Method for separating and recovering molybdenum and nickel from molybdenum-nickel ore
Through the joint treatment of molybdenum-nickel ore with calcifying agent and potassium carbonate, the problems of difficult separation of molybdenum and nickel and environmental pollution in black rock series nickel-molybdenum ore are solved, and efficient molybdenum and nickel recovery and low-cost production are achieved.
Patent Information
- Application Number
- CN202410960194.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing technology has problems such as SO2 flue gas pollution, high consumption of alkali reagents, low molybdenum leaching rate and difficulty in subsequent purification when processing black rock series nickel-molybdenum ores. In addition, the large amount of sulfuric acid added is highly corrosive to equipment, making it difficult to effectively separate and recover molybdenum. ,nickel.
Molybdenum nickel ore is mixed and roasted with calcifying agent to form calcified molybdenum calcined sand, which is then mixed with carbonate to granulate, and then roasted for the second time. After crushing and grinding, it is leached with water, and a pure molybdenum acid solution is obtained by purifying and removing impurities. And low matte nickel products are obtained through reduction smelting, and potassium carbonate is used to convert calcium molybdate into soluble potassium molybdate to avoid the use of acid and alkali reagents.
It achieves efficient separation and recovery of nickel and molybdenum, reduces SO2 gas emissions, reduces production costs, avoids equipment corrosion, and improves molybdenum leaching rate and recovery rate.
Smart Images

Figure SMS_3
Abstract
Description
Technical Field
[0001] The present application relates to the field of nonferrous metal smelting, and in particular to a method for separating and recovering molybdenum and nickel from molybdenum-nickel ore. Background Art
[0002] Molybdenum is a nonferrous metal with high melting point and high boiling point. It is widely used in defense industry, metallurgy, chemical industry, mechanical electronics, new materials and other fields due to its good thermal and electrical conductivity, corrosion resistance and small expansion coefficient. It is one of the strategic nonferrous metals in short supply in China. Nickel is an important raw material in the battery industry. With the promotion and application of "high nickel batteries", its demand is increasing rapidly. With the rapid development of my country's national economy, molybdenum and nickel resources have been widely mined and utilized, resulting in insufficient supply. The black rock nickel-molybdenum ore is a complex mineral resource unique to my country. The content of nickel and molybdenum is 0.17%-7.03% and 0.35%-8.17% respectively. The proven reserves are 9.37 million tons, which has huge development and utilization value.
[0003] Black rock molybdenum-nickel ore is a black polymetallic sedimentary shale rich in nickel and molybdenum. The primary ore has a high organic carbon content, low molybdenum-nickel grade, and a close mineral mosaic relationship. Nickel ore, molybdenum ore, pyrite and other mineral phases are mutually encapsulated and embedded, making it difficult to separate and enrich the valuable components using existing physical or chemical beneficiation technologies. So far, there has been no major technological breakthrough. Therefore, direct smelting is the main way to process this ore at this stage.
[0004] The industrial development and utilization of nickel-molybdenum ore began in the 1980s, and the main treatment method has developed from pure pyrometallurgical process to pyrometallurgical-hydrometallurgical combined process. At present, the main treatment process of nickel-molybdenum ore in production is oxidative roasting-normal pressure / pressure alkaline leaching process to extract molybdenum. The process is simple and molybdenum and nickel are effectively separated, but there are problems such as SO2 flue gas pollution of the environment, large consumption of alkaline reagents, low molybdenum leaching rate, and difficulty in subsequent purification. The patented technology of "A method for preparing sodium molybdate using nickel-molybdenum ore" (CN103952543A) adopts oxidative roasting desulfurization-sodium roasting-water leaching of molybdenum-purification and impurity removal-concentration and crystallization to prepare sodium molybdate products. This method can effectively separate nickel and molybdenum and extract molybdenum from nickel-molybdenum ore, but the oxidative roasting temperature is 600~800℃, the sodium roasting temperature is 550~750℃, and the time is 3~6 hours. The energy consumption is large, and SO2 flue gas pollutes the environment. The patented technology of "A process for simultaneously extracting nickel and molybdenum from nickel-molybdenum ore" (CN104232935A) uses nickel-molybdenum ore plus calcium oxidation roasting-low-temperature sulfuric acid roasting-water leaching process to simultaneously extract molybdenum and nickel. This method has high molybdenum and nickel leaching rates and can effectively reduce the pollution caused by SO2 flue gas to the environment, but the amount of sulfuric acid added is 75%~100%, the acid consumption is large and the equipment is corrosive. Summary of the invention
[0005] The purpose of this application is to provide a method for separating and recovering molybdenum and nickel from molybdenum-nickel ore to solve the above problems.
