Method for harmlessly applying aluminum electrolysis waste refractory material to preparation of asphalt mixture

The aluminum electrolytic waste refractory materials treated with calcium salt and biological materials are mixed with asphalt, which solves the problem of its safe application and stability in asphalt mixtures, significantly improves the high temperature and water stability performance of asphalt mixtures, and reduces The consumption of limestone ore powder realizes resource recycling and environmental protection.

CN118724508APending Publication Date: 2024-10-01GUANGXI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410996648.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

How to process aluminum electrolysis waste refractory materials so that they can be used safely and long-term in asphalt mixtures and ensure high temperature stability and water stability.

Method used

After calcium salt precipitation treatment, biomaterials chitosan and glutaraldehyde are used for acid and alkali resistance treatment, and superhydrophobic modification is performed to obtain surface organic superhydrophobic aluminum electrolytic waste refractory materials mixed with asphalt and coarse and fine aggregates. Aluminum electrolysis waste refractory material asphalt mixture is formed.

Benefits of technology

It achieves harmless treatment of waste, improves the high-temperature stability and water stability of asphalt mixtures, reduces the consumption of high-quality limestone powder, alleviates the problem of lack of mineral resources, and significantly improves the water resistance of asphalt mixtures. Stripping capabilities and environmental benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004960420520000061
    Figure BDA0004960420520000061
  • Figure BDA0004960420520000071
    Figure BDA0004960420520000071
  • Figure BDA0004960420520000072
    Figure BDA0004960420520000072
Patent Text Reader

Abstract

The invention provides a method for harmlessly applying an aluminum electrolysis waste refractory material to preparation of an asphalt mixture, which comprises the following steps: precipitating the aluminum electrolysis waste refractory material with calcium salt, treating with a biological material chitosan, carrying out acid and alkali resistance treatment with glutaraldehyde, and finally carrying out super-hydrophobic modification. And heating the obtained surface organic super-hydrophobic aluminum electrolysis waste refractory material, asphalt and coarse and fine aggregate, and mixing in an asphalt mixture stirrer. The method endows the aluminum electrolysis waste refractory material with acid and alkali resistant environment stability and non-polar end groups, has excellent adhesion performance with asphalt, and effectively controls the exudation of the toxicity of the aluminum electrolysis waste refractory material, so that the aluminum electrolysis waste refractory material can be safely applied to an asphalt mixture, and the service life of the aluminum electrolysis waste refractory material is prolonged. Meanwhile, the high-temperature stability and the water stability of the asphalt mixture are remarkably improved, and remarkable social benefits and environmental protection benefits are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of highway pavement engineering, and in particular to a method for harmlessly applying waste refractory materials from aluminum electrolysis to prepare asphalt mixture. Background Art

[0002] Highway construction is the focus of my country's infrastructure construction, and the mileage of highways is increasing year by year. Asphalt pavement has the advantages of short construction period, continuous and seamless structure, stable driving environment, and easy maintenance, more than 90% of highway pavements adopt asphalt concrete structure. Mineral powder is one of the key components in asphalt concrete. With its fine particle characteristics and high activity, mineral powder plays an important role in asphalt mixture, enhancing the density, impermeability and crack resistance of the road, thereby effectively extending the service life of the road. However, large-scale road construction around the world in the past few decades, especially the rapid development of highways, has greatly increased the demand for mineral powder, leading to rapid consumption of natural resources.

[0003] In modern industrial production, the process of aluminum electrolysis produces a large amount of waste refractory materials (SPL), which contain a variety of chemical components and metal oxides, such as alumina, silicate, and a small amount of fluoride and carbon. The harmless treatment and resource utilization of these waste materials have become important issues in the field of environmental protection and resource recycling. At present, the methods for treating such waste refractory materials mainly include landfill, recycling and chemical treatment. However, landfill not only occupies a large amount of land, but also may cause groundwater pollution. Although chemical treatment methods can separate useful components, the processing cost is high and the by-product treatment is complicated. Recycling and reuse need to solve the problem of harmlessness of harmful components in the material before it can be widely used in other industries.

