Thermoplastic polyolefin waterproof coiled material and preparation process thereof

Through the blending and process optimization of components such as polyolefin composite materials and thermoplastic elastomers, a thermoplastic polyolefin waterproof membrane with excellent performance is formed, which solves the problems of poor adhesion and difficult construction of existing membranes and improves durability. and construction efficiency, achieving environmentally friendly and sustainable material development.

CN118725468AInactive Publication Date: 2024-10-01JIANGSU HONGYUAN ZHONGFU WATERPROOF MATERIAL
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410963753.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing thermoplastic polyolefin waterproofing membranes have problems such as poor adhesion, high construction requirements, and difficulty in bonding when constructing complex base layers. In addition, traditional waterproofing materials have poor weather resistance, are prone to aging, and have high maintenance costs.

Method used

It uses components such as polyolefin composite materials, thermoplastic elastomers, nano-silicate fillers, liquid crystal polymers, inorganic nano-antibacterial agents, plasticizers, foaming agents and nucleating agents, through melt blending, foaming and The dispersion process forms a waterproof membrane with excellent performance, improving bonding strength and construction convenience.

Benefits of technology

It has significantly improved the comprehensive performance, durability, mechanical properties, antibacterial performance and construction efficiency of the membrane, extended its service life, and achieved environmentally friendly and sustainable material development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725468A_ABST
    Figure CN118725468A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of waterproof coiled materials, in particular to a thermoplastic polyolefin waterproof coiled material and a preparation process thereof, and solves the defects in the prior art. Comprising the following components: a polyolefin composite material, a thermoplastic elastomer, a nano silicate filler, a liquid crystal high-molecular polymer, an inorganic nano antibacterial agent, a plasticizer, a foaming agent, a nucleating agent and a crystallization accelerant. The novel waterproof coiled material with excellent performance is successfully prepared by accurately controlling the proportion and processing conditions of all the components. The coiled material not only has high strength, high elongation, excellent weather resistance and low-temperature flexibility, but also has good processability and mechanical properties. Besides, by introducing specific functional additives, such as a nano silicate filler, a liquid crystal high-molecular polymer and an inorganic nano antibacterial agent, the durability, the antibacterial property and the mechanical property of the coiled material are further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of waterproof coiled materials, and in particular to a thermoplastic polyolefin waterproof coiled material and a preparation process thereof. Background Art

[0002] With the rapid development of the construction industry, the demand for waterproof materials is increasing. Although traditional waterproof materials such as asphalt and rubber have certain waterproof effects, they have exposed many problems during long-term use, such as poor weather resistance, easy aging, and difficult construction. These problems not only affect the service life of waterproof materials, but also increase maintenance costs. Therefore, the development of a new type of waterproof material with superior performance, simple construction and environmental protection has become an urgent need in the industry.

[0003] As a new type of polymer material, thermoplastic polyolefin (TPO) has shown great application potential in the field of waterproof materials due to its excellent weather resistance, UV resistance, high temperature resistance and ozone resistance. However, the existing TPO waterproof membrane still has some shortcomings, such as poor adhesion, high construction requirements, and the need to splice multiple pieces when constructing complex bases, making it difficult to bond the overlaps.

[0004] Therefore, we propose a thermoplastic polyolefin waterproof membrane and a preparation process thereof to solve the above problems. Summary of the invention

[0005] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a thermoplastic polyolefin waterproofing membrane and a preparation process thereof.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A thermoplastic polyolefin waterproof coiled material comprises the following components in parts by weight: 40-50 parts of a polyolefin composite material, 10-20 parts of a thermoplastic elastomer, 5-10 parts of a nano-silicate filler, 5-10 parts of a liquid crystal high molecular polymer, 1-2 parts of an inorganic nano-antibacterial agent, 5-10 parts of a plasticizer, 2-5 parts of a foaming agent, 1-3 parts of a nucleating agent, and 0.5-2 parts of a crystallization accelerator.

[0008] As the preferred technical solution:

[0009] The thermoplastic polyolefin waterproof membrane as described above comprises the following components in parts by weight: 44 parts of polyolefin composite material, 15 parts of thermoplastic elastomer, 7 parts of nano-silicate filler, 8 parts of liquid crystal polymer, 1 part of inorganic nano-antibacterial agent, 8 parts of plasticizer, 3 parts of foaming agent, 2 parts of nucleating agent and 1.5 parts of crystallization accelerator.

[0010] A thermoplastic polyolefin waterproof coiled material as described above, wherein the inorganic nano antibacterial agent is one or more of nano silver and nano zinc oxide, the thermoplastic elastomer is a thermoplastic polyolefin elastomer formed by combining ethylene propylene rubber and polypropylene, the plasticizer is phthalate esters, the foaming agent is one of azodicarbonamide and sodium bicarbonate, the nucleating agent is one of sodium benzoate and talc, and the crystallization accelerator is one of sorbitol compounds and organic tin compounds.

[0011] The thermoplastic polyolefin waterproofing coiled material as described above, wherein the average particle size of the polyolefin composite material is 100-200 nanometers, the molecular weight distribution index of the thermoplastic elastomer is 2.0-2.5Mw / Mn, the particle ellipticity is 1.0-1.2, and the specific surface area of ​​the nano-silicate filler is 100-300m 2 / g, the order degree of the liquid crystal phase of the liquid crystal polymer is 90% to 99%, the average molecular weight is 100,000 to 200,000, the solubility parameter difference between the plasticizer and the polyolefin composite material is less than 1.0, and the mobility in the coil is less than 5%.

[0012] A thermoplastic polyolefin waterproofing coiled material as described above, wherein a low molecular weight polyolefin and a high molecular weight polyolefin are blended in the polyolefin composite material to form a microscopic phase separation structure, and the elastic modulus of the blend is set to E_{blend}, then;

[0013] E_{blend}=E_{low}\cdot\phi_{low}+E_{high}\cdot\phi_{high}+\DeltaE_{interface};

[0014] Wherein, E_{blend}: elastic modulus of the blend, representing the stiffness of the material; E_{low} and E_{high}: elastic modulus of low molecular weight polyolefin and high molecular weight polyolefin; \phi_{low} and \phi_{high}: volume fractions of low molecular weight polyolefin and high molecular weight polyolefin; \DeltaE_{interface}: contribution of interfacial energy change due to phase separation structure to the elastic modulus.

