Preparation method and application of super-plasticizing enhancer for filling gold ore full-tailing paste
By using superplasticizing strengtheners in the gold mine tailings paste, the problems of low filling mass concentration, long initial setting time and insufficient body strength are solved, achieving efficient filling effects and an environmentally friendly production process.
Patent Information
- Application Number
- CN202410862637.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-01
AI Technical Summary
The high methylene blue content of the whole tailings of the gold mine results in a thick slurry that is difficult to transport, increases water demand, has a long initial setting time, has low filling mass concentration and body strength, and is high in cost.
A superplasticizing strengthener is used to prepare a combination of materials A, B and C, using polyether monomers, hydroxyethyl acrylate, polyethylene glycol, ammonium persulfate, ferrous iron, mercaptopropionic acid, VC, acrylic acid, triethanolamine and other materials form an environmentally friendly high plasticizing and strengthening functional solvent, which is used to improve the filling quality of gold mine tailings paste.
It effectively improves the filling mass concentration and body strength, shortens the initial setting time, reduces the filling cost, forms a stable homogeneous body, prevents solid-liquid separation and water volatilization, and improves the dispersion and fluidity of the slurry.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of mine filling, and in particular relates to a superplasticizing intensifier for gold mine full tailings paste filling and a preparation method thereof, as well as an application of the superplasticizing intensifier in gold mine full tailings paste filling materials. Background Art
[0002] The whole tailings of gold mines have a high content of methylene blue and poor binding properties with cementitious material particles. A high content of methylene blue usually causes the slurry to be too viscous and difficult to transport, resulting in increased water demand when using tailings for filling, long initial setting time, low filling mass concentration, low filling body strength, and large amounts of cementitious materials.
[0003] The solution to the above-mentioned gold mine tailings filling defects is to add new materials to solve the problems of high filling cost, low filling mass concentration and low filling body strength of gold mine underground filling slurry. Therefore, how to improve the filling mass concentration and filling body strength of gold mine tailings filling and reduce the initial setting time and filling cost has become the research focus of existing technicians.
[0004] In response to these problems faced by full tailings filling in gold mines, the technicians of the present invention have developed a superplasticizer strengthening agent for full tailings filling in gold mines to solve the problems of low mass concentration of full tailings filling in gold mines, long initial setting time, low filling body strength, etc., to improve the filling efficiency, increase the mineral mining rate and the safety level of mine production. Summary of the invention
[0005] The purpose of the present invention is to provide a superplasticizing strengthener for gold mine tailings paste filling. The preparation method is simple and easy to operate, and can effectively improve the problems of low mass concentration, long initial setting time, low filling strength and the like of gold mine tailings filling. The present invention belongs to a green and environmentally friendly new material.
[0006] In order to achieve the purpose of the present invention, the present invention provides a method for preparing a superplasticizing intensifier for gold mine tailings paste filling, which specifically comprises the following steps: S1. Material A: Add an appropriate amount of deionized water to the reactor and start stirring, add polyether monomers, and then add hydroxyethyl acrylate, polyethylene glycol, ammonium persulfate, and ferrous iron in sequence to fully dissolve them; S2. Prepare material B: Add an appropriate amount of deionized water to the container bottle, add mercaptopropionic acid and VC, and fully dissolve them; S3. Preparation of material C: Add an appropriate amount of deionized water to a container bottle, add acrylic acid, triethanolamine and deionized water to fully dissolve; S4. Add the above material B dropwise into material A, stir and react for 4-6 hours, then add material C, stir and mix for 1-2 hours to obtain a superplasticizer.
[0007] Furthermore, in step S4, the initial dropping temperature of material B does not exceed 20°C, the dropping time is 120-200 min, the dropping end temperature does not exceed 30°C, and the stirring reaction temperature does not exceed 30°C.
[0008] Furthermore, in step S4, the initial dropping temperature of the C material is not more than 30°C, the dropping time is 120-150 min, the dropping end temperature is not more than 60°C, and the stirring reaction temperature is not more than 60°C.
[0009] Furthermore, the superplasticizing strengthener is composed of the following raw materials in parts by weight: 65-85 parts of material A, 15-25 parts of material B, and 10-20 parts of material C.
[0010] Furthermore, the material A is composed of the following components in parts by weight: 45-65 parts of polyether monomers, 10-25 parts of hydroxyethyl acrylate, 5-10 parts of polyethylene glycol, 0.5-2 parts of ammonium persulfate, 5-7.5 parts of ferrous iron and 5-15 parts of deionized water.
[0011] Furthermore, the polyether monomer is any one of vinyl polyoxyethylene ether, methyl allyl polyether or isopentanol polyoxyethylene ether.
