Method for advanced oxidation and zero emission of electronickelling flushing wastewater
Through dual-stage oxidation treatment and membrane distillation concentration technology, the problem of removal of organic and inorganic pollutants in nickel electroplating washing wastewater has been solved, efficient treatment and recycling of wastewater has been achieved, and the goal of zero discharge has been achieved, which has good social and environmental benefits. .
Patent Information
- Application Number
- CN202310339891.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-01
AI Technical Summary
Existing technology is difficult to effectively treat organic and inorganic pollutants in nickel electroplating flushing wastewater, resulting in incomplete removal of pollutants, affecting the recycling of wastewater and environmental pollution.
A two-stage oxidation treatment method is adopted. First, H2O2 is used for efficient oxidation in an activated carbon catalytic reactor. Then, the concentrated liquid is further processed through membrane distillation concentration technology, and catalyst-loaded activated carbon particles are used for catalytic oxidation to ensure that pollutants meet the standards of the electroplating solution. , achieve zero emissions.
It achieves efficient oxidation and concentration of nickel plating washing wastewater, ensures the removal of pollutants, achieves the purity of the electroplating solution, and realizes the recycling of wastewater, which has dual economic and environmental benefits.
Smart Images

Figure CN118724239A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of wastewater treatment, and in particular relates to a method for advanced oxidation and zero discharge of nickel electroplating flushing wastewater. Background Art
[0002] Nickel electroplating is a method of depositing a layer of nickel on the surface of ferrous or non-ferrous metal parts by electrochemical action. It can be used as a surface coating, but it is mainly used for chrome plating to prevent corrosion, increase wear resistance, gloss and beauty. It is widely used in the manufacturing industry of machinery, instruments, meters, medical equipment, household appliances, etc. The workpiece is used as the cathode and the pure nickel plate is used as the anode. It is hung in an electrolyte composed of nickel sulfate, sodium chloride and boric acid for electroplating.
[0003] After electroplating, the surface of the plated parts will carry a small amount of electroplating solution. Therefore, the plated parts need to be rinsed after electroplating. During the rinsing process, rinsing wastewater will be generated. The main pollutants in the rinsing wastewater are the diluted electroplating solution. The main components of the commonly used Watt electroplating solution include nickel chloride, nickel sulfate, boric acid and a small amount of organic additives. Among them, inorganic components such as nickel chloride, nickel sulfate and boric acid will basically not change during the electroplating process, while organic additives will undergo oxidation, decomposition and other reactions as the electroplating time increases. Therefore, the main pollutants in the rinsing wastewater include nickel, boron, organic matter, etc.
[0004] N201310345579.0 discloses a device and method for recovering nickel from nickel-containing wastewater using a microbial electrolytic cell, the device includes a microbial electrolytic cell, a data acquisition system and a recording unit; the microbial electrolytic cell is a double-chamber microbial electrolytic cell; the microbial electrolytic cell uses a conductive inert material as an anode electrode and a conductive inert material as a cathode electrode, and the anode electrode and the cathode electrode are connected by a titanium wire, a constant potential instrument and a resistor; the data acquisition system is connected in parallel with the resistor, and the recording unit is connected to the data acquisition system. It provides a feasibility analysis and specific operation method for electrolytically recovering nickel from nickel-containing wastewater using a microbial electrolytic cell, and realizes the recovery of nickel from nickel-containing wastewater using a microbial electrolytic cell. Compared with the traditional method of electrolytically recovering nickel from water, this method greatly reduces energy consumption, reduces the use of chemical reagents, reduces costs, and avoids environmental pollution.
[0005] CN201410301526.3 discloses a method for treating nickel-containing wastewater in the electroplating industry. The method for treating nickel-containing wastewater comprises the following steps: (1) adding an oxidant to the nickel-containing wastewater under acidic conditions to carry out an oxidation reaction; (2) adding alkali to the nickel-containing wastewater after the oxidation reaction in step (1) to make the nickel-containing wastewater alkaline, then standing and settling, and taking out the supernatant; (3) adding a precipitant and a flocculant to the supernatant in step (2) in sequence to carry out co-precipitation, and the resulting final supernatant is the treated dischargeable wastewater. The treatment method is simple to operate, has a stable effect, and the reagents used will not cause secondary pollution to the environment; the treatment method utilizes the co-precipitation effect of the flocculant and the precipitate on the basis of secondary precipitation, which can ensure that the total nickel concentration of the treated effluent from the nickel-containing wastewater can meet the discharge standard.