[0015] The second aspect of the present invention provides a preparation process of a thermoplastic polyolefin waterproof membrane, comprising the following steps:

[0016] S1: melting a low molecular weight polyolefin and a high molecular weight polyolefin respectively, melting the low molecular weight polyolefin and the high molecular weight polyolefin in different screw regions respectively, and then blending them through a twin-screw extruder. During the blending process, a uniform microscopic phase separation structure is formed by adjusting the screw speed and temperature to obtain a polyolefin composite material;

[0017] S2: heating the thermoplastic elastomer to a molten state, and then mixing it with the blended polyolefin composite material to obtain a matrix having both flexibility and strength;

[0018] S3: adding a foaming agent to the matrix, forming a uniform microporous structure by controlling the decomposition temperature and pressure of the foaming agent, adding a nucleating agent and a crystallization accelerator during the blending process, changing the microscopic crystalline structure of the material, and obtaining a blend;

[0019] S4: uniformly dispersing the nanosilicate filler in the blend;

[0020] S5: During the melt blending process, continue to add the liquid crystal polymer;

[0021] S6: adding an inorganic nano antibacterial agent to the molten blend to impart broad-spectrum antibacterial properties to the coil, and adding a plasticizer to improve the plasticity and processing properties of the coil;

[0022] S7: Extruding the above blend into sheets through an extruder, and then calendering, cooling, and cutting into required sizes to prepare the required thermoplastic polyolefin waterproof membrane.

[0023] As the preferred technical solution:

[0024] A preparation process of a thermoplastic polyolefin waterproof membrane as described above, in S1, a low molecular weight polyolefin and a high molecular weight polyolefin are melted separately, and the low molecular weight and high molecular weight polyolefins are melted in different screw areas respectively, the low molecular weight polyolefin melting temperature is: 160-180°C, the screw speed is: 100-200rpm, the high molecular weight polyolefin melting temperature is: 180-200°C, the screw speed is: 80-150rpm, and then blended by a twin-screw extruder, the blending temperature is 190-210°C, and the screw speed is 120-180rpm. During the blending process, a uniform microscopic phase separation structure is formed by adjusting the screw speed and temperature to obtain a polyolefin composite material.

[0025] As described above, a preparation process of a thermoplastic polyolefin waterproof membrane, in S3, a foaming agent is added to the matrix, the decomposition temperature of the foaming agent is controlled at 180-200°C, and the pressure is 10-20MPa to form a uniform microporous structure, a nucleating agent is added during the blending process, the blending temperature is 190-210°C, a crystallization promoter is added, and the blending time is 5-10 minutes to change the microscopic crystalline structure of the material to obtain a blend.

[0026] In the above-mentioned preparation process of a thermoplastic polyolefin waterproofing membrane, the thermoplastic elastomer is chemically modified to introduce linearly arranged functional side chains, so that the elastomer can enhance the compatibility with the polyolefin composite material while maintaining flexibility. The introduction rate of the functional side chain is set to I_R, then:

[0027] I_R=\frac{N_{functional}}{N_{total}}

[0028] Where, N_{functional}: the number of elastomer molecules with successfully introduced functional side chains; N_{total}: ​​the total number of elastomer molecules;

[0029] L_{chain}=\frac{\sum_{i=1}^{n}l_i\cdotN_i}{N_{functional}}

[0030] Wherein, L_{chain}: average side chain length; l_i: length of the i-th side chain; (N_i): number of elastomer molecules with the i-th side chain length; (N_{functional}): number of elastomer molecules with successfully introduced functional side chains;

[0031] L_{linearity}=\frac{L_{straight}}{L_{chain}}

[0032] Among them, L_{linearity}: linearity of the side chain; L_{straight}: length of the straight part of the side chain; L_{chain}: total length of the side chain.

[0033] As described above, in the preparation process of a thermoplastic polyolefin waterproof roll material, in S4, the nanosilicate filler is uniformly dispersed in the blend, the dispersion temperature is 180-200°C, and the dispersion time is 10-20 minutes. The size effect of the nanosilicate filler is utilized to more effectively fill the gaps in the polymer matrix, thereby enhancing the density and strength of the roll material; in S5, during the melt blending process, a liquid crystal polymer is added, the blending temperature is 200-220°C, and the blending time is 5-10 minutes. The self-assembly and orientation order of the liquid crystal polymer are utilized to improve the mechanical properties and weather resistance of the roll material.

[0034] Compared with the prior art, the present invention is composed of polyolefin composite material, thermoplastic elastomer, nano silicate filler, liquid crystal polymer, inorganic nano antibacterial agent, plasticizer, foaming agent, nucleating agent and crystallization accelerator. During the preparation process, each component is melted, blended, foamed, dispersed and extruded under precisely controlled temperature and process conditions to finally form a waterproof roll with excellent performance.

[0035] Beneficial effects:

[0036] Improved overall performance: The polyolefin composite material and thermoplastic elastomer in the coil form a uniform microscopic phase separation structure through blending technology. This structure not only retains the elasticity of rubber, but also increases the weldability of plastic, thereby greatly improving the overall performance of the coil.

[0037] Enhanced durability and weather resistance: The addition of liquid crystal polymers, through their self-assembly and oriented order, produces a synergistic effect with the polyolefin matrix, significantly improving the durability and weather resistance of the coil. This means that the coil can maintain a longer service life under extreme climate conditions.

[0038] Enhanced mechanical properties: The synergistic effect of nano-silicate fillers and polyolefin matrix effectively enhances the density and strength of the coil by filling the voids in the matrix. This enhancement effect is manifested as higher tensile strength and elongation in mechanical property tests, allowing the coil to withstand greater stress and deformation.

[0039] Synergistic improvement of antibacterial and hygienic properties: The addition of inorganic nano antibacterial agents forms a synergistic effect with the coil matrix, which not only gives the coil a broad-spectrum antibacterial property, but also effectively inhibits bacterial growth. This synergistic effect is crucial to improving the hygienic performance and service life of the coil, especially in a humid environment.

[0040] Coordinated optimization of processing performance and construction efficiency: By precisely controlling the ratio of each component and processing conditions, the coil exhibits good plasticity and processing performance. This not only facilitates on-site operation for construction personnel, but also greatly improves construction efficiency. At the same time, the excellent weldability of the coil also ensures the reliability of construction quality.

[0041] Coordinated realization of environmental protection and sustainability: Most of the materials used in the present invention are recyclable and reusable, which is consistent with the current development trend of green environmental protection. By optimizing the material formula and preparation process, it not only reduces environmental pollution, but also realizes the effective utilization and recycling of resources.

[0042] In summary, the present invention achieves significant improvements in comprehensive performance, durability, mechanical properties, antibacterial and hygienic properties, processing and construction efficiency, and environmental sustainability of the coiled material through the mutual coordination and enhancement of various components. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 It is a data line chart of the detection data 1 of the embodiment and the comparative example of the present invention;

[0044] Figure 2 It is a data line chart of the detection data 2 of the embodiment and the comparative example of the present invention;

[0045] Figure 3 It is a data line graph of the detection data 3 of the embodiment and the comparative example of the present invention;

[0046] Figure 4 It is a data line chart of detection data 4 of the embodiment and comparative example of the present invention. DETAILED DESCRIPTION

[0047] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs. In the event of a conflict, the definitions in the specification shall prevail. "When mass, concentration, temperature, time, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values ​​and lower preferred values, this should be understood to specifically disclose all ranges formed by any pairing of any upper range limit or preferred value with any lower range limit or preferred value, regardless of whether the range is disclosed separately. For example, a range of 1-50 should be understood to include 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60, 61, 62, 63, 64, 65, 66, 67, 68, 69, 70, 71, 72, 73, 74, 75, 76, 77, 78, 79, 80, 81, 82, 83, 84, 85, 86, 87, 88, 89, 90, 91 6, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, or 50, any number, combination of numbers, or subrange, and all decimal values ​​between the above integers, for example, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, and 1.9. With respect to subranges, "nested subranges" extending from any endpoint within the range are specifically contemplated. For example, nested subranges of the exemplary range 1-50 may include 1-10, 1-20, 1-30, and 1-40 in one direction, or 50-40, 50-30, 50-20, and 50-10 in the other direction."

