Preparation method, product and application of modified lithium-rich manganese-based positive electrode material
Through the composite modification method of internal doping and external coating, the problem of poor cycle stability of lithium-rich manganese-based cathode materials is solved, using the bond between aluminum, yttrium and other metal elements and oxygen and the multi-element metal oxide coating layer. It improves high capacity and high cycle stability and is suitable for lithium-ion battery applications.
Patent Information
- Application Number
- CN202410730631.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-06
- Publication Date
- 2024-10-01
AI Technical Summary
Lithium-rich manganese-based cathode materials have poor stability during cycling, which limits their commercial application. Traditional modification methods are difficult to effectively improve the cycle performance of the materials.
Using a composite modification method of internal doping and external cladding, the lattice oxygen is stabilized by the introduction of bonds between metal elements such as aluminum and yttrium and oxygen, and a multi-element metal oxide coating layer is formed on the surface to improve the cycle stability of the material. properties and electrochemical properties.
The cycle stability and specific capacity of lithium-rich manganese-based cathode materials have been significantly improved. The discharge specific capacity has reached more than 276.43mAh/g, and the capacity retention rate for 500 cycles can reach 95%, achieving a balance between high capacity and high cycle stability.
Smart Images

Figure CN118724079A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium-ion batteries, and in particular to a preparation method, product and application of a modified lithium-rich manganese-based positive electrode material. Background Art
[0002] Lithium-ion batteries have taken a mainstream position due to their wide voltage window, high energy density, long cycle life, low self-discharge rate, and green safety. At present, the positive electrode material, as a key part of the battery system, has become the key to improving the performance of the entire battery. The new charge compensation mechanism of lithium-rich manganese-based lattice oxide materials in the positive electrode material has attracted the attention and research of academia and industry. However, while improving the charge and discharge capacity, the special mechanism of the redox of the anion lattice oxygen introduced makes it easier to produce gas during operation, and whether it can be stable, efficient, and long-term cycled has always been controversial. This severely limits the commercial application of lithium-rich manganese-based positive electrode materials.
[0003] Therefore, it is necessary to modify it to achieve a wide range of uses. At present, the most commonly used modification methods are surface coating and element doping. In addition, methods such as surface post-treatment and structural design can also be used to improve material performance. However, although the traditional modification method has improved the performance of lithium-rich manganese-based positive electrode materials to a certain extent, it still cannot solve the problem of poor cycle performance of lithium-rich manganese-based positive electrode materials. Therefore, a lithium-rich manganese-based positive electrode material with high cycle stability and high specific capacity is prepared, and it is modified at the same time to achieve a balance between capacity and cycle performance. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention discloses a method for preparing a modified lithium-rich manganese-based positive electrode material. The prepared modified lithium-rich manganese-based positive electrode material has both high capacity and excellent cycle stability.
[0005] The specific technical solutions are as follows:
[0006] A method for preparing a modified lithium-rich manganese-based positive electrode material comprises the following steps:
[0007] Step 1: Weigh a lithium source, a nickel source, a cobalt source, a manganese source, an optionally added doping metal source, a complexing agent and water and mix them evenly to obtain a precursor solution;
[0008] Step 2: obtaining a precursor powder by high temperature spray drying the precursor solution;
[0009] Step 3: sintering the precursor powder at high temperature to obtain a lithium-rich manganese-based positive electrode material;
[0010] Step 4: Evenly mix the lithium-rich manganese-based positive electrode material, the coating metal source and the solvent, and then prepare a modified lithium-rich manganese-based positive electrode material through post-treatment.
[0011] Through the improvement of the preparation process, the present invention introduces metal elements with a greater oxygen-binding energy to stabilize the unstable lattice oxygen during the long cycle process, which can greatly improve the stability of the material. In addition, by introducing a multi-metal oxide surface coating layer, the long cycle performance is improved. It has been found through experiments that the composite modification method of internal doping and external coating can further improve the electrochemical performance of the lithium-rich manganese-based cathode material.