[0006] CN201410473920.5 discloses a nickel-containing wastewater treatment device, including a nickel-containing wastewater storage and input device, a nickel-containing wastewater pH adjustment tank, a pump system, an electrolysis device and a control device, and also includes a sewage circulation treatment device. It also discloses a treatment method corresponding to the nickel-containing wastewater treatment device, which adds chemical nickel waste liquid and nickel-containing sewage concentrate into the nickel-containing wastewater pH adjustment tank for mixing, and adjusts the pH value to 6-7; the wastewater with the adjusted pH value is passed into an electrolytic tank for electrolysis at 65-75°C to recover elemental nickel, and the nickel discharge concentration of the wastewater after electrolysis is below 0.02g / L, and the recovery rate is above 97%; the wastewater after electrolysis is further treated by reverse osmosis resin exchange, and the treated wastewater can be directly discharged or recycled.
[0007] If the organic matter in the flushing wastewater is removed and the flushing wastewater is concentrated, and a small amount of organic additives are added after the concentrate reaches the concentration of the electroplating solution, the nickel-containing flushing wastewater can be recycled. In order to ensure the purity of the electroplating solution, no new substances can be introduced during the removal of organic matter. Summary of the invention
[0008] In order to solve the above technical problems, the purpose of the present invention is to provide a method for advanced oxidation and zero discharge of nickel electroplating flushing wastewater.
[0009] The technical solution of the present invention is:
[0010] A method for advanced oxidation and zero discharge of nickel electroplating flushing wastewater, comprising the following steps:
[0011] (1) Electroplating nickel washing wastewater is mixed with H2O2 in a pipeline mixer I, and then enters an activated carbon catalytic reactor I after mixing. The activated carbon catalytic reactor I is filled with activated carbon particles loaded with a catalyst;
[0012] (2) The effluent from the activated carbon catalytic reactor I enters the membrane distillation concentration device: the effluent from the activated carbon catalytic reactor I is heated to 50-80°C. The membrane of the membrane distillation system is a hydrophobic membrane. The water vapor from the heated nickel-containing flushing wastewater side passes through the membrane and enters the steam side. On the steam side, a vacuum pump is used to pump the water vapor that has passed through the membrane into a condenser, where the water vapor is condensed into condensed water.
[0013] (3) The concentrated liquid after membrane distillation is mixed with H2O2 in the pipeline mixer II, and then enters the activated carbon catalytic reactor II. The hydraulic retention time of the concentrated liquid in the activated carbon catalytic reactor II is 18 to 24 hours.
[0014] Furthermore, in the step (1), the water quality of the nickel electroplating rinsing wastewater is: Ni 2+ 300~1000mg / L, Cl - 80~300mg / L, SO4 2- 250~800mg / L, B20~70mg / L, COD80~400mg / L.
[0015] Furthermore, in the step (1), the mass ratio of H2O2 added is H2O2:COD=2:1 to 3:1.
[0016] Furthermore, in step (1), the hydraulic retention time of the nickel electroplating flushing wastewater in the activated carbon catalytic reactor I is 1 to 3 hours.
[0017] Furthermore, the heating in step (2) can be achieved by steam heating, electric heating or heating using waste flue gas or the like.
[0018] Furthermore, in step (2), the membrane distillation concentration adopts multi-stage series concentration, and the concentrated liquid after membrane concentration is circulated to the inlet of the membrane distillation component for further concentration until the nickel content in the concentrated liquid reaches the requirement of the electroplating liquid, and part of the concentrated liquid is discharged, and the concentrated liquid enters the subsequent treatment system for further treatment.
[0019] Furthermore, the multi-stage series concentration is 2-5 stages.
[0020] According to the method for advanced oxidation and zero emission of nickel electroplating flushing wastewater of the present invention, preferably, the activated carbon particles loaded with catalyst in step (1) and step (3) are prepared by the following steps: selecting coconut shell granular activated carbon, the particle size of the activated carbon is 3-5 mm, washing, drying, immersing the dried activated carbon in nitric acid, the concentration of nitric acid is 10-30%, adding cobalt nitrate and nickel nitrate, wherein the molar ratio of cobalt nitrate to nickel nitrate is 2:1-1:2, heating the solution to 80-85°C, and reacting at a constant temperature for 8-10 hours; filtering and drying to constant weight, placing the activated carbon adsorbed with cobalt nitrate and nickel nitrate in a carbonization furnace, heating to 750-850°C, keeping the temperature constant for 2-3 hours, and then cooling to room temperature to form a cobalt and nickel activated carbon catalyst.