[0048] The present invention is further explained below in conjunction with specific examples. The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are all commercially available unless otherwise specified.

[0049] A thermoplastic polyolefin waterproof coiled material comprises the following components in parts by weight: 40-50 parts of a polyolefin composite material, 10-20 parts of a thermoplastic elastomer, 5-10 parts of a nano-silicate filler, 5-10 parts of a liquid crystal high molecular polymer, 1-2 parts of an inorganic nano-antibacterial agent, 5-10 parts of a plasticizer, 2-5 parts of a foaming agent, 1-3 parts of a nucleating agent, and 0.5-2 parts of a crystallization accelerator.

[0050] The inorganic nano antibacterial agent is one or more of nano silver and nano zinc oxide, the thermoplastic elastomer is a thermoplastic polyolefin elastomer formed by combining ethylene propylene rubber and polypropylene, the plasticizer is phthalate esters, the foaming agent is one of azodicarbonamide and sodium bicarbonate, the nucleating agent is one of sodium benzoate and talc, and the crystallization accelerator is one of sorbitol compounds and organic tin compounds;

[0051] The average particle size of the polyolefin composite material is 100-200 nanometers, the molecular weight distribution index of the thermoplastic elastomer is 2.0-2.5Mw / Mn, the particle ellipticity is 1.0-1.2, and the specific surface area of ​​the nano-silicate filler is 100-300m 2 / g, the order of the liquid crystal phase of the liquid crystal polymer is 90% to 99%, the average molecular weight is 100,000-200,000, the difference in solubility parameters between the plasticizer and the polyolefin is less than 1.0, and the mobility in the coil is less than 5%;

[0052] In the polyolefin composite material, low molecular weight polyolefin and high molecular weight polyolefin are blended to form a microscopic phase separation structure, and the elastic modulus of the blend is set to E_{blend}, then;

[0053] E_{blend}=E_{low}\cdot\phi_{low}+E_{high}\cdot\phi_{high}+\DeltaE_{interface};

[0054] Wherein, E_{blend}: elastic modulus of the blend, representing the stiffness of the material; E_{low} and E_{high}: elastic modulus of low molecular weight polyolefin and high molecular weight polyolefin; \phi_{low} and \phi_{high}: volume fractions of low molecular weight polyolefin and high molecular weight polyolefin; \DeltaE_{interface}: contribution of interfacial energy change due to phase separation structure to the elastic modulus.

[0055] The polyolefin composite material is blended by low molecular weight polyolefin (e.g. polyethylene, elastic modulus E_{low}=100 MPa) and high molecular weight polyolefin (e.g. high molecular weight polyethylene, elastic modulus E_{high}=1000 MPa). The volume fraction of low molecular weight polyolefin is set to 0.6, and the volume fraction of high molecular weight polyolefin is set to 0.4.

[0056] The elastic modulus of the blend is calculated according to the formula E_{blend}=E_{low}\cdot\phi_{low}+E_{high}\cdot\phi_{high}+\DeltaE_{interface}. Here, the contribution of the interfacial energy change caused by the phase separation structure to the elastic modulus is set to \DeltaE_{interface}=50MPa.

[0057] Then the elastic modulus of the blend is E_{blend}=100MPa*0.6+1000MPa*0.4+50MPa=510MPa.

[0058] In addition, during the preparation process, attention should be paid to controlling the dispersion uniformity and compatibility of each component to ensure the performance stability of the coil. For example, a twin-screw extruder can be used for melt blending and the blending effect can be controlled by adjusting parameters such as screw speed and temperature; an appropriate amount of compatibilizer can also be added to improve the compatibility between the components.

[0059] Embodiment 1

[0060] A thermoplastic polyolefin waterproofing coiled material comprises the following components in parts by weight: 40 parts of a polyolefin composite material, 10 parts of a thermoplastic elastomer, 5 parts of a nano-silicate filler, 5 parts of a liquid crystal high molecular polymer, 1 part of an inorganic nano-antibacterial agent, 5 parts of a plasticizer, 2 parts of a foaming agent, 1 part of a nucleating agent, and 0.5 parts of a crystallization accelerator.

[0061] Among them, the inorganic nano-antibacterial agent is nano-zinc oxide (Shanghai Xiangtian Nanomaterials Co., Ltd.), the thermoplastic elastomer is Santoprene TPV series (DuPont), which is a thermoplastic polyolefin elastomer formed by the combination of ethylene propylene rubber and polypropylene, the plasticizer is dioctyl phthalate (Hengshui Jiali Lubricating Oil Co., Ltd.), the foaming agent is azodicarbonamide, the nucleating agent is sodium benzoate (Shenzhen Longdi Chemical Co., Ltd.), and the crystallization accelerator is sorbitol compounds.

[0062] The embodiment also provides a preparation process of a thermoplastic polyolefin waterproofing membrane, comprising the following steps:

[0063] S1: melt low molecular weight polyolefin (low molecular weight polyethylene (LMPE), molecular weight 3000Da) and high molecular weight polyolefin (high density polyethylene (HDPE), molecular weight 50,000Da) respectively, melt low molecular weight and high molecular weight polyolefin in different screw regions, melt temperature of low molecular weight polyolefin: 160°C, screw speed: 100rpm, melt temperature of high molecular weight polyolefin: 180°C, screw speed: 80rpm, then blend through a twin-screw extruder, blend temperature is 190°C, screw speed is 120rpm, during the blending process, a uniform microscopic phase separation structure is formed by adjusting the screw speed and temperature, and a polyolefin composite material is obtained;

[0064] S2: heating the thermoplastic elastomer to a molten state at a melting temperature of 150°C, and then mixing it with the blended polyolefin composite material at a mixing temperature of 170°C for 5 minutes to obtain a matrix having both flexibility and strength;

[0065] S3: In a screw extruder, a foaming agent is added to the matrix, the decomposition temperature of the foaming agent is controlled at 180°C, the pressure is controlled at 10MPa, a uniform microporous structure is formed, a nucleating agent is added during the blending process, the blending temperature is 190°C, a crystallization accelerator is added, the blending time is 5 minutes, the microscopic crystalline structure of the material is changed, and a blend is obtained;

[0066] S4: In a screw extruder, the nano-silicate filler is uniformly dispersed in the blend, the dispersion temperature is 180°C, and the dispersion time is 10 minutes. The size effect of the nano-silicate filler is utilized to more effectively fill the voids in the polymer matrix, thereby enhancing the density and strength of the coil;

[0067] S5: In a screw extruder, during the melt blending process, a liquid crystal polymer is added, the blending temperature is 200° C., and the blending time is 5 minutes, and the self-assembly and orientation order of the liquid crystal polymer are utilized to improve the mechanical properties and weather resistance of the coil;

[0068] S6: in a screw extruder, adding an inorganic nano antibacterial agent to the molten blend to impart broad-spectrum antibacterial properties to the coil, and adding a plasticizer to improve the plasticity and processing properties of the coil. The blending temperature at this time is 190° C., and the blending time is 5 minutes;

[0069] S7: The above blend is extruded into a sheet through an extruder, and then calendered and cooled, the extrusion temperature is 180°C, the calendering temperature is 160°C, the calendering speed is 5m / min, cooled to room temperature, the cooling rate is: 10°C / min, cut into the required size, and made into the required thermoplastic polyolefin waterproof membrane.