[0012] In Step 1:
[0013] The lithium source is selected from one or more of lithium sulfate, lithium nitrate, lithium acetate, and lithium oxalate;
[0014] The nickel source is selected from one or more of nickel sulfate, nickel nitrate, nickel acetate, and nickel oxalate;
[0015] The cobalt source is selected from one or more of cobalt sulfate, cobalt nitrate, cobalt acetate, and cobalt oxalate;
[0016] The manganese source is selected from one or more of manganese sulfate, manganese nitrate, manganese acetate, and manganese oxalate;
[0017] The doping metal in the doping metal source is selected from one or more of aluminum, yttrium, niobium, lanthanum, cerium, praseodymium, neodymium, samarium, europium, gadolinium, terbium, dysprosium, and erbium, and the doping metal source is selected from one or more of the sulfates, nitrates, acetates, and oxalates corresponding to the doping metal;
[0018] The complexing agent is selected from one or more of citric acid, ammonia water, carbonates, and bicarbonates.
[0019] Preferably:
[0020] Weigh the lithium source, nickel source, cobalt source, manganese source, and doping metal source Me according to the stoichiometric ratio corresponding to the chemical general formula Li 1.2 Ni 0.13+x Co 0.13-2x Mn 0.54 Me x O2, where 0 ≤ x < 0.06; preferably, 0 < x < 0.06, more preferably, 0.01 ≤ x ≤ 0.05, and even more preferably 0.03.
[0021] In the precursor solution, the total concentration of the mixed solution is 0.1 - 10 mol / L, and more preferably, the total concentration is 1 - 5 mol / L.
[0022] The concentration of the complexing agent is 0.05 - 5 mol / L, and more preferably, the total concentration is 1 - 5 mol / L.
[0023] In Step 2:
[0024] The spray drying has an inlet temperature of 150-280°C, an outlet temperature of 70-120°C, a peristaltic pump speed of 200-1000 ml / h, a needle passing frequency of 5-30 Hz, and a spray pressure of 0.1-0.5 MPa;
[0025] The spray drying atmosphere is air and / or oxygen.
[0026] Preferred:
[0027] The inlet temperature is 200-250°C, the outlet temperature is 100-120°C, the peristaltic pump speed is 500-800ml / h, the needle passing frequency is 10-20Hz, and the spray pressure is 0.1-0.3MPa.
[0028] In step three:
[0029] The high temperature sintering is carried out by heating the temperature from room temperature to 600-1200°C at a heating rate of (1-10)°C / min, keeping the temperature for 0.2-24h and then cooling naturally; the preferred sintering temperature is 800-1200°C.
[0030] In step 4:
[0031] The coating metal in the coating metal source is selected from one or more of aluminum, yttrium, niobium, lanthanum, cerium, praseodymium, neodymium, samarium, europium, gadolinium, terbium, dysprosium, and erbium, and the coating metal source is selected from one or more of sulfates, nitrates, acetates, and oxalates corresponding to the coating metal;
[0032] The solvent is selected from one or more of deionized water, ethanol, chloroform, oleic acid, N-methylformamide, and dimethyl sulfoxide;
[0033] Based on the mass of the lithium-rich manganese-based positive electrode material being 100%, the mass of the added coating metal source accounts for 1 to 5%;
[0034] The mass volume ratio of the lithium-rich manganese-based cathode material to the solvent is 0.01 to 1.00 g / mL;
[0035] The post-processing includes grinding and high-temperature sintering.
[0036] Preferably, the grinding includes ball milling and hand milling;
[0037] The ball mill has a rotation speed of 100 to 600 r / min and a ball milling time of 0.5 to 3 h;
[0038] The hand grinding time is 10 to 60 minutes;
[0039] The high temperature sintering is to raise the temperature to 300-1000° C. at a heating rate of 1-10° C. / min, keep the temperature for 2-20 hours and then cool naturally.
[0040] Based on the above process and raw materials, further preferred is:
[0041] In step 1, the doping metal in the doping metal source is selected from aluminum and yttrium, and the molar ratio of the aluminum source to the yttrium source is 1:1;
[0042] In step 4, the coating metal in the coating metal source is selected from aluminum and yttrium, and the molar ratio of the aluminum source to the yttrium source is 1:(0.6-1.0).