[0021] Furthermore, the drying is carried out in a drying oven at 105°C.
[0022] Furthermore, in the step (3), the mass ratio of H2O2 added is H2O2:COD=4:1~6:1. Detailed description of the invention:
[0024] The water quality of nickel electroplating rinsing wastewater is as follows: Ni 2+ 300~1000mg / L, Cl - 80~300mg / L, SO4 2- 250~800mg / L, B20~70mg / L, COD80~400mg / L
[0025] The electroplating nickel washing wastewater to be treated is mixed with H2O2 in the pipeline mixer I. The amount of H2O2 added is in accordance with the mass ratio of H2O2:COD of 2:1 to 3:1. After mixing, it enters the activated carbon catalytic reactor I. The hydraulic retention time of the electroplating nickel washing wastewater in the activated carbon catalytic reactor I is 1 to 3 hours. The activated carbon catalytic reactor I is filled with activated carbon particles loaded with catalysts. In the activated carbon catalytic reactor I, H2O2, as an oxidant, oxidizes and decomposes the organic pollutants in the washing wastewater into harmless substances such as carbon dioxide and water under the catalytic action of the catalyst; at the same time, the activated carbon has a certain adsorption effect, which can first adsorb the organic matter in the activated carbon particles, prolong the contact time between the organic matter and the catalyst, and improve the oxidation efficiency. H2O2 is decomposed into H2O and O2, and no new substances will be added; the catalyst itself, as a catalyst for the oxidation reaction, does not participate in the reaction and will not change. It is recycled after the reaction, and does not affect the use of the concentrated and recovered electroplating solution.
[0026] The preparation process of the high-efficiency catalyst is as follows: coconut shell granular activated carbon is selected, and the particle size of the activated carbon is 3-5 mm. The activated carbon is rinsed with pure water and placed in a drying oven at 105°C to dry to constant weight. The dried activated carbon is soaked in nitric acid, the concentration of nitric acid is 10-30%, cobalt nitrate (Co(NO3)2) and nickel nitrate (Ni(NO3)2) are added, wherein the molar ratio of cobalt nitrate to nickel nitrate is 2:1-1:2, the solution is heated to 80-85°C, and the reaction is carried out at a constant temperature for 8-10 hours; after the reaction is completed, the water is filtered out by vacuum filtration, and the activated carbon is placed in a drying oven at 105°C to dry to constant weight; then the dried activated carbon adsorbed with cobalt nitrate and nickel nitrate is placed in a carbonization furnace, the temperature is raised to 750-850°C, the temperature is kept constant for 2-3 hours, and then cooled to room temperature, so that Co and Ni are loaded on the surface of the activated carbon to form a cobalt and nickel activated carbon catalyst, which has a good catalytic oxidation effect on organic matter.
[0027] The effluent from the activated carbon catalytic reactor I enters the membrane distillation concentration device. The effluent from the activated carbon catalytic reactor I is heated to 50-80°C. The heating can be done by steam heating, electric heating or waste flue gas heating. The membrane of the membrane distillation system is a hydrophobic membrane that only allows water vapor to pass through. The water vapor on the side of the heated nickel-containing flushing wastewater passes through the membrane and enters the steam side. On the water vapor side, a vacuum pump is used to pump the water vapor that passes through the membrane into the condenser, thereby ensuring the vapor pressure difference on both sides of the membrane. The water vapor is condensed into condensed water in the condenser, and the condensed water is returned to the production process for use. In order to ensure the quality of the produced water, multi-stage series concentration (2-5 stages) can be used, and the water produced by the following stages is used as the inlet water of the first stage. The concentrated liquid after membrane concentration is circulated to the inlet of the membrane distillation component for further concentration until the nickel content in the concentrated liquid reaches the requirements of the electroplating solution (nickel ion content 10-20%), and part of the concentrated liquid begins to be discharged, and the concentrated liquid enters the subsequent treatment system for further treatment.
[0028] After concentration by membrane distillation, the organic matter content in the concentrate is also concentrated. In order to ensure the purity of the plating solution, the organic matter in it needs to be further removed. The concentrate is mixed with H2O2 in the pipeline mixer Ⅱ. The amount of H2O2 added is 4.:1 to 6:1 according to H2O2:COD. After mixing, it enters the activated carbon catalytic reactor Ⅱ. The hydraulic retention time of the concentrate in the activated carbon catalytic reactor Ⅱ is 18 to 24 hours. The structure of the activated carbon catalytic reactor Ⅱ is the same as that of the activated carbon catalytic reactor Ⅰ. The organic matter in the concentrate is continued to be decomposed in the activated carbon catalytic reactor to further reduce the concentration of organic matter.