[0012] Furthermore, the mass ratio of mercaptopropionic acid to VC in the material B is (0.5-0.7):1.
[0013] Furthermore, the mass ratio of acrylic acid to triethanolamine in the C material is (0.3-0.5):1.
[0014] The superplasticizing intensifier for gold mine tailings paste filling provided by the present invention can be applied to gold mine tailings paste filling and is added at 0.1-0.2% of the total mass of the gold mine tailings paste filling slurry.
[0015] The present invention has achieved the following beneficial effects: 1. The superplasticizing enhancer of the present invention adopts a unique physical and chemical process at room temperature and pressure, and is prepared by a composite of environmentally friendly biomass and safe and environmentally friendly surfactants. It is a safe, non-toxic, harmless, environmentally friendly high-plasticizing enhancing functional solvent, which has the functions of preventing slurry from bleeding and segregation, reducing viscosity, and improving filling mass concentration and filling body strength. It is a new green and environmentally friendly material.
[0016] 2. The superplasticizer of the present invention can combine the dispersed particles in the filling slurry with other particles and water around it to form a weak but strong three-dimensional spatial structure, thereby effectively preventing the precipitation of particles and preventing the separation between solid and liquid; at the same time, the colloid, mine tailings and water can be fully dispersed to form a stable homogeneous body without segregation or water seepage, shortening the initial setting time and preventing mud after consolidation.
[0017] 3. The present invention adopts acrylic acid and triethanolamine as C materials and dopes them in the formula, which can increase the density of the slurry, thereby improving the hardness of the filling body, improving the interaction force between the slurry particles, reducing the tendency of particle aggregation, and improving the dispersibility of the slurry. Through its adsorption on the surface of the slurry particles, it can effectively prevent the volatilization of water, improve the fluidity of the slurry, and reduce the adhesion and internal friction of the slurry to a certain extent.
[0018] 4. The present invention adjusts appropriate proportions of polyethylene glycol, hydroxyethyl acrylate, acrylic acid, and triethanolamine to react with water, whole tailings, and cementitious materials in the slurry, thereby promoting the hydration reaction of the cementitious materials, reducing the porosity in the slurry, and increasing the stability and homogeneity of the slurry, thereby effectively improving the problems of low mass concentration of whole tailings paste filling in gold mines, long initial setting time, and low filling strength.
[0019] 5. The superplasticizing strengthener of the present invention can give full play to the hydration and hardening bonding performance of the colloid particles and the gold tailings particles, thereby greatly improving the strength of the filling body. DETAILED DESCRIPTION
[0020] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] The preparation method and application of the superplasticizing strengthening agent for gold mine tailings paste filling of the present invention are described below in conjunction with specific embodiments. Example 1
[0022] The preparation method of the superplasticizing strengthening agent for filling the gold mine tailings paste in this embodiment is as follows: S1. Configuration of material A: After adding 1.17kg of deionized water to the reactor, stirring was started, 4.5kg of methyl allyl polyether was added, followed by 2.5kg of hydroxyethyl acrylate, 1.0kg of polyethylene glycol, 150g of ammonium persulfate, 680g of ferrous iron, and stirred until completely dissolved; S2. Prepare material B: add an appropriate amount of deionized water to a container bottle, add 3kg of mercaptopropionic acid and 5kg of VC (vitamin C), and fully dissolve; S3. Preparation of material C: Add an appropriate amount of deionized water to a container bottle, add 2kg of acrylic acid and 5kg of triethanolamine, and fully dissolve; S4. At a temperature below 20°C, place 6.5kg of material A in a reactor, then drop 2.5kg of material B into material A while stirring, and control the dropping time within 195±5min to ensure that the temperature does not exceed 30°C at the end of the dropping. After the dropping is completed, stir the reaction at a rate of 1200rpm for 6h, and the reaction temperature does not exceed 30°C; then drop 2.0kg of material C into material A while stirring, and control the dropping time within 145±5min. After the dropping is completed, stir and mix at a rate of 1200rpm for 2h, and the temperature does not exceed 60°C, and ensure that the temperature does not exceed 60°C at the end of the dropping, so as to obtain the required superplasticizer. Example 2