[0006] To achieve the above objectives, the present application provides a method for separating and recovering molybdenum and nickel from molybdenum-nickel ore, comprising: Mixing molybdenum-nickel ore and a calcifying agent, and first roasting to obtain calcified molybdenum roasted sand; The calcified molybdenum roasted sand and carbonate are mixed and granulated to obtain green balls; The green balls are subjected to a second roasting to obtain roasted balls, and the roasted balls are crushed and ground to obtain roasted clinker; The roasted clinker is mixed with water for leaching, and a leaching solution and a leaching residue are obtained after solid-liquid separation; The leachate is purified and impurity-removed to obtain a pure molybdic acid solution; The leached slag is subjected to reduction smelting to obtain a low-grade nickel matte product; The carbonate includes potassium carbonate.
[0007] Optionally, the calcifying agent includes one or more of slaked lime, quicklime and limestone.
[0008] Optionally, the amount of the calcifying agent used is 1 to 3 times the theoretical amount calculated based on the sulfur content.
[0009] Optionally, the first calcination temperature is 400° C.-600° C., and the calcination time is 1 h-3 h.
[0010] Optionally, the mass ratio of the carbonate to the calcified molybdenum roasted sand is (0.2-1.5):1.
[0011] Optionally, the second calcination temperature is 150° C.-300° C., and the calcination time is 1 h-3 h.
[0012] Optionally, the leaching includes leaching at normal pressure, and the solid-liquid ratio of the leaching at normal pressure is (0.1 kg -0.5 kg):1L.
[0013] Optionally, the temperature of the atmospheric pressure leaching is 30°C-90°C, and the stirring time is 1 h-3 h.
[0014] Optionally, the finely ground particle size is 50 mesh-300 mesh.
[0015] Optionally, the molybdenum content of the molybdenum-nickel ore is 2%-10%, and the nickel content is 2%-10%.
[0016] Compared with the prior art, the beneficial effects of this application include: The method for separating and recovering molybdenum and nickel from molybdenum-nickel ore provided in the present application comprises adding a calcifying agent to fix sulfur, wherein S is fixed in roasted sand in the form of CaSO4, thereby preventing SO2 gas emission and helping to reduce environmental pollution, and MoS2 is converted into CaMoO4 under the action of the calcifying agent; potassium carbonate and calcified molybdenum roasted sand are mixed and granulated and then roasted, and CaMoO4 is selectively converted into soluble K2MoO4 under the action of potassium carbonate, and the roasted material can be directly leached in water, and the nickel is preserved in the leached residue, thereby achieving efficient separation of nickel and molybdenum; the leaching process does not consume acid and alkali reagents, the equipment corrosion pressure is small, and the production cost is reduced. DETAILED DESCRIPTION
[0017] As used herein: "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0018] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.
[0019] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values and all integers and fractions within the range.
[0020] In these examples, parts and percentages are by mass unless otherwise indicated.
[0021] "Mass parts" refers to the basic unit of measurement for expressing the mass ratio of multiple components. 1 part can represent any unit mass, such as 1g or 2.689g. If we say that the mass parts of component A are a parts and the mass parts of component B are b parts, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass parts of all components is not limited to 100 parts.
[0022] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).
[0023] The present application provides a method for separating and recovering molybdenum and nickel from molybdenum-nickel ore, comprising: Mixing molybdenum-nickel ore and a calcifying agent, and first roasting to obtain calcified molybdenum roasted sand; The calcified molybdenum roasted sand and carbonate are mixed and granulated to obtain green balls; The green balls are subjected to a second roasting to obtain roasted balls, and the roasted balls are crushed and ground to obtain roasted clinker; The roasted clinker is mixed with water for leaching, and a leaching solution and a leaching residue are obtained after solid-liquid separation; The leachate is purified and impurity-removed to obtain a pure molybdic acid solution; The leached slag is subjected to reduction smelting to obtain a low-grade nickel matte product; The carbonate includes potassium carbonate.
[0024] In some embodiments, the calcifying agent includes one or more of slaked lime, quicklime, and limestone.
[0025] In some embodiments, the amount of the calcifying agent used is 1 to 3 times the theoretical amount calculated based on the sulfur content.
[0026] Optionally, the dosage of the calcifying agent is 1 times, 1.5 times, 2 times, 2.5 times, 3 times or any value between 1 times and 3 times the theoretical amount calculated based on the sulfur content.
[0027] In some embodiments, the first calcination temperature is 400° C.-600° C., and the calcination time is 1 h-3 h.
[0028] Optionally, the temperature of the first calcination may be 400°C, 450°C, 500°C, 550°C, 600°C or any value between 400°C and 600°C, and the calcination time may be 1h, 1.5h, 2h, 2.5h, 3h or any value between 1h and 3h.
[0029] It should be noted that when the temperature of the first roasting is 400°C-600°C and the roasting time is 1h-3h, the obtained calcified molybdenum roasted sand has a sulfur fixation effect of more than 92% and a molybdenum conversion rate of more than 95%.