[0004] For aluminum electrolysis waste refractory materials, research shows that their main components are silicate materials, alumina, etc., which can be used as excellent fillers in building materials. However, due to the fluoride and other harmful substances contained, direct use of these wastes has certain risks in environmental protection. Therefore, developing a method to safely utilize these waste refractory materials in asphalt mixtures is of great significance to environmental protection and resource recycling.

[0005] The solution proposed by the present invention aims to effectively remove or fix harmful substances in waste refractory materials through specific processing technology, so that they can be safely used in the preparation of asphalt mixtures. By changing the microstructure and chemical stability of waste materials through physical and chemical methods while maintaining their filling properties, it not only achieves harmless treatment of waste, but also improves the pavement performance of the final product. Summary of the invention

[0006] The technical problem to be solved by the present invention is: how to treat aluminum electrolysis waste refractory materials (SPL) so that they can be used safely and for a long time in asphalt mixtures, and also ensure the high temperature stability and water stability of the asphalt mixtures.

[0007] The technical problem to be solved by the present invention is achieved through the following technical solutions:

[0008] A method for harmlessly applying aluminum electrolysis waste refractory materials to prepare asphalt mixtures comprises the following steps: subjecting the aluminum electrolysis waste refractory materials to calcium salt precipitation, treating them with biomaterial chitosan, further treating them with glutaraldehyde for acid and alkali resistance, and finally performing superhydrophobic modification. The obtained surface organic superhydrophobic aluminum electrolysis waste refractory materials, asphalt, and coarse and fine aggregates are heated and mixed in an asphalt mixture mixer.

[0009] The method for harmlessly using waste refractory materials from aluminum electrolysis to prepare asphalt mixture comprises the following steps:

[0010] 1) Preparation of surface organic super-hydrophobic aluminum electrolysis waste refractory materials:

[0011] ① Take the powder of waste refractory materials from aluminum electrolysis, add deionized water and calcium hypochlorite, and continue to stir and react for more than 24 hours; then add calcium chloride, continue to stir and react for more than 24 hours, and then filter;

[0012] ② The filter cake obtained in step ① was repeatedly washed until the pH of the filtrate was 6-8, the filter cake was taken out and dried in a vacuum drying oven at 60°C for 24 hours, and then crushed through a 200-mesh sieve to obtain a solid powder for later use;

[0013] ③ Take chitosan and add it to acetic acid solution, and stir vigorously at 60℃ for 2h to fully dissolve it;

[0014] ④ Add the solid powder obtained in step ② to the solution obtained in step ③, stir vigorously for 6 hours to fully disperse it, then add sodium hydroxide solution, continue stirring and reacting for 10 minutes and then filter;

[0015] ⑤ Wash the filter cake obtained in step ④ repeatedly until the pH of the filtrate is 6-8, take out the filter cake and dry it in a vacuum drying oven at 60°C for 24 hours for later use;

[0016] ⑥ Add glutaraldehyde aqueous solution to the filter cake obtained in step ⑤ and continue stirring and reacting for 6 hours. After standing for 18 hours, filter with suction, take out the filter cake and dry it in a vacuum drying oven at 60°C for 24 hours for later use;

[0017] ⑦ Prepare an ethanol aqueous solution with a volume ratio of V (anhydrous ethanol): V (deionized water) = 3:1, add hydrochloric acid to adjust the pH to 4-5, add octyl triethoxy silane according to the volume ratio of octyl triethoxy silane to the ethanol aqueous solution being 1%, and continue stirring the hydrolysis reaction at room temperature for 72 hours;

[0018] ⑧ Add the filter cake obtained in step ⑥ to the solution reacted in step ⑦ and continue stirring and reacting for 24 hours before filtering;

[0019] ⑨ Take out the filter cake obtained in step ⑧ and wash it repeatedly until the pH of the filtrate is 6-8, take out the filter cake and dry it in a vacuum drying oven at 60° C. for 24 hours to obtain the surface organic super-hydrophobic aluminum electrolysis waste refractory material, which is recorded as OTS-CS-SPL for standby use;

[0020] 2) Take asphalt, coarse and fine aggregates and OTS-CS-SPL, place them in an oven at 180°C and heat them for 4 hours, then place the asphalt, coarse and fine aggregates and OTS-CS-SPL in an asphalt mixture mixer for mixing, and after mixing for 2 minutes, an asphalt mixture of aluminum electrolysis waste refractory materials is obtained.