[0029] Beneficial Effects
[0030] The present invention provides a method for zero discharge of electroplating nickel-containing flushing wastewater, wherein the flushing wastewater is treated by primary hydrogen peroxide high-efficiency activated carbon catalytic oxidation, membrane distillation concentration, and secondary hydrogen peroxide high-efficiency activated carbon catalytic oxidation. The water produced by membrane distillation is recycled as flushing water, and the water produced by secondary hydrogen peroxide high-efficiency activated carbon catalytic oxidation can also be recycled as plating solution after adding a small amount of organic additives. After being treated by the present invention, the water and effective plating solution components such as nickel chloride, nickel sulfate, and boric acid in the electroplating flushing wastewater can be recycled respectively, and the process does not generate waste. The invention has both economic and environmental protection effects, and has good social and environmental benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a process flow chart of the method for advanced oxidation and zero discharge of nickel electroplating flushing wastewater provided by the present invention. DETAILED DESCRIPTION
[0032] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with embodiments, but the content of the present invention is not limited to the following embodiments.
[0033] Example 1
[0034] Water quality of nickel electroplating rinsing wastewater: Ni 2+ 650mg / L, Cl - 165mg / L, SO4 2- 523mg / L, B45mg / L, COD230mg / L.
[0035] H2O2 is mixed with nickel electroplating flushing wastewater, with a H2O2:COD mass ratio of 2.5:1, and then enters the activated carbon catalytic reactor I. The hydraulic retention time of nickel electroplating flushing wastewater in the activated carbon catalytic reactor I is 2h. The COD in the effluent of the activated carbon catalytic reactor I is 19mg / L.
[0036] The preparation process of the high-efficiency catalyst is as follows: coconut shell granular activated carbon is selected, and the particle size of the activated carbon is 3-5 mm. The activated carbon is rinsed with pure water and placed in a drying oven at 105°C to dry to constant weight. The dried activated carbon is soaked in nitric acid with a concentration of 20%, and cobalt nitrate (Co(NO3)2) and nickel nitrate (Ni(NO3)2) are added, wherein the molar ratio of cobalt nitrate to nickel nitrate is 1:1, and the solution is heated to 85°C and reacted at a constant temperature for 9 hours; after the reaction is completed, the water is filtered out by vacuum filtration and placed in a drying oven at 105°C to dry to constant weight; then the activated carbon adsorbed with nitric acid and nickel nitrate after drying is placed in a carbonization furnace, heated to 800°C, kept at a constant temperature for 2.5 hours, and then cooled to room temperature, so that Co and Ni are loaded on the surface of the activated carbon to form a cobalt and nickel activated carbon catalyst.
[0037] A two-stage membrane distillation concentration process was used to heat the effluent from the activated carbon catalytic reactor I to 70°C. The first-stage membrane distillation process produced water with a conductivity of 3.2μs / cm, Ni of 0.01mg / L, Ni of 11.2g / L, and COD of 425mg / L in the concentrated solution. The second-stage membrane distillation process produced water with a conductivity of 58.63μs / cm, Ni of 2.5mg / L, Ni of 142g / L, and COD of 5120mg / L in the concentrated solution.
[0038] H2O2 was added to the membrane distillation concentrate, and the H2O2 addition amount was 5:1 according to the H2O2:COD mass ratio. The hydraulic retention time of the concentrate in the activated carbon catalytic reactor II was 21h. The COD of the effluent of the activated carbon catalytic reactor II was reduced to 305mg / L.
[0039] Example 2
[0040] Water quality of nickel electroplating rinsing wastewater: Ni 2+ 320mg / L, Cl - 90mg / L, SO4 2- 295mg / L, B23mg / L, COD102mg / L.
[0041] H2O2 is mixed with nickel electroplating flushing wastewater, with a mass ratio of H2O2:COD of 2:1, and then enters the activated carbon catalytic reactor I. The hydraulic retention time of nickel electroplating flushing wastewater in the activated carbon catalytic reactor I is 1h. The COD in the effluent of the activated carbon catalytic reactor I is 16mg / L.