[0043] Most preferably, in step 4, the molar ratio of the aluminum source to the yttrium source is 1:0.6, and based on the mass of the lithium-rich manganese-based positive electrode material being 100%, the mass of the added coating metal source accounts for 3%.
[0044] The invention also discloses a modified lithium-rich manganese-based positive electrode material prepared according to the method and application thereof in a lithium-ion battery.
[0045] Compared with the prior art, the present invention has the following beneficial effects:
[0046] (1) Due to the problems of lattice oxygen precipitation, transition metal ion migration and electrolyte corrosion of the positive electrode material, the lithium-rich manganese-based positive electrode material has a high specific capacity but poor stability. The present invention uses aluminum, yttrium, niobium and the like as doping metal elements to slow down the generation of oxygen vacancies through strong bonding with oxygen, block the migration path of transition metal ions, reduce the phase transition rate of the material, reduce the transfer internal resistance during the cycle, and can better maintain the median voltage, thereby enhancing the cycle stability of the lithium-rich manganese-based positive electrode material; at the same time, by coating the surface of the lithium-rich manganese-based positive electrode material with a coating layer containing aluminum, yttrium, niobium oxide and the like and then performing low-temperature sintering, the high specific surface area of the lithium-rich manganese-based positive electrode material can be ensured while improving the internal structural stability of the material and preventing the performance of the material from deteriorating during the charge and discharge process.
[0047] (2) The modified lithium-rich manganese-based positive electrode material prepared by the present invention has a discharge specific capacity of up to 276.43 mAh / g and a capacity retention rate of up to 95% after 500 cycles, which has both high capacity and high cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 The cycle curve of the battery assembled with the yttrium-aluminum co-coated lithium-rich manganese-based positive electrode material prepared in Example 1;
[0049] Figure 2 The cycle curve of the battery assembled with the composite doped and coated lithium-rich manganese-based positive electrode material prepared in Example 5;
[0050] Figure 3 This is a scanning electron microscope image of the composite doped and coated lithium-rich manganese-based positive electrode material prepared in Example 5;
[0051] Figure 4 This is a transmission electron microscope image of the composite doped and coated lithium-rich manganese-based positive electrode material prepared in Example 5;
[0052] Figure 5 The cycle curve of the battery assembled with the product prepared in Comparative Example 1;
[0053] Figure 6 This is a scanning electron microscope image of the product prepared in Comparative Example 1;
[0054] Figure 7 This is a transmission electron microscope image of the product prepared in Comparative Example 1;
[0055] Figure 8 The cycle curve of the battery assembled with the product prepared in Comparative Example 2;
[0056] Fig. 9 This is a scanning electron microscope image of the product prepared in Comparative Example 2;
[0057] Fig.10 The cycle curve of the battery assembled with the product prepared in Comparative Example 3;
[0058] Fig.11 This is a scanning electron microscope image of the product prepared in Comparative Example 3;
[0059] Fig.12 The cycle curve of the battery assembled with the product prepared in Comparative Example 4;
[0060] Fig.13 This is a scanning electron microscope image of the product prepared in Comparative Example 4. DETAILED DESCRIPTION
[0061] The present invention is further described in detail below in conjunction with examples and comparative examples, but the embodiments of the present invention are not limited thereto.
[0062] Example 1
[0063] (1) Press Li 1.2 Ni 0.13 Co 0.13 Mn 0.54 The ingredients were prepared in a stoichiometric ratio of 2 mol / L to 1 mol / L O2. Lithium acetate, nickel acetate, cobalt acetate and manganese acetate were dissolved in deionized water to prepare a mixed salt solution with a total concentration of 2 mol / L. 3 mol / L of complexing agent citric acid was added to the mixed salt solution, and the solution was stirred on a magnetic stirrer for 1 hour to mix the solution evenly to obtain a spray solution.
[0064] (2) The spray solution is pumped into a spray dryer, the atmosphere is air, the inlet temperature is 230°C, the outlet temperature is 115°C, the peristaltic pump speed is 600mL / h, the needle frequency is 15Hz, and the spray pressure is 0.2MPa. The precursor powder of the layered lithium-rich manganese-based positive electrode material is prepared by granulation by spray drying.
