Moisture and heat resistant epoxy resin based on plasma surface modification and preparation method thereof
Plasma surface modification of biphenyl epoxy resin solves the aging problem of epoxy resin in hot and humid environments, significantly improves its resistance to humid and heat, and is suitable for the application of high-voltage outdoor insulation materials.
Patent Information
- Application Number
- CN202410794532.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-19
AI Technical Summary
The existing epoxy resin ages in a hot and humid environment, causing the performance of the insulation material to decline and affecting the reliability of the power system. Moreover, traditional composite insulation materials have insufficient heat and humidity resistance, making it difficult to meet the needs of high-voltage outdoor applications.
Using a plasma surface modification method, the epoxy resin monomer is fused with raw materials such as biphenyl and 4,4'-diaminodiphenyl sulfone, and plasma modification treatment is performed under an argon atmosphere to increase the strength of the epoxy resin. Resistant to moisture and heat, forming a hydrophobic surface.
Significantly improves the moisture and heat resistance of epoxy resin, enhances its stability and insulation properties in humid environments, and extends the service life of the material.
Smart Images

Figure CN118725259A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polymer composite materials and electrical engineering, and specifically relates to a moisture-heat resistant epoxy resin based on plasma surface modification and a preparation method thereof. Background Art
[0002] In the natural environment, composite insulators are subjected to erosion and damage from various factors in the natural environment for a long time, especially erosion and aging caused by high humidity, alternating high and low temperatures, ultraviolet radiation, rain and acid rain in the atmospheric environment, and the degree of aging continues to increase with time; at the same time, the high-voltage electromagnetic field of the load will cause the polarization trend of the polar groups of the material and affect the material performance, causing the insulation material to age under the strong electromagnetic field. The moisture in the operating environment will reduce the insulation properties of the material, and the epoxy resin has poor thermal conductivity. It will continue to be affected by heat during the operation of the equipment, causing the epoxy resin to age; the equipment is subjected to the influence of moisture and heat for a long time, which will cause irreversible oxidation decomposition reactions, damage the insulation, and seriously affect the operational reliability of the power system.
[0003] To improve weather resistance, high-voltage outdoor composite insulators are generally composed of an insulating core rod, an umbrella cover, and an end metal fixed on the insulating core rod. Among them, the insulating core rod is made of epoxy resin-based fiber-reinforced composite materials, and the umbrella cover is mostly made of high-temperature vulcanized rubber or epoxy resin plus coating with strong weather resistance because it is directly facing a complex and changeable environment. Vulcanized silicone rubber is soft in texture and has poor mechanical strength. On the one hand, it limits its application scenarios. On the other hand, it is prone to discharge defects due to its inability to withstand bird pecking, which seriously endangers the normal operation of transmission lines; the structure of epoxy resin strong weather-resistant coating can well compensate for the shortcomings of silicone rubber's soft texture, but the coating also has the disadvantages of thin thickness, difficulty in homogenization, and poor long-term protection effect. Traditional composite insulator rod cores are made of bisphenol A epoxy resin to withstand mechanical and electrical loads; but its moisture and heat resistance is poor, so it is not suitable for external insulation materials that are in direct contact with the natural environment.
[0004] Therefore, it is necessary to study an epoxy resin external insulation material with strong moisture and heat resistance, which is of great significance to the stable operation of transmission lines. Summary of the invention
[0005] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.
[0006] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.
[0007] Therefore, the object of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing a moisture-heat resistant epoxy resin based on plasma surface modification.
[0008] In order to solve the above technical problems, the present invention provides the following technical solution: a method for preparing a moisture-heat resistant epoxy resin based on plasma surface modification, comprising:
[0009] When epoxy resin monomer is melted, it becomes a transparent light yellow liquid;
[0010] Add curing agent, stir until the curing agent is completely dispersed in the melted epoxy resin liquid, and vacuum it to remove bubbles;
[0011] Add an accelerator, stir, pour into a mold, and solidify to obtain an epoxy resin matrix;
[0012] The surface of the epoxy resin substrate is evenly coated with dimethyl silicone oil, and plasma modified in an argon atmosphere to obtain a modified moisture-heat resistant epoxy resin;
[0013] Wherein, the epoxy resin monomer includes biphenyl epoxy resin, the curing agent includes 4,4'-diaminodiphenyl sulfone, and the accelerator includes 2-ethyl-4-methylimidazole.