[0021] Preferably, the mass ratio of the aluminum electrolysis waste refractory material, calcium hypochlorite and calcium chloride in step ① is 1:1:5.

[0022] Preferably, the mass ratio of the solid powder in step ② to the chitosan in step ③ is 50:1.

[0023] Preferably, the usage ratio of the filter cake obtained in step ⑤ to the 2.5% by mass glutaraldehyde aqueous solution is 1 g:3 mL.

[0024] Preferably, the mass ratio of the asphalt, coarse and fine aggregates and OTS-CS-SPL is 5:96:4.

[0025] Preferably, the asphalt is one of road petroleum asphalt No. 70 and SBS modified asphalt.

[0026] Preferably, the coarse and fine aggregates are diabase.

[0027] Preferably, the aluminum electrolysis waste refractory material is obtained by grinding with a vibrating screen machine, and the aluminum electrolysis waste refractory material simultaneously meets the requirements that the proportion of less than 0.6 mm is 100%, the proportion of less than 0.15 mm is 90-100%, and the proportion of less than 0.075 mm is 90-100%.

[0028] Compared with the prior art, the present invention has the following technical effects:

[0029] (1) The present invention uses OTS-CS-SPL to replace limestone powder, which can greatly reduce the consumption of high-quality limestone powder, alleviate the problem of mineral resource scarcity, and is beneficial to ecological environment protection. The surface of the treated OTS-CS-SPL material is grafted with octyl carbon chain non-polar functional groups, showing super hydrophobicity, solving the problem that polar non-polar functional groups such as silicate materials and fluorides have good compatibility with asphalt molecules, making the aluminum electrolysis waste refractory material adhere better to asphalt and have strong water-resistant stripping ability; SPL is a hazardous solid waste. According to statistics, the annual discharge of aluminum electrolysis waste refractory materials in my country is as high as 1.1 million tons. The present invention uses SPL to prepare OTS-CS-SPL, which is widely used in asphalt concrete, which is beneficial to environmental governance, saving resources, and turning waste into treasure.

[0030] (2) The present invention is to treat SPL with biomaterial chitosan after calcium salt precipitation, and then use glutaraldehyde to treat CS-SPL with acid and alkali resistance, and finally perform superhydrophobic modification. This method gives SPL acid and alkali resistance stability and non-polar end groups, has excellent adhesion properties with asphalt, effectively controls the toxicity of SPL itself, enables it to be safely used in asphalt mixtures, and significantly improves the high temperature stability and water stability of asphalt mixtures, with significant social and environmental benefits. DETAILED DESCRIPTION

[0031] Example 1

[0032] A method for harmlessly treating waste refractory materials from aluminum electrolysis and applying them to prepare asphalt mixture, comprising the following steps:

[0033] 1) Preparation of surface organic super-hydrophobic aluminum electrolysis waste refractory material (OTS-CS-SPL):

[0034] ① Take 100g of aluminum electrolysis waste refractory (SPL) powder, add 1000mL of deionized water and 100g of calcium hypochlorite, and continue to stir and react for more than 24h; then add 500g of calcium chloride, continue to stir and react for more than 24h and then filter; the SPL powder is obtained by grinding with a vibrating screen machine, and the particle size of the SPL powder satisfies the following requirements: the proportion of less than 0.6mm is 100%, the proportion of less than 0.15mm is 90-100%, and the proportion of less than 0.075mm is 90-100%.

[0035] ② The filter cake obtained in step ① was repeatedly washed until the pH of the filtrate was 6, the filter cake was taken out and dried in a vacuum drying oven at 60°C for 24 hours, and then crushed through a 200-mesh sieve to obtain a solid powder for later use;

[0036] ③ Take 1.0g chitosan and add 200mL 5% (v / v) acetic acid solution, and stir vigorously at 60℃ for 2h to fully dissolve it;

[0037] ④ Add 50.0 g of the solid powder obtained in step ② to the entire solution obtained in step ③, stir vigorously for 6 h to fully disperse it, then add 100 mL of 1 mol / L sodium hydroxide solution, continue stirring and reacting for 10 min, and then filter;