[0065] (3) The precursor powder is placed in a muffle furnace with air for sintering, and the temperature is increased from room temperature to 1000°C at a rate of 5°C / min and kept constant for 20 minutes, and then naturally cooled to room temperature. The sintered lithium-manganese-rich positive electrode material powder is fully ground and then passed through a 500-mesh sieve for use.
[0066] (4) 2g of lithium-rich manganese cathode material powder, 0.0263g of yttrium acetate, 0.0337g of aluminum acetate and 0.0134g of lithium acetate were mixed into 50mL of deionized water and ultrasonically stirred evenly. The total mass ratio of aluminum acetate and yttrium acetate to the lithium-rich manganese cathode material was 3:100, and the molar ratio of aluminum acetate to yttrium acetate was 5:3. The mixed solution after ultrasonic stirring was placed in a planetary ball mill and milled at 500r / min for 1h, then taken out and dried. The dried powder was ground for 20min, and then placed in a muffle furnace for annealing at 600℃ at a heating rate of 5℃ / min for 10h to obtain a yttrium-aluminum co-coated lithium-rich manganese-based cathode material, which was recorded as 3YAl@LRMO.
[0067] The yttrium aluminum doped and coated lithium-rich manganese positive electrode material, conductive agent (SuperP) and binder (sodium carboxymethyl cellulose CMC) prepared in this embodiment are mixed into a slurry at a mass ratio of 85:10:5. After stirring evenly, it is coated on the aluminum foil current collector to obtain a positive electrode plate. The above-mentioned positive electrode plate is used, the metal Li plate is used as the reference electrode and the counter electrode, the diaphragm is Celgard-2400, and the electrolyte is Xinzhoubang 3045I. It is assembled in an argon-filled glove box with oxygen and water content less than 0.01ppm. Its electrochemical performance is tested by charging and discharging 2025 button batteries on the Xinwei test system, and the test voltage window is 2.0~4.8V. The test temperature is 27±1℃, and the first three cycles are activated at a rate of 0.1C (1C=200mAh / g), and the 1C rate cycle is used from the 4th cycle. The performance test results are shown in Table 1.
[0068] Example 2
[0069] The preparation process is basically the same as that of Example 1, except that in step (4):
[0070] The mass of yttrium acetate is replaced with 0.0438 g, the mass of aluminum acetate is replaced with 0.0562 g, and the mass of lithium acetate is replaced with 0.0496 g; at this time, the mass ratio of the total mass of aluminum acetate and yttrium acetate to the lithium-rich manganese positive electrode material is replaced with 5:100.
[0071] The prepared yttrium-aluminum co-coated lithium-manganese-rich based positive electrode material is denoted as 5YAl@LRMO.
[0072] The battery assembly process is the same as in Example 1, and the performance test results are listed in Table 1.
[0073] Example 3
[0074] (1) Press Li 1.2 Ni 0.16 Co 0.07 Mn 0.54 Al 0.015 Y 0.015 The ingredients are prepared according to the stoichiometric ratio of O2. Lithium acetate, nickel acetate, cobalt acetate, manganese acetate, yttrium acetate and aluminum acetate are dissolved in deionized water to prepare a mixed salt solution with a total concentration of 2 mol / L, and 3 mol / L of complexing agent citric acid is added to the mixed salt solution, and the solution is stirred on a magnetic stirrer for 1 hour to mix the solution evenly to obtain a spray solution;
[0075] Steps (2-3) are exactly the same as those in Example 1;
[0076] (4) 2g of lithium-rich manganese cathode material powder, 0.0112g of yttrium acetate, 0.0088g of aluminum acetate and 0.0086g of lithium acetate were mixed into 50mL of deionized water and ultrasonically stirred evenly. The total mass ratio of aluminum acetate and yttrium acetate to the lithium-rich manganese cathode material was 1:100, and the molar ratio of aluminum acetate to yttrium acetate was 1:1. The mixed solution after ultrasonic stirring was placed in a planetary ball mill and milled at 500r / min for 1h, then taken out and dried. The dried powder was ground for 20min, and then placed in a muffle furnace for annealing at 600℃ for 10h at a heating rate of 5℃ / min to obtain a composite doped and coated lithium-rich manganese-based cathode material, which was recorded as 1YAl@YAl-LRMO.