[0014] As a preferred embodiment of the preparation method of the present invention, the epoxy resin monomer is 30 to 35 parts, the curing agent is 20 to 25 parts, and the accelerator is 0.2 to 0.5 parts, calculated by weight of the raw materials.
[0015] As a preferred embodiment of the preparation method of the present invention, the biphenyl epoxy resin is a light yellow block solid, and the molar ratio of the biphenyl group to the epoxy group is 1:2.
[0016] As a preferred embodiment of the preparation method of the present invention, the curing agent is in the form of a white powder solid, and the molar ratio of the sulfone group to the amino group is 1:2.
[0017] As a preferred embodiment of the preparation method of the present invention, the epoxy resin monomer is melted, wherein the melting temperature is 120-130° C. and the melting time is 30-50 min.
[0018] As a preferred embodiment of the preparation method of the present invention, wherein: the curing obtains an epoxy resin matrix, wherein the curing conditions include:
[0019] After curing at 150°C for 1 hour, continue curing at 140°C for 4 hours.
[0020] As a preferred embodiment of the preparation method of the present invention, the plasma modification treatment has a discharge power of 50 W and a plasma modification treatment time of 20 to 30 minutes.
[0021] Another object of the present invention is to overcome the deficiencies in the prior art and provide a plasma surface-modified moisture- and heat-resistant epoxy resin.
[0022] Another object of the present invention is to overcome the deficiencies in the prior art and provide a plasma surface modified moisture and heat resistant epoxy resin for use as an external insulation material for transmission lines.
[0023] Beneficial effects of the present invention:
[0024] The present invention provides a method for preparing a moisture-heat resistant epoxy resin, wherein a biphenyl structure with higher skeleton strength and a sulfone structure with better thermal stability are introduced into the epoxy resin to increase the moisture-heat resistance of the epoxy resin from the inside;
[0025] At the same time, the surface of the epoxy resin is plasma modified to increase the hydrophobicity of the epoxy resin surface, making it more difficult for water molecules to enter the epoxy resin matrix when the epoxy resin is in a humid environment, thereby further enhancing the moisture and heat resistance of the epoxy resin. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:
[0027] Figure 1 Schematic diagram of a plasma modification platform in an embodiment of the present invention.
[0028] Figure 2 Schematic diagram of the mold in the embodiment of the present invention.
[0029] Figure 3 This is a physical picture of the biphenyl epoxy resin prepared in Example 1 of the present invention.
[0030] Figure 4 This is a physical picture of the bisphenol A epoxy resin prepared in Comparative Example 1 of the present invention.
[0031] Figure 5 This is a contact angle diagram of the modified epoxy resin in Example 2 of the present invention.
[0032] Figure 6 This is a contact angle diagram of epoxy resin before plasma modification in Example 2 of the present invention.
[0033] Figure 7 This is the contact angle diagram of the modified epoxy resin in Comparative Example 2 of the present invention.
[0034] Figure 8 This is the contact angle diagram of the modified epoxy resin in Comparative Example 3 of the present invention. DETAILED DESCRIPTION
[0035] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0036] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0037] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0038] Step 1: Prepare the raw materials required for the epoxy resin matrix:
[0039] Step 1.1, prepare 35 parts of biphenyl epoxy resin monomer, the raw material is Japanese jER biphenyl type crystalline epoxy YX4000 series, the supplier is Shanghai Zhongsi Industrial Co., Ltd., it is a light yellow block solid, and the molar ratio of biphenyl group to epoxy group is 1:2.
[0040] Step 1.2, prepare 25 parts of curing agent, the raw material is 4,4'-diaminodiphenyl sulfone, the supplier is Aladdin Biochemical Technology Co., Ltd., it is a white powder solid, and the molar ratio of the sulfone group to the amino group is 1:2.