[0030] In some embodiments, the mass ratio of the carbonate to the calcified molybdenum roasted sand is (0.2-1.5):1.
[0031] Optionally, the mass ratio of carbonate to calcified molybdenum roasted sand can be 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1 or any value between (0.2-1.5):1.
[0032] In some embodiments, the second calcination temperature is 150° C.-300° C., and the calcination time is 1 h-3 h.
[0033] Optionally, the temperature of the second calcination can be 150°C, 160°C, 180°C, 200°C, 220°C, 240°C, 260°C, 280°C, 300°C or any value between 150°C and 300°C, and the calcination time can be 1h, 1.5h, 2h, 2.5h, 3h or any value between 1h and 3h.
[0034] It should be noted that potassium carbonate is used for the second calcination in this application, and its calcination temperature is much lower than that of sodium carbonate. This is because the temperature required for the calcium molybdate conversion reaction under the participation of potassium carbonate is lower than that of sodium carbonate. θ (Unit: KJ) (obtained from HSC Chemistry6.0) as shown in Table 1.
[0035] (1); (2); Table 1 Chemical reaction equations for molybdenum conversion and corresponding standard Gibbs free energy
[0036] In some embodiments, the leaching includes normal pressure leaching, and the solid-liquid ratio of the normal pressure leaching is (0.1kg-0.5kg):1L.
[0037] Optionally, the solid-liquid ratio of atmospheric pressure leaching can be 0.1kg:1L, 0.2kg:1L, 0.3kg:1L, 0.4kg:1L, 0.5kg:1L or any value between (0.1kg-0.5kg):1L.
[0038] It should be noted that the present application uses water for atmospheric pressure leaching, and the colloidal molybdenum sulfide (MoS2) in the raw ore is converted into water-soluble potassium molybdate (K2MoO4) through two-stage roasting, which can be directly leached by water leaching.
[0039] In some embodiments, the temperature of the atmospheric pressure leaching is 30°C-90°C, and the stirring time is 1h-3h.
[0040] Optionally, the temperature of atmospheric pressure leaching can be 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C or any value between 30°C and 90°C, and the stirring time can be 1h, 1.5h, 2h, 2.5h, 3h or any value between 1h and 3h.
[0041] In some embodiments, the finely ground particle size is 50 mesh to 300 mesh.
[0042] Optionally, the ground particle size can be 50 mesh, 100 mesh, 150 mesh, 200 mesh, 250 mesh, 300 mesh or any value between 50 mesh and 300 mesh.
[0043] In some embodiments, the molybdenum content of the molybdenum-nickel ore is 2%-10%, and the nickel content is 2%-10%.
[0044] Optionally, the molybdenum content in the molybdenum-nickel ore can be 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% or any value between 2% and 10%, and the nickel content can be 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10% or any value between 2% and 10%.
[0045] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0046] Example 1 This embodiment provides a method for separating and recovering molybdenum and nickel from molybdenum-nickel ore, comprising: 30g of nickel-molybdenum ore and 20g of calcifying agent slaked lime, quicklime and limestone were mixed, and roasted at a temperature of 500°C for 2.5h to obtain calcified molybdenum roasted sand; 20g of potassium carbonate and calcium molybdenum roasted sand were mixed evenly, and then 10% of water was sprayed into the mixture and placed in a granulator to obtain green balls. The mass ratio of carbonate to calcium molybdenum roasted sand was 1.5:1. The green balls were roasted at 200°C for 2.0h, and then ground into powder to obtain roasted clinker. Add water to the roasted clinker at a solid-liquid ratio of 0.2kg / L:1, and stir at 90°C for 2.5h to separate the solid and liquid to obtain molybdenum-rich leaching solution and nickel-containing leaching residue; The leachate is purified and impurities are removed, and a potassium sulfide solution is used to precipitate heavy metal cation impurities in the leachate; then barium hydroxide is added to generate barium sulfate precipitation to remove sulfate in the potassium molybdate solution; then an ammonium magnesium salt precipitation method is used to remove phosphate to obtain a pure potassium molybdate solution; The leached slag is subjected to reduction smelting at a smelting temperature of 1550°C for 3 hours to obtain a low-grade nickel matte product; The molybdenum recovery rate obtained in this embodiment is 95.2%.