[0070] Embodiment 2

[0071] A thermoplastic polyolefin waterproofing coiled material comprises the following components in parts by weight: 43 parts of a polyolefin composite material, 14 parts of a thermoplastic elastomer, 6 parts of a nano-silicate filler, 7 parts of a liquid crystal high molecular polymer, 1 part of an inorganic nano-antibacterial agent, 6 parts of a plasticizer, 3 parts of a foaming agent, 2 parts of a nucleating agent, and 0.8 parts of a crystallization accelerator.

[0072] Among them, the inorganic nano-antibacterial agent is nanosilver (Beike Nano), the thermoplastic elastomer is a thermoplastic polyolefin elastomer formed by the combination of ethylene propylene rubber and polypropylene, the plasticizer is phthalate esters (Ji Ye Sheng), the foaming agent is azodicarbonamide (Sheng Bang), the nucleating agent is talcum powder (Haicheng Hetai Powder), and the crystallization accelerator is a sorbitol compound (sorbitol, Guangzhou Jie Yu Chemical Co., Ltd.).

[0073] The embodiment also provides a preparation process of a thermoplastic polyolefin waterproofing membrane, comprising the following steps:

[0074] S1: Melting low molecular weight polyolefin and high molecular weight polyolefin separately, the low molecular weight polyolefin and the high molecular weight polyolefin are melted in different screw regions, the melting temperature of low molecular weight polyolefin is 165°C, the screw speed is 120rpm, the melting temperature of high molecular weight polyolefin is 190°C, the screw speed is 110rpm, and then blending is carried out through a twin-screw extruder, the blending temperature is 195°C, and the screw speed is 130rpm. During the blending process, a uniform microscopic phase separation structure is formed by adjusting the screw speed and temperature to obtain a polyolefin composite material;

[0075] S2: heating the thermoplastic elastomer to a molten state at a melting temperature of 155°C, and then mixing it with the blended polyolefin composite material at a mixing temperature of 175°C for 6 minutes to obtain a matrix having both flexibility and strength;

[0076] S3: In a screw extruder, a foaming agent is added to the matrix, the decomposition temperature of the foaming agent is controlled at 190°C, the pressure is controlled at 13MPa, a uniform microporous structure is formed, a nucleating agent is added during the blending process, the blending temperature is 195°C, a crystallization accelerator is added, the blending time is 7 minutes, the microscopic crystalline structure of the material is changed, and a blend is obtained;

[0077] S4: In a screw extruder, the nano-silicate filler is uniformly dispersed in the blend at a dispersion temperature of 185°C and a dispersion time of 13 minutes. The size effect of the nano-silicate filler is utilized to more effectively fill the voids in the polymer matrix, thereby enhancing the compactness and strength of the coil.

[0078] S5: In a screw extruder, during the melt blending process, a liquid crystal polymer is added, the blending temperature is 210° C., and the blending time is 6 minutes, and the self-assembly and orientation order of the liquid crystal polymer are utilized to improve the mechanical properties and weather resistance of the coil;

[0079] S6: in a screw extruder, adding an inorganic nano antibacterial agent to the molten blend to impart broad-spectrum antibacterial properties to the coil, and adding a plasticizer to improve the plasticity and processing properties of the coil. At this time, the blending temperature is 195° C. and the blending time is 7 minutes;

[0080] S7: The above blend is extruded into a sheet through an extruder, and then calendered and cooled, with the extrusion temperature being 185°C, the calendering temperature being 165°C, and the calendering speed being 7m / min, and then cooled to room temperature, with a cooling rate of 13°C / min, and cut into the required size to make the required thermoplastic polyolefin waterproof membrane.

[0081] Embodiment 3

[0082] A thermoplastic polyolefin waterproofing coiled material comprises the following components in parts by weight: 48 parts of a polyolefin composite material, 17 parts of a thermoplastic elastomer, 9 parts of a nano-silicate filler, 8 parts of a liquid crystal high molecular polymer, 2 parts of an inorganic nano-antibacterial agent, 7 parts of a plasticizer, 4 parts of a foaming agent, 2 parts of a nucleating agent, and 1.5 parts of a crystallization accelerator.

[0083] Among them, the inorganic nano-antibacterial agent is nano-zinc oxide (Nanjing Baoket New Materials Co., Ltd.), the thermoplastic elastomer is a thermoplastic polyolefin elastomer formed by combining ethylene propylene rubber and polypropylene (DuPont), the plasticizer is phthalate (Ji Ye Sheng), the foaming agent is sodium bicarbonate (Jinan Xinweida Chemical Co., Ltd.), the nucleating agent is sodium benzoate (Shenzhen Longdi Chemical Co., Ltd.), and the crystallization promoter is an organic tin compound (dibutyl tin).

[0084] The embodiment also provides a preparation process of a thermoplastic polyolefin waterproof membrane, comprising the following steps:

[0085] S1: Melting low molecular weight polyolefin and high molecular weight polyolefin separately, the low molecular weight polyolefin and the high molecular weight polyolefin are melted in different screw regions, the melting temperature of low molecular weight polyolefin is 170°C, the screw speed is 170rpm, the melting temperature of high molecular weight polyolefin is 190°C, the screw speed is 130rpm, and then blending is carried out through a twin-screw extruder, the blending temperature is 200°C, and the screw speed is 160rpm. During the blending process, a uniform microscopic phase separation structure is formed by adjusting the screw speed and temperature to obtain a polyolefin composite material;

[0086] S2: heating the thermoplastic elastomer to a molten state at a melting temperature of 160°C, and then mixing it with the blended polyolefin composite material at a mixing temperature of 180°C for 8 minutes to obtain a matrix having both flexibility and strength;

[0087] S3: In a screw extruder, a foaming agent is added to the matrix, the decomposition temperature of the foaming agent is controlled at 190°C, the pressure is controlled at 18MPa, a uniform microporous structure is formed, a nucleating agent is added during the blending process, the blending temperature is 200°C, a crystallization accelerator is added, the blending time is 8 minutes, the microscopic crystalline structure of the material is changed, and a blend is obtained;

[0088] S4: In a screw extruder, the nano-silicate filler is uniformly dispersed in the blend at a dispersion temperature of 190°C and a dispersion time of 18 minutes. The size effect of the nano-silicate filler is utilized to more effectively fill the voids in the polymer matrix, thereby enhancing the compactness and strength of the coil.