[0041] Step 1.3, prepare 0.5 parts of accelerator, the raw material is 2-ethyl-4-methylimidazole, the supplier is Aladdin Biochemical Technology Co., Ltd., and it is a brown viscous transparent liquid.
[0042] Step 2, preparation of biphenyl epoxy resin:
[0043] Step 2.1, add the raw epoxy resin monomer into the reactor, heat it at 120°C for 30 minutes, and turn it into a transparent light yellow liquid after it is completely melted.
[0044] Step 2.2: Add curing agent powder in the mass ratio in step 1, stir for 30 minutes until the curing agent powder is completely dispersed in the melted epoxy resin liquid. This step is carried out at 120°C.
[0045] Step 2.3: Vacuum the mixture to remove air bubbles. This step is performed at 120°C.
[0046] Step 2.4: Spray the mold release agent on the mold and preheat it at 140°C.
[0047] Step 2.5, add accelerator in the mass ratio in step 1, stir for 2 minutes and then pour into the preheated mold. After curing at 150°C for 1 hour, continue curing at 140°C for 4 hours to obtain a biphenyl epoxy resin sheet.
[0048] Step 3: Plasma modification of the epoxy resin sheet obtained in step 2, as shown in the attached Figure 1 As shown, 1 is argon gas with a purity of 99.999%, 2 is a gas distributor with a set flow rate of 50 ml / min, 3 is a reaction chamber, 4 is a modified epoxy resin, 5 is a ground electrode, 6 is a high-voltage electrode, 7 is an AC power regulator, and 8 is an oscilloscope.
[0049] Step 3.1, placing the epoxy resin sheet prepared in step 2 in the high voltage electrode and the ground electrode in the reaction chamber, and evenly applying dimethyl silicone oil on the surface;
[0050] Step 3.2, continue to introduce argon gas for 3 minutes to remove the original air in the reaction chamber;
[0051] Step 3.3: Slowly increase the input voltage to about 30V and adjust the discharge frequency until a continuous and uniform arc appears between the upper and lower electrodes and the waveform of the oscilloscope tends to be stable. The discharge power is maintained at about 50W, and the plasma modification treatment is performed for 20 minutes.
[0052] Step 3.4: Turn the epoxy resin sheet over and repeat the above plasma modification steps to obtain a moisture-heat-resistant epoxy resin with enhanced surface hydrophobicity.
[0053] Example 1
[0054] Raw materials: biphenyl epoxy resin 10.68g, curing agent 4,4'-diaminodiphenyl sulfone 7.62g, accelerator 2-ethyl-4-methylimidazole 0.61g;
[0055] The raw epoxy resin monomer is added into the reactor and heated at 120°C for 30 minutes. After it is completely melted, it becomes a transparent light yellow liquid. The curing agent powder is added and stirred for 30 minutes until the curing agent powder is completely dispersed in the melted epoxy resin liquid. Vacuum treatment is performed to remove bubbles. The accelerator is added and stirred for 2 minutes. Then, the mixture is poured into a mold and cured at 150°C for 1 hour. Then, the curing is continued at 140°C for 4 hours to obtain a completely cross-linked biphenyl epoxy resin.
[0056] Biphenyl epoxy resin physical picture see Figure 3 .
[0057] Comparative Example 1
[0058] Compare with the most common bisphenol A epoxy resin on the market, keeping other conditions unchanged.
[0059] Raw materials: bisphenol A epoxy resin 11.12g, curing agent 4,4'-diaminodiphenyl sulfone 8.11g, accelerator 2-ethyl-4-methylimidazole 0.72g;
[0060] Add the raw epoxy resin monomer into the reactor, heat at 120°C for 30 minutes, add curing agent powder, stir for 30 minutes until the curing agent powder is completely dispersed in the melted epoxy resin liquid, vacuum treatment is performed to remove bubbles, add accelerator, stir for 2 minutes, then pour into the mold, cure at 150°C for 1 hour, and continue to cure at 140°C for 4 hours to obtain a completely cross-linked bisphenol A epoxy resin.