[0038] ⑤ The filter cake obtained in step ④ was repeatedly washed until the pH of the filtrate was 6, and the filter cake was taken out and dried in a vacuum drying oven at 60°C for 24 hours for later use;

[0039] ⑥ Add 2.5% glutaraldehyde aqueous solution to the filter cake obtained in step ⑤ at a ratio of 1 g:3 mL, and continue stirring and reacting for 6 hours. After standing for 18 hours, filter the filter cake with suction, and dry it in a vacuum drying oven at 60°C for 24 hours for later use;

[0040] ⑦ Prepare an ethanol aqueous solution with a volume ratio of V (anhydrous ethanol): V (deionized water) = 3:1, add 0.1 mol / L hydrochloric acid to adjust the pH to 4, add octyl triethoxy silane according to the volume ratio of octyl triethoxy silane to the ethanol aqueous solution of 1%, and continue stirring and hydrolyzing for 72 hours at room temperature;

[0041] ⑧ Add the filter cake obtained in step ⑥ to the solution reacted in step ⑦ in a ratio of 1 g:5 mL, continue stirring and reacting for 24 hours, and then filter;

[0042] ⑨ Take out the filter cake obtained in step ⑧ and wash it repeatedly until the pH of the filtrate is 6, take out the filter cake and dry it in a vacuum drying oven at 60°C for 24 hours to obtain OTS-CS-SPL for use;

[0043] 2) No. 70 road petroleum asphalt, diabase and OTS-CS-SPL were weighed in a mass ratio of 5:96:4, and placed in an oven at 180°C for heating for 4 hours. Then, No. 70 road petroleum asphalt, diabase and OTS-CS-SPL were placed in an asphalt mixture mixer for mixing. After mixing for 2 minutes, an asphalt mixture of aluminum electrolysis waste refractory materials was obtained.

[0044] Example 2

[0045] A method for harmlessly treating waste refractory materials from aluminum electrolysis and applying them to prepare asphalt mixture, comprising the following steps:

[0046] 1) Preparation of surface organic super-hydrophobic aluminum electrolysis waste refractory material (OTS-CS-SPL):

[0047] ① Take 100g of SPL powder, add 1000mL of deionized water and 100g of calcium hypochlorite, and continue to stir and react for more than 24h; then add 500g of calcium chloride, continue to stir and react for more than 24h and then filter; the SPL powder is obtained by grinding with a vibrating screen machine, and the particle size of the SPL powder satisfies the following requirements: 100% is less than 0.6mm, 90-100% is less than 0.15mm, and 90-100% is less than 0.075mm.

[0048] ② The filter cake obtained in step ① was repeatedly washed until the pH of the filtrate was 7, the filter cake was taken out and dried in a vacuum drying oven at 60°C for 24 hours, and then crushed through a 200-mesh sieve to obtain a solid powder for later use;

[0049] ③ Take 1.0g chitosan and add 200mL 5% (v / v) acetic acid solution, and stir vigorously at 60℃ for 2h to fully dissolve it;

[0050] ④ Add 50.0 g of the solid powder obtained in step ② to the entire solution obtained in step ③, stir vigorously for 6 h to fully disperse it, then add 100 mL of 1 mol / L sodium hydroxide solution, continue stirring and reacting for 10 min, and then filter;

[0051] ⑤ Wash the filter cake obtained in step ④ repeatedly until the pH of the filtrate is 7, take out the filter cake and dry it in a vacuum drying oven at 60°C for 24 hours for later use;

[0052] ⑥ Add 2.5% glutaraldehyde aqueous solution to the filter cake obtained in step ⑤ at a ratio of 1 g:3 mL, and continue stirring and reacting for 6 hours. After standing for 18 hours, filter the filter cake with suction, and dry it in a vacuum drying oven at 60°C for 24 hours for later use;

[0053] ⑦ Prepare an ethanol aqueous solution with a volume ratio of V (anhydrous ethanol): V (deionized water) = 3:1, add 0.1 mol / L hydrochloric acid to adjust the pH to 4.5, add octyl triethoxy silane according to the volume ratio of octyl triethoxy silane to the ethanol aqueous solution of 1%, and continue stirring the hydrolysis reaction at room temperature for 72 hours;

[0054] ⑧ Add the filter cake obtained in step ⑥ to the solution reacted in step ⑦ in a ratio of 1 g:5 mL, continue stirring and reacting for 24 hours, and then filter;

[0055] ⑨ Take out the filter cake obtained in step ⑧ and wash it repeatedly until the pH of the filtrate is 7, take out the filter cake and dry it in a vacuum drying oven at 60°C for 24 hours to obtain OTS-CS-SPL for use;

[0056] 2) The preparation of asphalt mixture of waste refractory materials from aluminum electrolysis is the same as in Example 1.