[0089] S5: In a screw extruder, during the melt blending process, a liquid crystal polymer is added, the blending temperature is 210° C., and the blending time is 9 minutes, and the self-assembly and orientation order of the liquid crystal polymer are utilized to improve the mechanical properties and weather resistance of the coil;

[0090] S6: in a screw extruder, adding an inorganic nano antibacterial agent to the molten blend to impart broad-spectrum antibacterial properties to the coil, and adding a plasticizer to improve the plasticity and processing properties of the coil. The blending temperature at this time is 200° C., and the blending time is 9 minutes;

[0091] S7: The above blend is extruded into a sheet through an extruder, and then calendered and cooled, with the extrusion temperature being 190°C, the calendering temperature being 170°C, and the calendering speed being 8m / min, and then cooled to room temperature, with a cooling rate of 17°C / min, and cut into the required size to make the required thermoplastic polyolefin waterproof membrane.

[0092] Embodiment 4

[0093] A thermoplastic polyolefin waterproofing coiled material comprises the following components in parts by weight: 50 parts of a polyolefin composite material, 20 parts of a thermoplastic elastomer, 10 parts of a nano-silicate filler, 10 parts of a liquid crystal high molecular polymer, 2 parts of an inorganic nano-antibacterial agent, 10 parts of a plasticizer, 5 parts of a foaming agent, 3 parts of a nucleating agent, and 2 parts of a crystallization accelerator.

[0094] Among them, the inorganic nano antibacterial agent is nano zinc oxide, the thermoplastic elastomer is a thermoplastic polyolefin elastomer formed by combining ethylene propylene rubber and polypropylene, the plasticizer is phthalate, the foaming agent is azodicarbonamide, the nucleating agent is sodium benzoate, and the crystallization accelerator is a sorbitol compound.

[0095] The embodiment also provides a preparation process of a thermoplastic polyolefin waterproof membrane, comprising the following steps:

[0096] S1: Melting low molecular weight polyolefin and high molecular weight polyolefin separately, the low molecular weight polyolefin and the high molecular weight polyolefin are melted in different screw regions, the melting temperature of low molecular weight polyolefin is 180°C, the screw speed is 200rpm, the melting temperature of high molecular weight polyolefin is 200°C, the screw speed is 150rpm, and then blending is carried out through a twin-screw extruder, the blending temperature is 210°C, and the screw speed is 180rpm. During the blending process, a uniform microscopic phase separation structure is formed by adjusting the screw speed and temperature to obtain a polyolefin composite material;

[0097] S2: heating the thermoplastic elastomer to a molten state at a melting temperature of 170°C, and then mixing it with the blended polyolefin composite material at a mixing temperature of 190°C for 10 minutes to obtain a matrix having both flexibility and strength;

[0098] S3: In a screw extruder, a foaming agent is added to the matrix, the decomposition temperature of the foaming agent is controlled at 200°C, the pressure is controlled at 20MPa, a uniform microporous structure is formed, a nucleating agent is added during the blending process, the blending temperature is 210°C, a crystallization accelerator is added, the blending time is 10 minutes, the microscopic crystalline structure of the material is changed, and a blend is obtained;

[0099] S4: In a screw extruder, the nano-silicate filler is uniformly dispersed in the blend, the dispersion temperature is 200°C, and the dispersion time is 20 minutes. The size effect of the nano-silicate filler is utilized to more effectively fill the voids in the polymer matrix, thereby enhancing the density and strength of the coiled material.

[0100] S5: In a screw extruder, during the melt blending process, a liquid crystal polymer is added, the blending temperature is 220° C., and the blending time is 10 minutes, and the self-assembly and orientation order of the liquid crystal polymer are utilized to improve the mechanical properties and weather resistance of the coil;

[0101] S6: In a screw extruder, an inorganic nano antibacterial agent is added to the molten blend to impart broad-spectrum antibacterial properties to the coil, and a plasticizer is added to improve the plasticity and processing properties of the coil. The blending temperature at this time is 210° C. and the blending time is 10 minutes;

[0102] S7: The above blend is extruded into a sheet through an extruder, and then calendered and cooled, the extrusion temperature is 200°C, the calendering temperature is 180°C, the calendering speed is 10m / min, cooled to room temperature, the cooling rate is: 20°C / min, cut into the required size, and made into the required thermoplastic polyolefin waterproof membrane.

[0103] Embodiment 5

[0104] On the basis of Example 4, the thermoplastic elastomer is chemically modified to introduce linearly arranged functional side chains, so that the elastomer maintains flexibility while enhancing the compatibility with the polyolefin composite material. The introduction rate of the functional side chain is set to I_R, then:

[0105] I_R=\frac{N_{functional}}{N_{total}}

[0106] Where, N_{functional}: the number of elastomer molecules with successfully introduced functional side chains; N_{total}: ​​the total number of elastomer molecules;

[0107] L_{chain}=\frac{\sum_{i=1}^{n}l_i\cdotN_i}{N_{functional}}

[0108] Wherein, L_{chain}: average side chain length; l_i: length of the i-th side chain; (N_i): number of elastomer molecules with the i-th side chain length; (N_{functional}): number of elastomer molecules with successfully introduced functional side chains;

[0109] L_{linearity}=\frac{L_{straight}}{L_{chain}}

[0110] Among them, L_{linearity}: linearity of the side chain; L_{straight}: length of the straight part of the side chain; L_{chain}: total length of the side chain.

[0111] In the preparation method of the thermoplastic polyolefin waterproofing membrane, the chemical modification of the thermoplastic elastomer described above and the introduction of linearly arranged functional side chains can be specifically implemented as illustrated by the following examples:

[0112] Specifically, a thermoplastic elastomer (a thermoplastic polyolefin elastomer formed by combining ethylene-propylene rubber and polypropylene) is reacted with a modifier (such as maleic anhydride) in a molten state to introduce linearly arranged functional side chains.

[0113] During the modification process, the reaction temperature was controlled to be 190°C and the reaction time was 20 minutes to ensure that the modifier and the elastomer fully reacted. After the reaction was completed, a modified thermoplastic elastomer was obtained.

[0114] In order to evaluate the modification effect, we calculated the introduction rate of functional side chains I_R, the average side chain length L_{chain} and the linearity of the side chains L_{linearity}. The specific data are as follows:

[0115] Introduction rate I_R: The elastomers before and after modification were analyzed by nuclear magnetic resonance (NMR) to calculate the ratio of the number of elastomer molecules with successfully introduced functional side chains N_{functional} to the total number of elastomer molecules N_{total}, that is, I_R = 0.8 (indicating that 80% of the elastomer molecules have successfully introduced functional side chains).

[0116] Average side chain length L_{chain}: The molecular weight distribution of the modified elastomer is obtained by gel permeation chromatography (GPC) analysis, and the average side chain length L_{chain}=10 is calculated (indicating that each functional side chain contains 10 monomer units on average).