[0023] The preparation method of the superplasticizing strengthening agent for filling the gold mine tailings paste in this embodiment is as follows: S1. Configuration of material A: 1.3kg of deionized water was added to the reactor and stirring was started. 6.5kg of prenol polyoxyethylene ether was added, followed by 1.0kg of hydroxyethyl acrylate, 500g of polyethylene glycol, 200g of ammonium persulfate, 500g of ferrous iron, and stirred until completely dissolved; S2. Prepare material B: add an appropriate amount of deionized water to a container bottle, add 3kg of mercaptopropionic acid and 5kg of VC (vitamin C), and fully dissolve; S3. Preparation of material C: Add an appropriate amount of deionized water to a container bottle, add 2kg of acrylic acid and 5kg of triethanolamine, and fully dissolve; S4. At a temperature below 20°C, place 8.5kg of material A in a reactor, then drop 1.5kg of material B into material A while stirring, and control the dropping time within 140±5min to ensure that the temperature does not exceed 30°C at the end of the dropping. After the dropping is completed, stir the reaction at a rate of 1200rpm for 5h, and the reaction temperature does not exceed 30°C; then drop 1.0kg of material C into material A while stirring, and control the dropping time within 115±5min. After the dropping is completed, stir and mix at a rate of 1200rpm for 1.5h, and the temperature does not exceed 60°C, and ensure that the temperature does not exceed 60°C at the end of the dropping, to obtain the required superplasticizer. Example 3
[0024] The preparation method of the superplasticizing strengthening agent for filling the gold mine tailings paste in this embodiment is as follows: S1. Configuration of material A: After adding 1.08kg of deionized water to the reactor and stirring, add 5.8kg of vinyl polyoxyethylene ether, then add 1.6kg of hydroxyethyl acrylate, 800g of polyethylene glycol, 120g of ammonium persulfate, 600g of ferrous iron, and stir until completely dissolved; S2. Prepare material B: add an appropriate amount of deionized water to a container bottle, add 3kg of mercaptopropionic acid and 5kg of VC (vitamin C), and fully dissolve; S3. Preparation of material C: Add an appropriate amount of deionized water to a container bottle, add 2kg of acrylic acid and 5kg of triethanolamine, and fully dissolve; S4. Place 7.2kg of material A in a reactor at a temperature below 20°C, then drop 2.2kg of material B into material A while stirring, and control the dropping time within 180±5min to ensure that the temperature does not exceed 30°C at the end of the dropping. After the dropping is completed, stir the reaction at a rate of 1200rpm for 6h, and the reaction temperature does not exceed 30°C; then drop 1.6kg of material C into material A while stirring, and control the dropping time within 130±5min. After the dropping is completed, stir and mix at a rate of 1200rpm for 2h, and the temperature does not exceed 60°C, and ensure that the temperature does not exceed 60°C at the end of the dropping, and the desired superplasticizer is obtained. Comparative Example 1
[0025] The preparation method of the superplasticizing strengthening agent for gold mine tailings paste filling and the raw materials and proportions used in this comparative example 1 are the same as those in Example 3, and specific reference is made to Example 3. The difference is that the formula A in this comparative example 1 is different, and the preparation method of the material A is as follows: at room temperature, 2.4 kg of deionized water is added to the reactor and stirring is started, 7.0 kg of vinyl polyoxyethylene ether is added, and 200 g of itaconic acid, 50 g of ammonium persulfate, and 850 g of ferrous iron are added in sequence every 5 minutes, and stirred until completely dissolved. Comparative Example 2
[0026] The preparation method of the superplasticizing agent for gold mine tailings paste filling and the raw materials and proportions used in this comparative example 2 are the same as those in Example 3, and specific reference is made to Example 3. The difference is that the B formula in this comparative example 2 is different, and the preparation method of the B material is: add an appropriate amount of deionized water to a container, add 4kg of mercaptopropionic acid and 5kg of VC, and fully dissolve. Comparative Example 3
[0027] The preparation method of the superplasticizing agent for gold mine tailings paste filling and the raw materials and proportions used in this comparative example 3 are the same as those in Example 3, and specific reference is made to Example 3. The difference is that step S4 in this comparative example 3 is: at a temperature below 20° C., material B and material C are directly added to material A in sequence, and the temperature is controlled within 60° C. and stirred for reaction for 8 hours to obtain the product. Comparative Example 4
[0028] The preparation method of the superplasticizing agent for gold mine tailings paste filling and the raw materials and proportions used in this comparative example 4 are the same as those in Example 3, and specific reference is made to Example 3. The difference is that the feeding temperature, the dropwise addition end temperature and the reaction temperature are not controlled in step S4 of this comparative example 4, that is, at room temperature, material A is placed in a reaction kettle, and then material B is added dropwise to material A, and the dropping time is controlled within 180±5min, and the stirring reaction is carried out at a rate of 1200rpm for 6h after the dropping is completed; material C is then added dropwise to material A, and the dropping time is controlled within 130±5min, and the stirring reaction is carried out at a rate of 1200rpm for 2h after the dropping is completed, so as to obtain the desired superplasticizing agent.