[0057] Example 3

[0058] A method for harmlessly treating waste refractory materials from aluminum electrolysis and applying them to prepare asphalt mixture, comprising the following steps:

[0059] 1) Preparation of surface organic super-hydrophobic aluminum electrolysis waste refractory material (OTS-CS-SPL):

[0060] ① Take 100g of SPL powder, add 1000mL of deionized water and 100g of calcium hypochlorite, and continue to stir and react for more than 24h; then add 500g of calcium chloride, continue to stir and react for more than 24h and then filter; the SPL powder is obtained by grinding with a vibrating screen machine, and the particle size of the SPL powder satisfies the following requirements: 100% is less than 0.6mm, 90-100% is less than 0.15mm, and 90-100% is less than 0.075mm.

[0061] ② The filter cake obtained in step ① was repeatedly washed until the pH of the filtrate was 8, the filter cake was taken out and dried in a vacuum drying oven at 60°C for 24 hours, and then crushed through a 200-mesh sieve to obtain a solid powder for later use;

[0062] ③ Take 1.0g chitosan and add 200mL 5% (v / v) acetic acid solution, and stir vigorously at 60℃ for 2h to fully dissolve it;

[0063] ④ Add 50.0 g of the solid powder obtained in step ② to the entire solution obtained in step ③, stir vigorously for 6 h to fully disperse it, then add 100 mL of 1 mol / L sodium hydroxide solution, continue stirring and reacting for 10 min, and then filter;

[0064] ⑤ The filter cake obtained in step ④ was repeatedly washed until the pH of the filtrate was 8, and the filter cake was taken out and dried in a vacuum drying oven at 60°C for 24 hours for later use;

[0065] ⑥ Add 2.5% glutaraldehyde aqueous solution to the filter cake obtained in step ⑤ at a ratio of 1 g:3 mL, and continue stirring and reacting for 6 hours. After standing for 18 hours, filter the filter cake with suction, and dry it in a vacuum drying oven at 60°C for 24 hours for later use;

[0066] ⑦ Prepare an ethanol aqueous solution with a volume ratio of V (anhydrous ethanol): V (deionized water) = 3:1, add 0.1 mol / L hydrochloric acid to adjust the pH to 5, add octyl triethoxy silane according to the volume ratio of octyl triethoxy silane to the ethanol aqueous solution of 1%, and continue stirring and hydrolyzing for 72 hours at room temperature;

[0067] ⑧ Add the filter cake obtained in step ⑥ to the solution reacted in step ⑦ in a ratio of 1 g:5 mL, continue stirring and reacting for 24 hours, and then filter;

[0068] ⑨ Take out the filter cake obtained in step ⑧ and wash it repeatedly until the pH of the filtrate is 8, take out the filter cake and dry it in a vacuum drying oven at 60°C for 24 hours to obtain OTS-CS-SPL for use;

[0069] 2) The preparation of asphalt mixture of waste refractory materials from aluminum electrolysis is the same as in Example 1.

[0070] Example 4

[0071] A method for harmlessly treating waste refractory materials from aluminum electrolysis and applying them to prepare asphalt mixture, comprising the following steps:

[0072] 1) The preparation of the surface organic super-hydrophobic aluminum electrolysis waste refractory material (OTS-CS-SPL) is the same as in Example 1;

[0073] 2) SBS modified asphalt, diabase and OTS-CS-SPL were weighed in a mass ratio of 5:96:4, and heated in an oven at 180°C for 4 hours. Then, the SBS modified asphalt, diabase and OTS-CS-SPL were mixed in an asphalt mixture mixer. After mixing for 2 minutes, an asphalt mixture of aluminum electrolysis waste refractory materials was obtained.