[0117] Linearity of side chain L_{linearity}: The morphology of the modified elastomer was observed by atomic force microscopy (AFM), and the ratio of the length of the straight part of the side chain L_{straight} to the total length of the side chain L_{chain} was measured, that is, L_{linearity} = 0.9 (indicating that 90% of the side chain is linearly arranged).

[0118] The modified thermoplastic elastomer is blended with the polyolefin composite material according to the steps in Example 4 to prepare a thermoplastic polyolefin waterproof roll. Since the modified elastomer has enhanced compatibility with the polyolefin composite material, the prepared roll has higher strength and weather resistance while maintaining flexibility.

[0119] Comparative Example 1

[0120] A thermoplastic polyolefin waterproofing membrane and a preparation process thereof are basically the same as those in Example 4, except that the nano-silicate filler is removed and the nano-silicate filler is not added in step S4.

[0121] Comparative Example 2

[0122] A thermoplastic polyolefin waterproofing membrane and a preparation process thereof are basically the same as those of the fourth embodiment, except that the thermoplastic elastomer is replaced with a common elastomer (natural rubber, China Petrochemical Rubber Co., Ltd.).

[0123] Comparative Example 3

[0124] A thermoplastic polyolefin waterproof membrane and a preparation process thereof are basically the same as those of Example 4, except that the microporous structure design step is omitted, no foaming agent is added in step S3, and no microporous structure design is performed.

[0125] Comparative Example 4

[0126] A thermoplastic polyolefin waterproofing coiled material and a preparation process thereof are basically the same as those in the fourth embodiment, except that the liquid crystal polymer is removed and the liquid crystal polymer is not added in the step S5.

[0127] The thermoplastic polyolefin waterproof membranes prepared in the above-mentioned Examples 1 to 4, Example 5, and Comparative Examples 1 to 4 were tested;

[0128] Tensile strength and elongation at break

[0129] National standard: GB / T 328.9-2007

[0130] Testing method: Cut dumbbell-shaped specimens according to the standard, perform tensile test on a tensile testing machine, and record the maximum force and elongation at break.

[0131] Heat resistance

[0132] National standard: Customized testing can be performed according to the method in GB / T 1731-1993 (Determination of heat resistance of paint films).

[0133] Testing method: Place the coil in a specified high temperature environment and observe changes in its performance, such as appearance, dimensional stability, etc.

[0134] Flexibility

[0135] National standard: It can be evaluated through bending test, such as the bending performance test method in GB / T 19816-2005.

[0136] Testing method: Bend the coil sample under specified conditions and observe whether it has cracks or damage.

[0137] Waterproof

[0138] National Standard: GB / T 17637-1998 (Dry sieve method for determination of effective pore size of geotextiles and related products) can be used to evaluate the waterproof performance of materials, or through customized water penetration tests.

[0139] Testing method: Use the hydrostatic pressure method or the hydrodynamic pressure method to test the water penetration resistance of the membrane.

[0140] The results are shown in Table 1:

[0141] Table 1

[0142]

[0143] Through the above Table 1, it can be determined directly that in Example 1 to Example 4; from Example 1 to Example 4, the tensile strength is gradually improved. Although the increase is not large each time, it generally shows a steady increase trend; all four examples have no significant changes at 120°C. This shows that in Example 1 to Example 4, the heat resistance of the material remains consistent, and it can remain stable at a high temperature of 120°C without significant performance changes, showing the good tolerance of the material in a high temperature environment; the flexibility of all four examples is that there is no crack at a bending radius of 5mm. In Example 1 to Example 4, the flexibility of the material remains unchanged, and no cracks appear when the bending radius is 5mm. The good performance of the material when subjected to bending force shows that it has good flexibility and crack resistance; all four examples can remain watertight for 24 hours under a hydrostatic pressure of 1.5MPa. In Example 1 to Example 4, the waterproof performance of the material is very stable and excellent, and can remain watertight for a long time under a high water pressure. This is a very important performance indicator of waterproof materials, showing the reliability of the materials in these examples in terms of waterproofing.

[0144] In summary, from Example 1 to Example 4, we can see that the material gradually improves in tensile strength, while maintaining consistent and excellent performance in heat resistance, flexibility and waterproof performance. This reflects the gradual optimization and improvement of material performance in these examples.

[0145] In Example 5, the tensile strength is increased to 17.8 MPa, while the tensile strength of Example 4 is 15.0 MPa. Compared with Example 4, the tensile strength is significantly improved by about 18.7% (from 15.0 MPa to 17.8 MPa). This improvement is attributed to the chemical modification of the thermoplastic elastomer in Example 5, especially the introduction of linearly arranged functional side chains, which enhances the interaction between the elastomer and the polyolefin composite material, thereby improving the overall tensile strength.

[0146] Heat resistance: Example 4 showed no significant change at 120°C. The deformation temperature of Example 5 was increased to 130°C. In terms of heat resistance, Example 5 also showed significant improvement compared to Example 4. The material in Example 5 began to deform at a higher temperature (130°C), which shows that the thermal stability of the material was enhanced by chemical modification. This improvement enables the material to maintain its performance in more demanding high-temperature environments.

[0147] Flexibility: The flexibility of Example 4 is 5 mm bending radius without cracks. The flexibility of Example 5 is improved to 4 mm bending radius without cracks. In terms of flexibility, Example 5 is improved compared with Example 4. The bending radius is reduced from 5 mm to 4 mm without cracks, indicating that the flexibility of the material has been enhanced. Although functional side chains are introduced, the optimized modification process does not sacrifice the flexibility of the material, but improves it.

[0148] Waterproof performance: Example 4 can remain watertight for 24 hours under a hydrostatic pressure of 1.5 MPa; Example 5 can remain watertight for 36 hours under the same hydrostatic pressure. In terms of waterproof performance, Example 5 has been significantly improved over Example 4. The time that the material in Example 5 can remain watertight under a hydrostatic pressure of 1.5 MPa is extended from 24 hours to 36 hours, which shows the superiority of the modified material in waterproof performance. This improvement is due to the fact that the modification enhances the compatibility between the elastomer and the polyolefin composite material, thereby improving the sealing and long-term waterproof ability of the coiled material.

[0149] Refer to the instruction manual Figure 1-4 , in Example 4 and Comparative Example 1, where other conditions are the same, the nanosilicate filler is removed from Comparative Example 1, and no nanosilicate filler is added in step S4. After testing, the tensile strength of the waterproof roll obtained is: Example 4: 15.0MPa; Comparative Example 1: 13.5MPa; the tensile strength of Example 4 is significantly higher than that of Comparative Example 1. Heat resistance: Example 4: no significant change at 120°C; Comparative Example 1: the temperature at which deformation begins is 110°C, and the material of Example 4 can still maintain its performance at a higher temperature, showing better heat resistance. Flexibility: Example 4: no cracks at a bending radius of 5mm; Comparative Example 1: no cracks at a bending radius of 6mm, and the material of Example 4 does not crack at a smaller bending radius, indicating that its flexibility is slightly better than that of Comparative Example 1. Waterproof performance: Both can remain watertight for 24 hours under a certain hydrostatic pressure, but the hydrostatic pressure bearing capacity of Example 4 (1.5MPa) is slightly higher than that of Comparative Example 1 (1.4MPa). The absence of nanosilicate fillers results in a decrease in the mechanical properties and thermal stability of the coil, as nanosilicates can enhance the density and strength of the material.