[0061] Bisphenol A epoxy resin physical picture see Figure 4 .
[0062] The two epoxy resins were placed in water at 95°C for hygrothermal aging. The moisture absorption rate per day and the measured glass transition temperature are shown in Table 1.
[0063] Moisture absorption rate η x The calculation is as follows:
[0064] η x =(m x -m 0 ) / m 0 ×100%
[0065] Where x is the number of days of aging, which can be 1, 2, 3, or 4; m 0 The quality before aging.
[0066] The measurement method of glass transition temperature refers to GB / T 19466.1-2004.
[0067] Table 1 Moisture absorption rate (%)
[0068]
[0069]
[0070] Table 2 Glass transition temperature (℃)
[0071] Aging days 1 2 3 4 Biphenyl epoxy resin 292 290 270 265 Bisphenol A epoxy resin 269 252 243 221
[0072] It can be found that the moisture absorption rate of the biphenyl epoxy resin in the present invention is always lower than that of the bisphenol A epoxy resin, and the glass transition temperature is always higher than that of the bisphenol A epoxy resin, which can prove that the biphenyl epoxy resin has a stronger moisture and heat resistance.
[0073] Example 2
[0074] Plasma modification of epoxy resin:
[0075] An epoxy resin sheet is placed in the high-voltage electrode and the ground electrode in the reaction chamber, and dimethyl silicone oil is evenly applied on its surface. As the hydrophobic Si-containing particles are modified to the epoxy resin surface by plasma, new Si-C and Si-O chemical bonds are formed. At the same time, the dimethyl silicone oil on the surface of the material prevents the O-containing active particles from contacting the epoxy resin surface, making it impossible for the hydrophilic active groups to be generated on the epoxy resin surface, thereby increasing the hydrophobicity of the epoxy resin surface.
[0076] Argon gas was continuously introduced for 3 minutes to remove the original air in the reaction chamber;
[0077] Slowly increase the input voltage to 30V and adjust the frequency until a continuous and uniform arc appears in the reactor, the waveform on the oscilloscope tends to be stable, and the discharge power remains at about 50W;
[0078] After 20 minutes of plasma modification, the epoxy resin sheet was turned over and the above steps were repeated.
[0079] The contact angle was measured to be about 113°, see Figure 5 .
[0080] The contact angle without plasma modification is about 87°, see Figure 6 .
[0081] It can be found that after plasma modification, the contact angle of the epoxy resin has been significantly improved. The higher the contact angle, the more difficult it is for water droplets to adhere to the surface of the epoxy resin, making it more difficult for water droplets to enter the interior of the epoxy resin.
[0082] Comparative Example 2
[0083] Under the conditions of Example 2, no dimethyl silicone oil is applied to the epoxy resin sheet, and other conditions are the same as those of Example 2.
[0084] like Figure 7The contact angle shown is 84°.
[0085] Comparative Example 3
[0086] Under the conditions of Example 2, dimethyl silicone oil was applied to the epoxy resin sheet, and no plasma treatment was performed. The surface was heated and dried (heating temperature was 60° C., time was 30 min). Other conditions were the same as in Example 2. The results were as follows: Figure 8 As shown, the contact angle is 98°.
[0087] It can be seen that the surface hydrophobicity of the epoxy resin is improved by applying dimethyl silicone oil on the epoxy resin sheet and combining with the synergistic effect of plasma.
[0088] Example 3
[0089] Raw materials: biphenyl epoxy resin 10.68g, curing agent 4,4'-diaminodiphenyl sulfone 6.62g, methyl hexahydrophthalic anhydride 1.0g, accelerator 2-ethyl-4-methylimidazole 0.61g;
[0090] Add the raw epoxy resin monomer into the reactor, heat at 120°C for 30 minutes, and turn into a transparent light yellow liquid after complete melting. Add the curing agent and stir for 30 minutes until the curing agent powder is completely dispersed in the melted epoxy resin liquid. Vacuum treatment is performed to remove bubbles, add the accelerator, stir for 2 minutes, and then pour into the mold. After curing at 150°C for 1 hour, continue to cure at 140°C for 4 hours to obtain a completely cross-linked biphenyl epoxy resin.