[0074] Example 5

[0075] A method for harmlessly treating waste refractory materials from aluminum electrolysis and applying them to prepare asphalt mixture, comprising the following steps:

[0076] 1) The preparation of the surface organic super-hydrophobic aluminum electrolysis waste refractory material (OTS-CS-SPL) is the same as in Example 2;

[0077] 2) The preparation of asphalt mixture of waste refractory materials from aluminum electrolysis is the same as in Example 4.

[0078] Example 6

[0079] A method for harmlessly treating waste refractory materials from aluminum electrolysis and applying them to prepare asphalt mixture, comprising the following steps:

[0080] 1) The preparation of the surface organic super-hydrophobic aluminum electrolysis waste refractory material (OTS-CS-SPL) is the same as in Example 3;

[0081] 2) The preparation of asphalt mixture of waste refractory materials from aluminum electrolysis is the same as in Example 4.

[0082] Comparative Example 1:

[0083] Replace OTS-CS-SPL with limestone powder of the same proportion. Other materials and preparation processes are as follows:

[0084] Road petroleum asphalt No. 70, diabase and limestone powder are weighed in a mass ratio of 5:96:4, placed in an oven at 180°C for heating for 4 hours, and then placed in an asphalt mixture mixer for mixing. After mixing for 2 minutes, the asphalt mixture is obtained.

[0085] Comparative Example 2:

[0086] Replace OTS-CS-SPL with limestone powder of the same proportion. Other materials and preparation processes are as follows:

[0087] SBS modified asphalt, diabase and limestone powder were weighed in a mass ratio of 5:96:4, heated in an oven at 180°C for 4 hours, and then mixed in an asphalt mixer. After mixing for 2 minutes, the asphalt mixture was obtained.

[0088] The asphalt mixture prepared by the above method was tested for performance according to the current domestic standards "Test Procedure for Asphalt and Asphalt Mixture for Highway Engineering" (JTG E20-2011) and "Solid Waste Leaching Reading Material Leaching Method Horizontal Oscillation Method" (HJ 557-2010):

[0089] Test items:

[0090]

[0091]

[0092] The standard rutting test, the Marshall test and the freeze-thaw splitting test were all tested in accordance with the "Testing Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" (JTG E20-2011). In order to further verify the effect of OTS-CS-SPL on the high-temperature performance of asphalt concrete, and considering the long-term hot and humid climate conditions in the southern region, on the basis of the standard rutting test, the test wheel contact pressure was kept at 0.7MPa, and the test temperature was increased from 60℃ to 70℃, and the asphalt mixture was subjected to a high-temperature rutting test. At the same time, combined with the current situation of the increasing number of automobiles in my country, the continuous development of the transportation industry, and the increase in the average load of freight trucks or even overloading, on the basis of the standard rutting test, the test temperature was kept at 60℃, and the test wheel contact pressure was increased from 0.7MPa to 1.0MPa, and the asphalt mixture was subjected to a heavy-load rutting test.

[0093] The fluoride ion leaching experiment of asphalt mixture is carried out according to the "Solid Waste Leaching Reading Leaching Method Horizontal Oscillation Method" HJ557-2010, and the fluoride ion concentration test in the leachate is carried out according to the method of "Hazardous Waste Identification Standard Toxic Substance Content Identification" GB5085.6-2007.

[0094] In addition, in order to further verify the effect of OTS-CS-SPL on the water stability of asphalt concrete, a water rutting test was conducted on the basis of the standard rutting test. The test temperature was kept at 60°C and the test wheel contact pressure was kept at 0.7MPa. The rutting specimens that had been formed and placed at room temperature for 48 hours were placed in a stainless steel high-temperature resistant basin together with the test mold. A sufficient amount of 60°C water was injected to completely immerse the specimens and the test mold. The basin containing the specimens and 60°C water was then transferred to an oven set at 60°C for 5 hours, followed by a rutting test to explore the effect of OTS-CS-SPL on the anti-rutting performance of asphalt concrete under pavement immersion conditions.

[0095] The test results are as follows:

[0096] 1. High temperature stability study:

[0097]

[0098] It can be seen from the test results and comparison results that due to the addition of OTS-CS-SPL, the standard dynamic stability of the matrix asphalt mixture reached a maximum of 6115 times / mm, and the standard dynamic stability of the SBS asphalt mixture reached a maximum of 7980 times / mm, which can enhance the anti-rutting performance of the asphalt mixture and to a certain extent improve and maintain the ability of the asphalt mixture to resist rutting damage.