[0150] In comparative example 2, the thermoplastic elastomer was replaced by an ordinary elastomer. After testing, the final waterproof roll obtained had a tensile strength: the tensile strength of Example 4 was similar to that of Comparative Example 2 (15.0MPa and 14.8MPa), indicating that the two were equivalent in tensile properties. Heat resistance: The initial deformation temperature of Comparative Example 2 was 118°C, slightly lower than 120°C of Example 4, indicating that the heat resistance of Example 4 was slightly better. Flexibility: The bending radius of Comparative Example 2 was 10mm, much larger than 5mm of Example 4, indicating that the material flexibility of Example 4 was significantly better than that of Comparative Example 2. Waterproof performance: The two performed similarly in waterproof performance, and both could remain watertight for 24 hours under a hydrostatic pressure of 1.5MPa. The use of ordinary elastomers to replace thermoplastic elastomers with self-healing properties resulted in a decrease in the flexibility and self-healing ability of the roll.

[0151] In comparative example three, the microporous structure design step is omitted, and no foaming agent is added in step S3, and no microporous structure design is performed. After testing, the tensile strength of the waterproof membrane finally obtained is: the tensile strength of comparative example three is slightly higher than that of example four (15.1MPa and 15.0MPa), but the difference is small. Example four and comparative example three have similar performances in heat resistance, and both can remain stable at 120°C. Flexibility: The two perform equally well in flexibility, and the bending radius is 5mm without cracks. Waterproof performance: Comparative example three can remain watertight for 24 hours under a lower hydrostatic pressure (1.1MPa), while example four can withstand a higher hydrostatic pressure (1.5MPa), indicating that example four is superior in waterproof performance. Microporous structure design can increase the specific surface area of ​​the material, improve waterproof performance and adsorption capacity. After omitting this step, these properties are significantly reduced.

[0152] In comparative example 4, the liquid crystal polymer was removed, and no liquid crystal polymer was added in step S5. After testing, the tensile strength of the waterproof roll obtained in Example 4 was significantly higher than that of the comparative example 4 (15.0MPa and 13.8MPa), and the initial deformation temperature of Example 4 was higher than that of the comparative example 4 (120°C and 116°C), showing better heat resistance; the two were comparable in flexibility, with a bending radius of 5mm without cracks; in terms of waterproof performance, both could remain watertight for 24 hours under a hydrostatic pressure of 1.5MPa, with similar performance. The lack of liquid crystal polymer leads to a decrease in the orderliness of the internal structure of the roll, thereby affecting its mechanical properties and weather resistance.

[0153] In summary, through comparative analysis, it can be seen that Example 4 shows certain advantages over Comparative Examples 1 to 4 in many aspects (especially tensile strength and heat resistance). These advantages are derived from the material formulation or treatment process in Example 4. At the same time, the comparative examples also show differences in certain specific properties, providing a reference for further optimizing material properties.

[0154] The present invention develops a new type of blended material by introducing polyolefins of different molecular weights. While maintaining flexibility, the heat resistance is improved. The specific method is to blend low molecular weight polyolefins with high molecular weight polyolefins to form a microscopic phase separation structure, thereby achieving performance optimization.

[0155] And use polymer materials with self-healing properties, such as thermoplastic elastomers; adopt microporous structure design to increase the specific surface area of ​​the material, improve its waterproof performance and adsorption capacity. Nanosilicate fillers can enhance the mechanical properties and thermal stability of the coiled material. Due to the size effect of nanomaterials, they can more effectively fill the tiny gaps in the polymer matrix, thereby improving the density and strength of the material.

[0156] Liquid crystal polymers have the characteristics of self-assembly and orderly orientation. Adding them to TPO can enhance the orderliness of the internal structure of the coil, thereby improving its mechanical properties and weather resistance.

[0157] Inorganic nano-antimicrobial agents such as nano-silver and nano-zinc oxide have broad-spectrum antimicrobial properties and are highly safe. Adding them to TPO membranes can give them antimicrobial properties, making them suitable for waterproofing projects with high hygiene requirements, such as hospitals and food processing plants.

[0158] The present invention achieves significant improvement in coil performance by precisely controlling the proportion of each component and optimizing the preparation process;

[0159] By adjusting the weight proportions of polyolefin composites, thermoplastic elastomers, nano-silicate fillers, liquid crystal polymers, inorganic nano-antibacterial agents, plasticizers, foaming agents, nucleating agents and crystallization accelerators, a balance of different performance requirements is achieved. In particular, the chemical modification of thermoplastic elastomers significantly enhances the compatibility of elastomers and polyolefin composites by introducing linearly arranged functional side chains.

[0160] The complete preparation process from raw material melting, blending, mixing, foaming, filler dispersion, liquid crystal polymer and antibacterial agent addition to final extrusion, calendering, cooling and molding. The uniformity of the coil microstructure and the stability of its performance are ensured by precisely controlling the temperature, time, pressure and other parameters of each step.

[0161] By optimizing the components and processes, the prepared TPO waterproof membrane has excellent performance in tensile strength, heat resistance, flexibility, waterproof performance and weather resistance. In particular, the introduction of functional side chains through chemical modification further improves the strength and weather resistance of the membrane.

[0162] By precisely controlling the proportion of components and the preparation process, the performance of the membrane is balanced and improved to meet the diverse needs of different application scenarios. The compatibility of the modified thermoplastic elastomer with polyolefin composites is significantly enhanced, which helps to form a more stable microstructure, thereby improving the overall performance of the membrane. The introduction of functional side chains not only maintains the flexibility of the membrane, but also significantly improves its strength and weather resistance, extending the service life of the membrane. The addition of inorganic nano-antibacterial agents gives the membrane broad-spectrum antibacterial properties, which is particularly suitable for waterproofing engineering scenarios with high hygiene requirements, such as hospitals, food processing plants, etc. The excellent performance makes this TPO waterproof membrane have broad application prospects in many fields such as roof waterproofing, basement waterproofing, and tunnel waterproofing.

[0163] In summary, the present invention prepares a thermoplastic polyolefin waterproof membrane with excellent performance, environmental protection and sustainability through component optimization and process innovation, providing a new solution for the field of waterproof engineering.

[0164] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A thermoplastic polyolefin waterproofing membrane, characterized in that: The invention comprises the following components in parts by weight: 40-50 parts of polyolefin composite material, 10-20 parts of thermoplastic elastomer, 5-10 parts of nano silicate filler, 5-10 parts of liquid crystal high molecular polymer, 1-2 parts of inorganic nano antibacterial agent, 5-10 parts of plasticizer, 2-5 parts of foaming agent, 1-3 parts of nucleating agent and 0.5-2 parts of crystallization accelerator.