[0042] The preparation process of the high-efficiency catalyst is as follows: coconut shell granular activated carbon is selected, and the particle size of the activated carbon is 3-5 mm. The activated carbon is rinsed with pure water and placed in a drying oven at 105°C to dry to constant weight. The dried activated carbon is soaked in nitric acid with a concentration of 10%, and cobalt nitrate (Co(NO3)2) and nickel nitrate (Ni(NO3)2) are added, wherein the molar ratio of cobalt nitrate to nickel nitrate is 2:1, and the solution is heated to 80°C and reacted at a constant temperature for 10 hours; after the reaction, the water is filtered out by vacuum filtration and placed in a drying oven at 105°C to dry to constant weight; then the activated carbon adsorbed with nitric acid and nickel nitrate after drying is placed in a carbonization furnace, heated to 750°C, kept at a constant temperature for 2 hours, and then cooled to room temperature, so that Co and Ni are loaded on the surface of the activated carbon to form a cobalt and nickel activated carbon catalyst.
[0043] A two-stage membrane distillation concentration process was used to heat the effluent from the activated carbon catalytic reactor I to 50°C. The first-stage membrane distillation process produced water with a conductivity of 3.2μs / cm, Ni0.01mg / L, Ni11.2g / L, and COD425mg / L in the concentrated solution. The second-stage membrane distillation process produced water with a conductivity of 58.63μs / cm, Ni2.5mg / L, Ni142g / L, and COD4580mg / L in the concentrated solution.
[0044] H2O2 was added to the membrane distillation concentrate, and the H2O2 addition amount was based on a H2O2:COD mass ratio of 4:1. The hydraulic retention time of the concentrate in the activated carbon catalytic reactor II was 21h. The COD of the effluent from the activated carbon catalytic reactor II was reduced to 231mg / L.
[0045] Example 3
[0046] Water quality of nickel electroplating rinsing wastewater: Ni 2+ 930mg / L, Cl - 290mg / L, SO4 2- 740mg / L, B63mg / L, COD352mg / L.
[0047] H2O2 is mixed with nickel electroplating washing wastewater, with a mass ratio of H2O2:COD of 3:1, and then enters the activated carbon catalytic reactor I. The hydraulic retention time of nickel electroplating washing wastewater in the activated carbon catalytic reactor I is 3h. The COD in the effluent of the activated carbon catalytic reactor I is 25mg / L.
[0048] The preparation process of the high-efficiency catalyst is as follows: coconut shell granular activated carbon is selected, and the particle size of the activated carbon is 3-5 mm. The activated carbon is rinsed with pure water and placed in a drying oven at 105°C to dry to constant weight. The dried activated carbon is soaked in nitric acid with a concentration of 30%, and cobalt nitrate (Co(NO3)2) and nickel nitrate (Ni(NO3)2) are added, wherein the molar ratio of cobalt nitrate to nickel nitrate is 1:2, and the solution is heated to 85°C and reacted at a constant temperature for 8 hours; after the reaction is completed, the water is filtered out by vacuum filtration and placed in a drying oven at 105°C to dry to constant weight; then the dried activated carbon adsorbed with nitric acid and nickel nitrate is placed in a carbonization furnace, heated to 850°C, kept at a constant temperature for 2 hours, and then cooled to room temperature, so that Co and Ni are loaded on the surface of the activated carbon to form a cobalt and nickel activated carbon catalyst, which has a good catalytic oxidation effect on organic matter.
[0049] A two-stage membrane distillation concentration process was used to heat the effluent from the activated carbon catalytic reactor I to 80°C. The first-stage membrane distillation process produced water with a conductivity of 7.5μs / cm, Ni of 0.02mg / L, Ni of 15.3g / L, and COD of 562mg / L in the concentrated solution. The second-stage membrane distillation process produced water with a conductivity of 91.5μs / cm, Ni of 3.69mg / L, Ni of 178g / L, and COD of 6210mg / L in the concentrated solution.
[0050] H2O2 was added to the membrane distillation concentrate, and the H2O2 addition amount was based on a H2O2:COD mass ratio of 6:1. The hydraulic retention time of the concentrate in the activated carbon catalytic reactor II was 24h. The COD of the effluent from the activated carbon catalytic reactor II was reduced to 326mg / L.
[0051] This embodiment. Those skilled in the art should recognize that the above embodiments are only used to illustrate the present invention, and are not intended to limit the present invention. As long as they are within the spirit of the present invention, any changes or modifications to the above embodiments will fall within the scope of the claims of the present invention.
