.07wt / %) to the mixed solution of step S1 and stir evenly. Calculate the amount of silicon-based waste phosphoric acid added according to the test results. Specifically, the mass ratio of phosphoric acid in silicon-based waste phosphoric acid to total iron in the mixed solution of step S1 is 0.40.

[0024] S3: Calculate the amount of oxidant added according to the test results, slowly add 3.65g sodium chlorate (purity = 99%) to the mixed solution after stirring in step S2 at room temperature, continue stirring at room temperature and pressure for 1h after adding sodium chlorate, and the stirring speed is 60.0r / min to obtain polyferric chloride, the total iron content of polyferric chloride is 11wt / %, the ferrous chloride content is 0.01wt / %, the basicity is 6.6%, and the yield is ≥99.6%. It is brown and transparent, and the stable days are 30 days.

[0025] Chemical equations involved:

[0026] 6Fe 2+ +ClO3 - +6H + ==6Fe 3+ +3H2O+Cl -

[0027] 6HCl+Fe2O3==2FeCl3+3H2O

[0028] Fe 3+ +OH - →Fe(OH) 2+

[0029] Fe 3+ +2OH - →Fe(OH)2 +

[0030] Fe 3+ +3OH - →Fe(OH)3↓(This precipitation is easy to occur if the reaction is not well controlled)

[0031] 2Fe 3+ +2OH -→Fe2(OH)2 4+

[0032] 3Fe 3+ +4OH - →Fe3(OH)4 5+

[0033] Overall polymerization reaction: m[Fe2(OH) n Cl 6-n ]==[Fe2(OH) n Cl 6-n ] m

[0034] Comparative Example 1:

[0035] The difference between this embodiment and embodiment 1 is that:

[0036] The amount of silicon-based waste phosphoric acid is 5.3 g, and the mass ratio of phosphoric acid in silicon-based waste phosphoric acid to total iron in the mixed solution of step S1 is 0.2. The total iron content of the obtained polyferric chloride is 11.35wt / %, the ferrous chloride content is 0.01wt / %, the basicity is 6.5%, and the yield is ≥99.6%. It is brown and transparent, and the stable days are 7 days.

[0037] Comparative Example 2:

[0038] The difference between this embodiment and embodiment 1 is that:

[0039] The amount of silicon-based waste phosphoric acid is 7.9 g, and the mass ratio of phosphoric acid in silicon-based waste phosphoric acid to total iron in the mixed solution of step S1 is 0.3. The total iron content of the obtained polyferric chloride is 11.16 wt / %, the ferrous chloride content is 0.00 wt / %, the basicity is 6.7%, and the yield is ≥99.6%. It is brown and transparent, and the stable days are 20 days.

[0040] Comparative Example 3:

[0041] The difference between this embodiment and embodiment 1 is that:

[0042] The amount of silicon-based waste phosphoric acid is 13.2 g, and the mass ratio of phosphoric acid in silicon-based waste phosphoric acid to total iron in the mixed solution of step S1 is 0.5. The total iron content of the obtained polyferric chloride is 10.90 wt / %, the ferrous chloride content is 0.01 wt / %, the basicity is 6.5%, and the yield is ≥99.6%. It is brown and transparent, and the stable days are 30 days.

[0043] According to the experimental results in the table above, it can be seen that it is feasible to use silicon-based cleaning waste phosphoric acid and steel pickling waste liquid as raw materials and auxiliary oxidants to produce water treatment agent PFC, which can also achieve the maximum utilization of waste resources. The optimal process ratio is: the mass ratio of phosphoric acid H3PO4 / Fe in the stabilizer is about 0.40, and the reaction at room temperature for 1 hour is the best.

[0044] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, it should be understood by those skilled in the art that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for producing polyferric chloride, characterized in that: The following steps are involved: S1: adding iron oxide powder to the steel pickling waste liquid containing ferrous ions and free acid, heating and dissolving the mixture to obtain a mixed solution; S2: Add a stabilizer to the mixed solution of step S1 and stir evenly; S3: slowly adding an oxidant to the mixed solution stirred evenly in step S2, and continuing stirring after adding the oxidant to obtain polyferric chloride.

2. The method for producing polyferric chloride according to claim 1, wherein The step S2 specifically includes: The mixed solution in step S1 is sampled to detect the total iron ion content, and the amount of stabilizer to be added is calculated based on the detection result.

3. The polyferric chloride production method according to claim 2, wherein: The stabilizer is silicon-based waste phosphoric acid for cleaning, and the mass ratio of the phosphoric acid in the stabilizer to the total iron in the mixed solution of step S1 is ≥0.

30.

4. The method for producing polyferric chloride according to claim 1, wherein: Before adding the oxidant, the mixed solution in step S1 is sampled to detect the ferrous ion and free acid content, and the amount of oxidant to be added is calculated based on the test results.

5. The method for producing polyferric chloride according to claim 1, wherein: The total iron content of the polyferric chloride is 9.85-11.20 wt / %, the basicity is 4.5-7%, and the yield is ≥99.6%.

6. The method for producing polyferric chloride according to claim 1, wherein: The steel pickling waste liquid has a ferrous chloride content of 19.6-25 wt / %, and a free acid content calculated as HCl of 2-8 wt / %.

7. The method for producing polyferric chloride according to claim 3, wherein: The phosphoric acid content in the waste phosphoric acid for silicon-based cleaning is 65-75 wt / %, and the sulfuric acid content is 6-7 wt / %.

8. The method for producing polyferric chloride according to claim 1, wherein: The purity of iron oxide powder is ≥90%; The oxidant is sodium chlorate with a purity of ≥99%.

9. The method for producing polyferric chloride according to claim 1, wherein: In step S3, after the oxidant is added, stirring is continued at room temperature and pressure for 0.8-1.2 hours.

10. Polyferric chloride, characterized in that: The polyferric chloride is prepared by the polyferric chloride production method according to any one of claims 1 to 9.