[0099] 2. Water stability study:

[0100] (I) Immersion Marshall test:

[0101] Test Project Standard stability (kN) Standard flow value (mm) Water immersion stability (kN) Residual stability (%) Example 1 13.11 4.78 11.04 84.21 Example 2 12.35 4.66 10.96 88.74 Example 3 11.91 4.97 10.31 86.57 Comparative Example 1 11.43 5.83 9.05 79.18 Example 4 14.76 3.31 13.33 90.34 Example 5 14.80 4.09 13.64 92.13 Example 6 15.18 4.41 13.45 88.64 Comparative Example 2 10.92 5.33 9.17 83.91

[0102] It can be seen from the test results and comparative results that due to the addition of OTS-CS-SPL, the residual stability of the matrix asphalt mixture after immersion in water reached a maximum of 88.74%, and the residual stability of the SBS asphalt mixture after immersion in water reached a maximum of 92.13%. Compared with mineral powder fillers, OTS-CS-SPL can effectively improve the water stability of asphalt mixtures.

[0103] (II) Freeze-thaw splitting test:

[0104]

[0105] From the test results and comparison results, it can be seen that due to the addition of OTS-CS-SPL, the freeze-thaw splitting tensile strength ratio of the matrix asphalt mixture reached a maximum of 91.45%, and the freeze-thaw splitting tensile strength ratio of the SBS asphalt mixture reached a maximum of 95.74%. Compared with mineral powder fillers, OTS-CS-SPL improves and maintains the water stability of asphalt mixtures to a certain extent.

[0106] (III) Water rutting test:

[0107] Test Project Dynamic stability under water immersion (times / mm) Example 1 3979 Example 2 3848 Example 3 3451 Comparative Example 1 2049 Example 4 3946 Example 5 4403 Example 6 4112 Comparative Example 2 3554

[0108] It can be seen from the test results and comparative results that due to the addition of OTS-CS-SPL, the dynamic stability of the matrix asphalt mixture under water immersion has increased to 3979 times / mm at most, and the dynamic stability of the SBS asphalt mixture under water immersion has increased to 4403 times / mm at most. Compared with mineral powder filler, the addition of OTS-CS-SPL can also improve and maintain the ability of the asphalt mixture to resist rutting disease to a certain extent, and also improve and maintain the ability of the asphalt mixture to resist water damage to a certain extent.

[0109] 3. Safety Research:

[0110] Fluoride ion leaching test:

[0111] Test Project Fluoride ion concentration of leachate (mg / L) Example 1 1.87 Example 2 0.96 Example 3 1.39 Example 4 0.97 Example 5 1.44 Example 6 1.11

[0112] It can be seen from the test results and comparative results that the maximum fluoride ion leaching liquid of asphalt mixture is only 1.87 mg / L (<100 mg / L), which is far less than the requirement of the specification (GB 5085.6-2007). After the surface organic superhydrophobic treatment, SPL is more compatible with asphalt. There is a barrier of asphalt molecules between water molecules and inorganic fluorides in SPL, which effectively reduces the ionization of inorganic fluorides in water and effectively inhibits the leaching of fluoride ions.

Claims

1. A method for harmlessly treating waste refractory materials from aluminum electrolysis and applying them to prepare asphalt mixture, characterized in that: The aluminum electrolysis waste refractory material is treated with biomaterial chitosan after calcium salt precipitation, and then treated with glutaraldehyde for acid and alkali resistance, and finally subjected to superhydrophobic modification. The obtained surface organic superhydrophobic aluminum electrolysis waste refractory material and asphalt, coarse and fine aggregates are heated and mixed in an asphalt mixture mixer.