[0029] The superplasticizer prepared in the above Examples 1-3 and Comparative Examples 1-4 was added to the gold mine tailings paste filling slurry, and prepared according to the method of "Test Method for Cement Mortar Strength (ISO)" (GB / T17671-2021). After preparation, various properties were tested according to the corresponding standards. The test results are shown in Table 1 below. Among them, the gold mine tailings paste filling slurry is composed of gold mine tailings, the superplasticizer of the present invention, a binder and water; the filling concentration refers to the mass percentage of the filling components (i.e., solid components) in the filling slurry, including gold mine tailings, a binder and a superplasticizer; the binder is a reference cement (P.O42.5) used by the building materials department to test the properties of admixtures, and the dosage is based on the total solid mass; the particle size of the gold mine tailings is 35% above 75 microns, 70% below 75 microns, and 50% below 38 microns; the superplasticizer (i.e., the reagent referred to in Table 1) is prepared in this embodiment and the comparative example, and the dosage (i.e., the reagent dosage) is based on the total solid mass; the water is tap water. Please refer to the preparation parameters and test items in Table 1 below.
[0030] Table 1 Performance test data of gold mine tailings paste filling slurry
[0031] It can be seen from the test data in Table 1 above that after the superplasticizer is added to the gold mine tailings paste filling slurry, the amount of filling cementitious material is significantly reduced, the filling mass concentration and filling body strength are improved, and the problems of low gold mine tailings filling mass concentration, high filling cost and low filling body strength are solved.
[0032] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0033] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A method for preparing a superplasticizing strengthening agent for filling gold mine tailings paste, characterized in that: The specific steps include: S1. Material A: Add an appropriate amount of deionized water to the reactor and start stirring, add polyether monomers, and then add hydroxyethyl acrylate, polyethylene glycol, ammonium persulfate, and ferrous iron in sequence to fully dissolve them; S2. Prepare material B: Add an appropriate amount of deionized water to the container bottle, add mercaptopropionic acid and VC, and fully dissolve them; S3. Preparation of material C: Add an appropriate amount of deionized water to a container bottle, add acrylic acid, triethanolamine and deionized water to fully dissolve; S4. Add the above material B dropwise into material A, stir and react for 4-6 hours, then add material C, stir and mix for 1-2 hours to obtain a superplasticizer.
2. The method for preparing a superplasticizing strengthening agent for filling a gold mine full tailings paste according to claim 1, characterized in that: In the step S4, the initial dropping temperature of the material B does not exceed 20°C, the dropping time is 120-200 min, the dropping end temperature does not exceed 30°C, and the stirring reaction temperature does not exceed 30°C.
3. The method for preparing a superplasticizing strengthening agent for filling a gold mine full tailings paste according to claim 1, characterized in that: In the step S4, the initial dropping temperature of the C material does not exceed 30°C, the dropping time is 120-150 min, the dropping end temperature does not exceed 60°C, and the stirring reaction temperature does not exceed 60°C.
4. The method for preparing a superplasticizing strengthening agent for filling a gold mine full tailings paste according to claim 1, characterized in that: The superplasticizing strengthener is composed of the following raw materials in parts by weight: 65-85 parts of material A, 15-25 parts of material B, and 10-20 parts of material C.
5. The method for preparing a superplasticizing strengthening agent for filling a gold mine full tailings paste according to claim 4, characterized in that: The material A is composed of the following components in parts by weight: 45-65 parts of polyether monomers, 10-25 parts of hydroxyethyl acrylate, 5-10 parts of polyethylene glycol, 0.5-2 parts of ammonium persulfate, 5-7.5 parts of ferrous iron and 5-15 parts of deionized water.
6. The method for preparing a superplasticizing strengthening agent for filling a gold mine full tailings paste according to claim 4, characterized in that: The polyether monomer is any one of vinyl polyoxyethylene ether, methyl allyl polyether or isopentanol polyoxyethylene ether.
7. The method for preparing a superplasticizing strengthening agent for filling a gold mine full tailings paste according to claim 4, characterized in that: The mass ratio of mercaptopropionic acid to VC in the material B is (0.5-0.7):
1.
8. The method for preparing a superplasticizing strengthening agent for filling gold mine tailings paste according to claim 4, characterized in that: The mass ratio of acrylic acid to triethanolamine in the C material is (0.3-0.5):
1.
9. An application of a superplasticizing strengthening agent for gold mine full tailings paste filling prepared by the preparation method according to any one of claims 1 to 8 in gold mine full tailings paste filling, characterized in that: Add 0.1-0.2% of the total mass of the gold mine tailings paste filling slurry.