2. A thermoplastic polyolefin waterproofing membrane according to claim 1, characterized in that: The invention comprises the following components in parts by weight: 44 parts of polyolefin composite material, 15 parts of thermoplastic elastomer, 7 parts of nano-silicate filler, 8 parts of liquid crystal high molecular polymer, 1 part of inorganic nano-antibacterial agent, 8 parts of plasticizer, 3 parts of foaming agent, 2 parts of nucleating agent and 1.5 parts of crystallization accelerator.

3. A thermoplastic polyolefin waterproofing membrane according to claim 1 or 2, characterized in that: The inorganic nano antibacterial agent is one or more of nano silver and nano zinc oxide, the thermoplastic elastomer is a thermoplastic polyolefin elastomer formed by combining ethylene propylene rubber and polypropylene, the plasticizer is phthalate esters, the foaming agent is one of azodicarbonamide and sodium bicarbonate, the nucleating agent is one of sodium benzoate and talc, and the crystallization accelerator is one of sorbitol compounds and organic tin compounds.

4. The thermoplastic polyolefin waterproofing membrane according to claim 1, characterized in that: The average particle size of the polyolefin composite material is 100-200 nanometers, the molecular weight distribution index of the thermoplastic elastomer is 2.0-2.5Mw / Mn, the particle ellipticity is 1.0-1.2, and the specific surface area of ​​the nano-silicate filler is 100-300m 2 / g, the order degree of the liquid crystal phase of the liquid crystal polymer is 90% to 99%, the average molecular weight is 100,000 to 200,000, the solubility parameter difference between the plasticizer and the polyolefin composite material is less than 1.0, and the mobility in the coil is less than 5%.

5. The thermoplastic polyolefin waterproofing membrane according to claim 1, characterized in that: In the polyolefin composite material, a low molecular weight polyolefin and a high molecular weight polyolefin are blended to form a microscopic phase separation structure, and the elastic modulus of the blend is set to E_{blend}, then; E_{blend}=E_{low}\cdot\phi_{low}+E_{high}\cdot\phi_{hig h}+\DeltaE_{interface}; Wherein, E_{blend}: elastic modulus of the blend, representing the stiffness of the material; E_{low} and E_{high}: elastic modulus of low molecular weight polyolefin and high molecular weight polyolefin; \phi_{low} and \phi_{high}: volume fractions of low molecular weight polyolefin and high molecular weight polyolefin; \DeltaE_{interface}: contribution of interfacial energy change due to phase separation structure to the elastic modulus.

6. A process for preparing the thermoplastic polyolefin waterproofing membrane according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1: melting a low molecular weight polyolefin and a high molecular weight polyolefin respectively, melting the low molecular weight polyolefin and the high molecular weight polyolefin in different screw regions respectively, and then blending them through a twin-screw extruder. During the blending process, a uniform microscopic phase separation structure is formed by adjusting the screw speed and temperature to obtain a polyolefin composite material; S2: heating the thermoplastic elastomer to a molten state, and then mixing it with the blended polyolefin composite material to obtain a matrix having both flexibility and strength; S3: adding a foaming agent to the matrix, forming a uniform microporous structure by controlling the decomposition temperature and pressure of the foaming agent, adding a nucleating agent and a crystallization accelerator during the blending process, changing the microscopic crystalline structure of the material, and obtaining a blend; S4: uniformly dispersing the nanosilicate filler in the blend; S5: During the melt blending process, continue to add the liquid crystal polymer; S6: adding an inorganic nano antibacterial agent to the molten blend to impart broad-spectrum antibacterial properties to the coil, and adding a plasticizer to improve the plasticity and processing properties of the coil; S7: Extruding the above blend into sheets through an extruder, and then calendering, cooling, and cutting into required sizes to prepare the required thermoplastic polyolefin waterproof membrane.

7. A process for preparing a thermoplastic polyolefin waterproof membrane according to claim 6, wherein in S1, a low molecular weight polyolefin and a high molecular weight polyolefin are melted separately, and the low molecular weight and high molecular weight polyolefins are melted in different screw regions, respectively, the low molecular weight polyolefin melting temperature is 160-180°C, the screw speed is 100-200rpm, the high molecular weight polyolefin melting temperature is 180-200°C, the screw speed is 80-150rpm, and then the mixture is blended by a twin-screw extruder, the blending temperature is 190-210°C, and the screw speed is 120-180rpm. During the blending process, a uniform microscopic phase separation structure is formed by adjusting the screw speed and temperature to obtain a polyolefin composite material.

8. According to the preparation process of a thermoplastic polyolefin waterproof membrane according to claim 6, in S3, a foaming agent is added to the matrix, the decomposition temperature of the foaming agent is controlled at 180-200°C, and the pressure is 10-20MPa to form a uniform microporous structure, a nucleating agent is added during the blending process, the blending temperature is 190-210°C, a crystallization promoter is added, and the blending time is 5-10 minutes to change the microscopic crystalline structure of the material to obtain a blend.

9. The process for preparing a thermoplastic polyolefin waterproofing membrane according to claim 6, characterized in that: The thermoplastic elastomer is chemically modified to introduce linearly arranged functional side chains, so that the elastomer maintains flexibility while enhancing compatibility with the polyolefin composite material. The introduction rate of the functional side chains is set to I_R, then: I_R=\frac{N_{functional}}{N_{total}} Where, N_{functional}: the number of elastomer molecules with successfully introduced functional side chains; N_{total}: ​​the total number of elastomer molecules; L_{chain}=\frac{\sum_{i=1}^{n}l_i\cdotN_i}{N_{functiona l}} Wherein, L_{chain}: average side chain length; l_i: length of the i-th side chain; (N_i): number of elastomer molecules with the i-th side chain length; (N_{functional}): number of elastomer molecules with successfully introduced functional side chains; L_{linearity}=\frac{L_{straight}}{L_{chain}} Among them, L_{linearity}: linearity of the side chain; L_{straight}: length of the straight part of the side chain; L_{chain}: total length of the side chain.

10. The process for preparing a thermoplastic polyolefin waterproofing membrane according to claim 6, characterized in that: In the S4, the nano-silicate filler is uniformly dispersed in the blend, the dispersion temperature is 180-200° C., and the dispersion time is 10-20 minutes. The size effect of the nano-silicate filler is utilized to more effectively fill the gaps in the polymer matrix, thereby enhancing the density and strength of the coil. In the S5, during the melt blending process, a liquid crystal polymer is added, the blending temperature is 200-220° C., and the blending time is 5-10 minutes. The self-assembly and orientation order of the liquid crystal polymer are utilized to improve the mechanical properties and weather resistance of the coil.

Citation Information

Patent Citations

  • Polymer composites of thermoplastic and liquid crystal polymers and process for their preparation

    CN1067913A

  • Exposed resin polymer waterproof coiled material and preparation method thereof

    CN108467533A

  • Composite elastomer modified thermoplastic polyolefin waterproof coiled material and preparation method thereof

    CN115975298A

  • Ethylene polymer blends and process for forming film

    US4547551A