[0077] The battery assembly process is the same as in Example 1, and the performance test results are listed in Table 1.
[0078] Example 4
[0079] The preparation process is basically the same as that in Example 3, except that in step (4):
[0080] The mass of yttrium acetate is replaced with 0.0339 g, the mass of aluminum acetate is replaced with 0.0261 g, and the mass of lithium acetate is replaced with 0.026 g; at this time, the mass ratio of the total mass of aluminum acetate and yttrium acetate to the lithium-rich manganese positive electrode material is replaced with 3:100, and the molar ratio of aluminum acetate and yttrium acetate is 1:1.
[0081] The prepared composite doped and coated lithium-rich manganese-based positive electrode material is recorded as 3YAl@YAl-LRMO.
[0082] The battery assembly process is the same as in Example 1, and the performance test results are listed in Table 1.
[0083] Example 5
[0084] The preparation process is basically the same as that in Example 3, except that in step (4):
[0085] The mass of yttrium acetate is replaced with 0.0263g, the mass of aluminum acetate is replaced with 0.0337g, and the mass of lithium acetate is replaced with 0.0134g; at this time, the mass ratio of the total mass of aluminum acetate and yttrium acetate to the lithium-rich manganese positive electrode material is replaced with 3:100, and the molar ratio of aluminum acetate and yttrium acetate is 5:3.
[0086] The prepared composite doped and coated lithium-rich manganese-based positive electrode material is recorded as 3YAl@YAl-LRMO.
[0087] The battery assembly process is the same as in Example 1, and the performance test results are listed in Table 1.
[0088] Example 6
[0089] (1) Press Li 1.2 Ni 0.16 Co 0.07 Mn 0.54 Al 0.015 Ga 0.015 The ingredients were prepared in a stoichiometric ratio of 1,2-dihydro-2-nitrogen (2,4-dihydro-2-nitrogen) and 1,2-dihydro-2-nitrogen (2,4-dihydro-2-nitrogen) (O2). Lithium acetate, nickel acetate, cobalt acetate, manganese acetate, gallium nitrate and aluminum nitrate were dissolved in deionized water to prepare a mixed salt solution with a total concentration of 2 mol / L. 3 mol / L of complexing agent citric acid was added to the mixed salt solution, and the solution was stirred on a magnetic stirrer for 1 hour to mix the solution evenly to obtain a spray solution.
[0090] Steps (2-3) are exactly the same as those in Example 1;
[0091] (4) 2g of lithium-rich manganese cathode material powder, 0.0273g of aluminum nitrate, 0.0327g of gallium nitrate and 0.0176g of additional lithium nitrate were mixed into 50mL of deionized water and ultrasonically stirred evenly. The total mass ratio of aluminum nitrate and gallium nitrate to the mass ratio of lithium-rich manganese cathode material was 3:100, and the molar ratio of aluminum nitrate to gallium nitrate was 1:1. The mixed solution after ultrasonic stirring was placed in a planetary ball mill at 500r / min for 1h and then taken out to dry. The dried powder was ground for 20min and then placed in a muffle furnace for annealing at 600℃ for 10h at a heating rate of 5℃ / min to obtain a composite doped and coated lithium-rich manganese-based cathode material, which was recorded as 3AlGa@AlGa-LRMO.
[0092] The battery assembly process is the same as in Example 1, and the performance test results are listed in Table 1.
[0093] Example 7
[0094] (1) Press Li 1.2 Ni 0.16 Co 0.07 Mn0.54 Al 0.03 The ingredients were prepared in a stoichiometric ratio of 1,2-dihydro-1,4-dihydro-2-nitrogen (2,4-dihydro-1,4-dihydro-2-nitrogen) and 1,2-dihydro-1,4-dihydro-2-nitrogen (2,4-dihydro-1,4-dihydro-2-nitrogen) (O2). Lithium acetate, nickel acetate, cobalt acetate, manganese acetate and aluminum acetate were dissolved in deionized water to prepare a mixed salt solution with a total concentration of 2 mol / L. 3 mol / L of complexing agent citric acid was added to the mixed salt solution, and the solution was stirred on a magnetic stirrer for 1 hour to mix the solution evenly to obtain a spray solution.