Claims
1. A method for advanced oxidation and zero discharge of nickel electroplating rinsing wastewater, characterized in that: The steps include: (1) Electroplating nickel washing wastewater is mixed with H2O2 in a pipeline mixer I, and then enters an activated carbon catalytic reactor I after mixing. The activated carbon catalytic reactor I is filled with activated carbon particles loaded with a catalyst; (2) The effluent from the activated carbon catalytic reactor I enters the membrane distillation concentration device: the effluent from the activated carbon catalytic reactor I is heated to 50-80°C. The membrane of the membrane distillation system is a hydrophobic membrane. The water vapor from the heated nickel-containing flushing wastewater side passes through the membrane and enters the steam side. On the steam side, a vacuum pump is used to pump the water vapor that has passed through the membrane into a condenser, where the water vapor is condensed into condensed water. (3) The concentrated liquid after membrane distillation is mixed with H2O2 in the pipeline mixer II, and then enters the activated carbon catalytic reactor II. The hydraulic retention time of the concentrated liquid in the activated carbon catalytic reactor II is 18 to 24 hours.
2. The method for advanced oxidation and zero discharge of nickel electroplating rinsing wastewater according to claim 1, characterized in that: The water quality of the nickel electroplating rinsing wastewater in step (1): Ni 2+ 300~1000mg / L, Cl - 80~300mg / L, SO4 2- 250~800mg / L, B20~70mg / L, COD80~400mg / L.
3. The method for advanced oxidation and zero discharge of nickel electroplating rinsing wastewater according to claim 1, characterized in that: In the step (1), the mass ratio of H2O2 added is H2O2:COD=2:1-3:
1.
4. The method for advanced oxidation and zero discharge of nickel electroplating rinsing wastewater according to claim 1, characterized in that: In the step (1), the hydraulic retention time of the nickel electroplating flushing wastewater in the activated carbon catalytic reactor I is 1 to 3 hours.
5. The method for advanced oxidation and zero discharge of nickel electroplating rinsing wastewater according to claim 1, characterized in that: The heating in step (2) can be steam heating, electric heating or heating using waste flue gas.
6. The method for advanced oxidation and zero discharge of nickel electroplating rinsing wastewater according to claim 1, characterized in that: In step (2), membrane distillation concentration adopts multi-stage series concentration, and the concentrated liquid after membrane concentration is circulated to the inlet of the membrane distillation component for further concentration until the nickel content in the concentrated liquid reaches the requirement of the electroplating liquid, and part of the concentrated liquid is discharged, and the concentrated liquid enters the subsequent treatment system for further treatment.
7. The method for advanced oxidation and zero discharge of nickel electroplating rinsing wastewater according to claim 6, characterized in that: The multi-stage series concentration is 2-5 stages.
8. The method for advanced oxidation and zero discharge of nickel electroplating rinsing wastewater according to claim 1, characterized in that: The activated carbon particles loaded with the catalyst in step (1) and step (3) are prepared by the following steps: selecting coconut shell granular activated carbon with a particle size of 3 to 5 mm, washing and drying, soaking the dried activated carbon in nitric acid with a concentration of 10 to 30%, adding cobalt nitrate and nickel nitrate, wherein the molar ratio of cobalt nitrate to nickel nitrate is 2:1 to 1:2, heating the solution to 80 to 85°C, and reacting at a constant temperature for 8 to 10 hours; filtering and drying to constant weight, placing the activated carbon adsorbed with cobalt nitrate and nickel nitrate in a carbonization furnace, heating to 750 to 850°C, keeping the temperature constant for 2 to 3 hours, and then cooling to room temperature to form a cobalt and nickel activated carbon catalyst.
9. The method for advanced oxidation and zero discharge of nickel electroplating rinsing wastewater according to claim 8, characterized in that: The drying is carried out in a drying oven at 105°C.
10. The method for advanced oxidation and zero discharge of nickel electroplating rinsing wastewater according to claim 1, characterized in that: In the step (3), the mass ratio of H2O2 added is H2O2:COD=4:1-6:1.
Citation Information
Patent Citations
Device for recycling nickel in nickel-containing wastewater of electroplating assembly line
CN104418442A
Wooden active carbon composite material for super capacitor and preparing method of wooden activated carbon composite material
CN104916452A
Preparation method of modified activated carbon catalyst for Fenton-like treatment
CN109894115A
Fe-Ni-Co composite Fenton-like catalyst and preparation method thereof
CN111151251A
Transition metal monatomic active catalyst as well as preparation method and application thereof
CN113600170A