[0091] Example 4
[0092] Raw materials: biphenyl epoxy resin 10.68g, curing agent methyl hexahydrophthalic anhydride 7.62g, accelerator 2-ethyl-4-methylimidazole 0.61g;
[0093] Add the raw epoxy resin monomer into the reactor, heat at 120°C for 30 minutes, and turn into a transparent light yellow liquid after complete melting. Add the curing agent and stir for 30 minutes until the curing agent powder is completely dispersed in the melted epoxy resin liquid. Vacuum treatment is performed to remove bubbles, add the accelerator, stir for 2 minutes, and then pour into the mold. After curing at 150°C for 1 hour, continue to cure at 140°C for 4 hours to obtain a completely cross-linked biphenyl epoxy resin.
[0094] See Table 3 for moisture absorption rate.
[0095] Table 3
[0096] Aging days 1 2 3 4 Example 1 0.153 1.796 2.959 3.306 Example 3 0.122 1.476 2.749 3.278 Example 4 0.286 1.882 3.168 3.402
[0097] It can be seen that methyl hexahydrophthalic anhydride and 4,4'-diaminodiphenyl sulfone as curing agents synergistically improve the moisture and heat resistance of epoxy resin.
[0098] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the present invention.
Claims
1. A method for preparing a heat-resistant epoxy resin based on plasma surface modification, characterized in that: include, When epoxy resin monomer is melted, it becomes a transparent light yellow liquid; Add curing agent, stir until the curing agent is completely dispersed in the melted epoxy resin liquid, and vacuum it to remove bubbles; Add an accelerator, stir, pour into a mold, and solidify to obtain an epoxy resin matrix; The surface of the epoxy resin substrate is evenly coated with dimethyl silicone oil, and plasma modified in an argon atmosphere to obtain a modified moisture-heat resistant epoxy resin; Wherein, the epoxy resin monomer includes biphenyl epoxy resin, the curing agent includes 4,4'-diaminodiphenyl sulfone, and the accelerator includes 2-ethyl-4-methylimidazole.
2. The preparation method according to claim 1, characterized in that: Calculated by the mass proportion of the raw materials, the epoxy resin monomer is 30 to 35 parts, the curing agent is 20 to 25 parts, and the accelerator is 0.2 to 0.5 parts.
3. The preparation method according to claim 1 or 2, characterized in that: The biphenyl epoxy resin is a light yellow block solid, and the molar ratio of the biphenyl group to the epoxy group is 1:
2.
4. The preparation method according to claim 1, characterized in that: The curing agent is in the form of white powder solid, and the molar ratio of the sulfone group to the amino group is 1:
2.
5. The preparation method according to claim 1, characterized in that: The epoxy resin monomer is melted, wherein the melting temperature is 120-130° C. and the melting time is 30-50 minutes.
6. The preparation method according to claim 1, characterized in that: The curing obtains an epoxy resin matrix, wherein the curing conditions include: After curing at 150°C for 1 hour, continue curing at 140°C for 4 hours.
7. The preparation method according to claim 1, characterized in that: The plasma modification treatment has a discharge power of 50 W and a plasma modification treatment time of 20 to 30 minutes.
8. The plasma surface modified moisture and heat resistant epoxy resin obtained by the preparation method according to any one of claims 1 to 7.
9. Use of the plasma surface modified moisture and heat resistant epoxy resin as claimed in claim 8 as an external insulation material for transmission lines.
Citation Information
Patent Citations
Graphene microsphere / epoxy resin composite material and preparation method thereof
CN110511535A
Insulating die-bonding adhesive for coating back surface of wafer and preparation method of insulating die-bonding adhesive
CN111187588A
Single-component epoxy resin composition containing latent imidazole curing accelerator as well as preparation method and application thereof
CN112194779A