[0095] Steps (2-4) are exactly the same as those in Example 1.
[0096] The prepared composite doped and coated lithium-rich manganese-based positive electrode material is recorded as 3YAl@Al-LRMO.
[0097] The battery assembly process is the same as in Example 1, and the performance test results are listed in Table 1.
[0098] Example 8
[0099] (1) Press Li 1.2 Ni 0.16 Co 0.07 Mn 0.54 Y 0.03 The ingredients were prepared in a stoichiometric ratio of 1,2-dihydrogen 2-nitrogen (2-H)- ...
[0100] Steps (2-4) are exactly the same as those in Example 1.
[0101] The prepared composite doped and coated lithium-rich manganese-based positive electrode material is recorded as 3YAl@Y-LRMO.
[0102] The battery assembly process is the same as in Example 1, and the performance test results are listed in Table 1.
[0103] Comparative Example 1
[0104] (1) According to 0.5Li2MnO3·0.5Li(Ni 0.33 Co 0.33 Mn 0.33 )O2 stoichiometric ratio, and the ingredients are prepared. Lithium acetate, nickel acetate, cobalt acetate, and manganese acetate are dissolved in deionized water to prepare a mixed salt solution with a total concentration of 2 mol / L, and 3 mol / L of complexing agent citric acid is added to the mixed salt solution, and stirred on a magnetic stirrer for 1 hour to mix the solution evenly to obtain a spray solution.
[0105] (2) The spray solution is pumped into a spray dryer, the atmosphere is air, the inlet temperature is 230°C, the outlet temperature is 115°C, the peristaltic pump speed is 600mL / h, the needle frequency is 15Hz, and the spray pressure is 0.2MPa. The precursor powder of the layered lithium-rich manganese-based positive electrode material is prepared by granulation by spray drying.
[0106] (3) The precursor powder is placed in a muffle furnace with air for sintering, and the temperature is increased from room temperature to 1000°C at a rate of 5°C / min and kept constant for 20 minutes, and then naturally cooled to room temperature. The sintered lithium-manganese-rich positive electrode material powder is fully ground and then passed through a 500-mesh sieve for use.
[0107] The battery assembly process is the same as in Example 1, and the performance test results are listed in Table 1.
[0108] Comparative Example 2
[0109] (1) Press Li 1.2 Ni 0.16 Co 0.07 Mn 0.54 Al 0.015 Y 0.015 The ingredients are prepared according to the stoichiometric ratio of O2. Lithium acetate, nickel acetate, cobalt acetate, manganese acetate, yttrium acetate and aluminum acetate are dissolved in deionized water to prepare a mixed salt solution with a total concentration of 2 mol / L, and 3 mol / L of complexing agent citric acid is added to the mixed salt solution, and the solution is stirred on a magnetic stirrer for 1 hour to mix the solution evenly to obtain a spray solution;
[0110] Steps (2-3) are exactly the same as those in Comparative Example 1.
[0111] The product was recorded as YAl-LRMO. The battery assembly process was the same as in Example 1. The performance test results are listed in Table 1.
[0112] Comparative Example 3
[0113] (1) Press Li 1.2 Ni 0.16 Co 0.07 Mn 0.54 Al 0.03 The ingredients were prepared in a stoichiometric ratio of 2 mol / L to 1 mol / L O2. Lithium acetate, nickel acetate, cobalt acetate, manganese acetate and aluminum acetate were dissolved in deionized water to prepare a mixed salt solution with a total concentration of 2 mol / L. 3 mol / L of complexing agent citric acid was added to the mixed salt solution, and the solution was stirred on a magnetic stirrer for 1 hour to mix the solution evenly to obtain a spray solution.
[0114] Steps (2-3) are exactly the same as those in Comparative Example 1.
[0115] The product was recorded as Al-LRMO. The battery assembly process was the same as in Example 1. The performance test results are listed in Table 1.