2. The method for harmlessly treating waste refractory materials from aluminum electrolysis and applying them to prepare asphalt mixture according to claim 1, characterized in that: The following steps are involved: 1) Preparation of surface organic super-hydrophobic aluminum electrolysis waste refractory materials: ① Take the powder of waste refractory materials from aluminum electrolysis, add deionized water and calcium hypochlorite, and continue to stir and react for more than 24 hours; then add calcium chloride, continue to stir and react for more than 24 hours, and then filter; ② The filter cake obtained in step ① was repeatedly washed until the pH of the filtrate was 6-8, the filter cake was taken out and dried in a vacuum drying oven at 60°C for 24 hours, and then crushed through a 200-mesh sieve to obtain a solid powder for later use; ③ Take chitosan and add it to acetic acid solution, and stir vigorously at 60℃ for 2h to fully dissolve it; ④ Add the solid powder obtained in step ② to the solution obtained in step ③, vigorously stir for 6 hours to fully disperse it, then add sodium hydroxide solution, continue stirring and reacting for 10 minutes and then filter; ⑤ Wash the filter cake obtained in step ④ repeatedly until the pH of the filtrate is 6-8, take out the filter cake and dry it in a vacuum drying oven at 60°C for 24 hours for later use; ⑥ Add glutaraldehyde aqueous solution to the filter cake obtained in step ⑤ and continue stirring and reacting for 6 hours. After standing for 18 hours, filter with suction, take out the filter cake and dry it in a vacuum drying oven at 60°C for 24 hours for later use; ⑦ Prepare an ethanol aqueous solution with a volume ratio of V (anhydrous ethanol): V (deionized water) = 3:1, add hydrochloric acid to adjust the pH to 4-5, add octyl triethoxy silane according to the volume ratio of octyl triethoxy silane to the ethanol aqueous solution being 1%, and continue stirring the hydrolysis reaction at room temperature for 72 hours; ⑧ Add the filter cake obtained in step ⑥ to the solution reacted in step ⑦ and continue stirring and reacting for 24 hours before filtering; ⑨ Take out the filter cake obtained in step ⑧ and wash it repeatedly until the pH value of the filtrate is 6-8, take out the filter cake and dry it in a vacuum drying oven at 60° C. for 24 hours to obtain the surface organic super-hydrophobic aluminum electrolysis waste refractory material, which is recorded as OTS-CS-SPL for standby use; 2) Take asphalt, coarse and fine aggregates and OTS-CS-SPL, place them in an oven at 180°C and heat them for 4 hours, then place the asphalt, coarse and fine aggregates and OTS-CS-SPL in an asphalt mixture mixer for mixing, and after mixing for 2 minutes, an asphalt mixture of aluminum electrolysis waste refractory materials is obtained.

3. The method for harmlessly treating waste refractory materials from aluminum electrolysis and applying them to prepare asphalt mixture according to claim 2, characterized in that: The mass ratio of the aluminum electrolysis waste refractory material, calcium hypochlorite and calcium chloride in step ① is 1:1:

5.

4. The method for harmlessly treating waste refractory materials from aluminum electrolysis and applying them to prepare asphalt mixture according to claim 2, characterized in that: The mass ratio of the solid powder in step ② to the chitosan in step ③ is 50:

1.

5. The method for harmlessly treating waste refractory materials from aluminum electrolysis and applying them to prepare asphalt mixture according to claim 2, characterized in that: The usage ratio of the filter cake obtained in step ⑤ to the 2.5% by mass glutaraldehyde aqueous solution is 1 g:3 mL.

6. The method for harmlessly treating waste refractory materials from aluminum electrolysis and applying them to prepare asphalt mixture according to claim 2, characterized in that: The mass ratio of the asphalt, coarse and fine aggregates and OTS-CS-SPL is 5:96:

4.

7. The method for harmlessly treating waste refractory materials from aluminum electrolysis and applying them to prepare asphalt mixture according to claim 2, characterized in that: The asphalt is one of road petroleum asphalt No. 70 and SBS modified asphalt.

8. The method for harmlessly treating waste refractory materials from aluminum electrolysis and applying them to prepare asphalt mixture according to claim 2, characterized in that: The coarse and fine aggregates are diabase.

9. The method for harmlessly treating waste refractory materials from aluminum electrolysis and applying them to prepare asphalt mixture according to claim 2, characterized in that: The aluminum electrolysis waste refractory material is obtained by grinding with a vibrating screen machine, and the aluminum electrolysis waste refractory material meets the requirements of 100% being less than 0.6 mm, 90-100% being less than 0.15 mm, and 90-100% being less than 0.075 mm.