[0116] Comparative Example 4
[0117] (1) Press Li 1.2 Ni 0.16 Co 0.07 Mn 0.54 Y 0.03 The ingredients were prepared in a stoichiometric ratio of 2 mol / L to 1 mol / L O2. Lithium acetate, nickel acetate, cobalt acetate, manganese acetate and yttrium acetate were dissolved in deionized water to prepare a mixed salt solution with a total concentration of 2 mol / L. 3 mol / L of citric acid as a complexing agent was added to the mixed salt solution, and the solution was stirred on a magnetic stirrer for 1 hour to mix the solution evenly to obtain a spray solution.
[0118] Steps (2-3) are exactly the same as those in Comparative Example 1.
[0119] The product was recorded as Y-LRMO. The battery assembly process was the same as in Example 1. The performance test results are listed in Table 1.
[0120] Comparative Example 5
[0121] (1) Press Li 1.2 Ni 0.16 Co 0.07 Mn 0.54 Nb 0.03 The ingredients were prepared in a stoichiometric ratio of 2 mol / L to 1 mol / L O2. Lithium acetate, nickel acetate, cobalt acetate, manganese acetate and niobium acetate were dissolved in deionized water to prepare a mixed salt solution with a total concentration of 2 mol / L. 3 mol / L of citric acid as a complexing agent was added to the mixed salt solution, and the solution was stirred on a magnetic stirrer for 1 hour to mix the solution evenly to obtain a spray solution.
[0122] Steps (2-3) are exactly the same as those in Comparative Example 1.
[0123] The product is recorded as Nb-LRMO. The battery assembly process is the same as in Example 1. The performance test results are listed in Table 1.
[0124] Table 1
[0125]
[0126]
[0127] By comparing Examples 1 and 5 with Comparative Examples 1 and 2, it can be seen that the electrochemical performance of the lithium-rich manganese layered oxide can be better improved by coating with aluminum and yttrium dual-component oxides; when aluminum and yttrium dual-component oxides are doped at the same time, the electrochemical performance is further improved.
[0128] By comparing Examples 1, 5, 7 and 8, it can be seen that when the doping element is single aluminum or single yttrium, the electrochemical performance of the modified lithium-rich manganese layered oxide prepared by internal doping and external coating is slightly worse than that of the dual-component oxide coated with aluminum and yttrium only.
[0129] By comparing Examples 1 to 6, it can be seen that when the outer coating layer is a two-component oxide of aluminum and yttrium, the electrochemical performance of the prepared modified lithium-rich manganese layered oxide is better, and when the mass ratio of the total mass of the coating metal source to the lithium-rich manganese positive electrode material is 3:100 and the molar ratio of the aluminum source to the yttrium source is 1:0.6, the electrochemical performance of the prepared modified lithium-rich manganese layered oxide is optimal.
[0130] Figure 3 and Figure 4 The SEM and TEM images of the product prepared in Example 5 of the present invention show that after mixed ball milling and re-firing, the primary particles are smaller, with a particle size between 100 and 200 nm, the particles are connected into sheets, and when the edge of the particles is enlarged, the surface structure changes, and the yttrium aluminum oxide coating layer is about 3 nm.
[0131] By comparing the SEM images of the products prepared in Example 5 and Comparative Example 1, it can be seen that the primary particle size in the product prepared in Example 5 becomes smaller.
[0132] By comparing the SEM images of the products prepared in Example 5 with those in Comparative Examples 2, 3, and 4, it can be seen that the particle agglomeration degree of the product prepared in Example 5 is lower, which is beneficial to the release of grain boundary stress of the lithium-rich manganese-based positive electrode material during the lithium ion insertion and extraction process.
[0133] The above-mentioned embodiments are preferred embodiments, but the protection scope of the present invention is not limited thereto. A person skilled in the art can easily understand the spirit of the present invention based on the above-mentioned embodiments and make different extensions and changes. However, as long as they do not deviate from the spirit of the present invention, they are all within the protection scope of the present invention.
Claims
1. A method for preparing a modified lithium-rich manganese-based positive electrode material, characterized in that: The steps include: Step 1: Weigh a lithium source, a nickel source, a cobalt source, a manganese source, an optionally added doping metal source, a complexing agent and water and mix them evenly to obtain a precursor solution; Step 2: obtaining a precursor powder by high temperature spray drying the precursor solution; Step 3: sintering the precursor powder at high temperature to obtain a lithium-rich manganese-based positive electrode material; Step 4: Evenly mix the lithium-rich manganese-based positive electrode material, the coating metal source and the solvent, and then prepare a modified lithium-rich manganese-based positive electrode material through post-treatment.
2. The method for preparing the modified lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: In step one: The lithium source is selected from one or more of lithium sulfate, lithium nitrate, lithium acetate and lithium oxalate; The nickel source is selected from one or more of nickel sulfate, nickel nitrate, nickel acetate, and nickel oxalate; The cobalt source is selected from one or more of cobalt sulfate, cobalt nitrate, cobalt acetate, and cobalt oxalate; The manganese source is selected from one or more of manganese sulfate, manganese nitrate, manganese acetate and manganese oxalate; The doping metal in the doping metal source is selected from one or more of aluminum, yttrium, niobium, lanthanum, cerium, praseodymium, neodymium, samarium, europium, gadolinium, terbium, dysprosium, and erbium, and the doping metal source is selected from one or more of sulfates, nitrates, acetates, and oxalates corresponding to the doping metal; The complexing agent is selected from one or more of citric acid, ammonia water, carbonate and bicarbonate.
3. The method for preparing the modified lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: In step one: According to the chemical formula Li 1.2 Ni 0.13+x Co 0.13-2x Mn 0.54 Me x Weigh the lithium source, nickel source, cobalt source, manganese source, and doping metal source Me in the stoichiometric ratio corresponding to O2, 0≤x<0.06; In the precursor solution, the total concentration of the mixed solution is 0.1-10 mol / L, and the concentration of the complexing agent is 0.05-5 mol / L.
4. The method for preparing the modified lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: In step 2: The spray drying has an inlet temperature of 150-280°C, an outlet temperature of 70-120°C, a peristaltic pump speed of 200-1000 ml / h, a needle passing frequency of 5-30 Hz, and a spray pressure of 0.1-0.5 MPa; The spray drying atmosphere is air and / or oxygen.
5. The method for preparing the modified lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: In step three: The high temperature sintering is carried out by heating the temperature from room temperature to 600-1200° C. at a heating rate of (1-10)° C. / min, keeping the temperature for 0.2-24 hours and then cooling naturally.
6. The method for preparing the modified lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: In step 4: The coating metal in the coating metal source is selected from one or more of aluminum, yttrium, niobium, lanthanum, cerium, praseodymium, neodymium, samarium, europium, gadolinium, terbium, dysprosium, and erbium, and the coating metal source is selected from one or more of sulfates, nitrates, acetates, and oxalates corresponding to the coating metal; The solvent is selected from one or more of deionized water, ethanol, chloroform, oleic acid, N-methylformamide, and dimethyl sulfoxide; Based on the mass of the lithium-rich manganese-based positive electrode material being 100%, the mass of the added coating metal source accounts for 1 to 5%; The mass volume ratio of the lithium-rich manganese-based cathode material to the solvent is 0.01 to 1.00 g / mL; The post-processing includes grinding and high-temperature sintering.
7. The method for preparing the modified lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: In step 1, the doping metal in the doping metal source is selected from aluminum and yttrium, and the molar ratio of the aluminum source to the yttrium source is 1:1; In step 4, the coating metal in the coating metal source is selected from aluminum and yttrium, and the molar ratio of the aluminum source to the yttrium source is 1:(0.6-1.0).
8. The method for preparing the modified lithium-rich manganese-based positive electrode material according to item 7, characterized in that: In step 4, the molar ratio of the aluminum source to the yttrium source is 1:0.
6. Based on the mass of the lithium-rich manganese-based positive electrode material being 100%, the mass of the added coating metal source accounts for 3%.
9. A modified lithium-rich manganese-based positive electrode material prepared by the method according to any one of claims 1 to 8.
10. Use of the modified lithium-rich manganese-based positive electrode material according to claim 9 in a lithium-ion battery.