[0047] Example 2 This embodiment provides a method for separating and recovering molybdenum and nickel from molybdenum-nickel ore, comprising: 30g of nickel-molybdenum ore and 20g of calcifying agent slaked lime, quicklime and limestone were mixed, and roasted at a temperature of 500°C for 2.5h to obtain calcified molybdenum roasted sand; 30g of potassium carbonate and calcium molybdenum roasted sand were mixed evenly, and then 10% of water was sprayed into the mixture and placed in a granulator to obtain green balls. The mass ratio of carbonate to calcium molybdenum roasted sand was 1.0:1. The green balls were roasted at 250°C for 3h and then ground into powder to obtain roasted clinker. Water was added to the roasted clinker at a solid-liquid ratio of 0.2kg / L:1, and then stirred at 80°C for 1h to separate the solid and liquid to obtain molybdenum-rich leaching solution and nickel-containing leaching residue; The leaching solution is purified and impurities removed to obtain a pure molybdic acid solution; The leached slag is subjected to reduction smelting to obtain a low-grade nickel matte product; The molybdenum recovery rate obtained in this embodiment is 96.6%.
[0048] Example 3 This embodiment provides a method for separating and recovering molybdenum and nickel from molybdenum-nickel ore, comprising: 50g of nickel-molybdenum ore and 50g of calcifying agent slaked lime, quicklime and limestone were mixed, and roasted at a temperature of 600°C for 2h to obtain calcified molybdenum roasted sand; 50g of potassium carbonate and calcium molybdenum roasted sand were mixed evenly, and then 10% of water was sprayed into the mixture and placed in a granulator to obtain green balls. The mass ratio of carbonate to calcium molybdenum roasted sand was 0.8:1. The green balls were roasted at 250°C for 1.5h, and then ground into powder to obtain roasted clinker. Add water to the roasted clinker at a solid-liquid ratio of 0.1kg / L:1, stir at 50°C for 1h, separate the solid and liquid, and obtain molybdenum-rich leaching solution and nickel-containing leaching residue; The leaching solution is purified and impurities removed to obtain a pure molybdic acid solution; The leached slag is subjected to reduction smelting to obtain a low-grade nickel matte product; The molybdenum recovery rate obtained in this embodiment is 96.1%.
[0049] Comparative Example 1 This comparative example provides a method for separating and recovering molybdenum and nickel from molybdenum-nickel ore. The difference from Example 1 is that a calcifying agent and potassium carbonate are mixed with the nickel-molybdenum ore at the same time, and other conditions are consistent with Example 1.
[0050] The molybdenum recovery rate obtained in this embodiment is 46.5%.
[0051] Comparative Example 2 This comparative example provides a method for separating and recovering molybdenum and nickel from molybdenum-nickel ore. The difference from Example 1 is that the carbonate in this comparative example is sodium carbonate, and other conditions are consistent with Example 1.
[0052] The platinum recovery rate obtained in this embodiment is 0%.
[0053] Comparative Example 3 This comparative example provides a method for separating and recovering molybdenum and nickel from molybdenum-nickel ore. The difference from Example 1 is that the carbonate in this comparative example is sodium carbonate, the roasting temperature is 600°C, and the other conditions are consistent with Example 1.
[0054] The platinum recovery rate obtained in this embodiment is 0%.
[0055] Comparative Example 4 This comparative example provides a method for separating and recovering molybdenum and nickel from molybdenum-nickel ore. The difference from Example 1 is that no calcifying agent is added in this comparative example, and other conditions are consistent with Example 1.
[0056] The molybdenum recovery rate obtained in this embodiment is 34.7%.
[0057] Comparative Example 5 This comparative example provides a method for separating and recovering molybdenum and nickel from molybdenum-nickel ore. The difference from Example 1 is that potassium carbonate is not added in this comparative example, and other conditions are consistent with Example 1.
[0058] The platinum recovery rate obtained in this embodiment is 0%.
[0059] It can be seen from the above embodiments and comparative examples that, as shown in Comparative Example 1, when the calcifying agent and potassium carbonate are mixed with nickel-molybdenum ore at the same time, potassium carbonate and the calcifying agent simultaneously assume the sulfur fixation effect in the desulfurization process, and potassium carbonate absorbs sulfur dioxide to generate potassium sulfate, resulting in reagent waste and high cost; As shown in Comparative Example 2, when the carbonate is sodium carbonate, under the condition of low second roasting temperature, the thermodynamic conditions for the reaction between sodium carbonate and calcium molybdate in calcified molybdenum roasted sand do not hold, resulting in unsuccessful molybdenum conversion and no leaching of molybdenum in the subsequent water leaching process; As shown in Comparative Example 3, when the carbonate is sodium carbonate, even if the roasting temperature is increased to 600° C., molybdenum and nickel cannot be separated by the water leaching method of the present application; As shown in Comparative Example 4, when no calcifying agent is added, sulfur dioxide produced by desulfurization of molybdenum-nickel ore is discharged, causing environmental pollution; As shown in Comparative Example 5, when potassium carbonate is not added, the calcium molybdate in the calcified molybdenum roasted sand cannot be completely converted into soluble molybdate, and molybdenum is not leached in the subsequent water leaching process.
[0060] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
[0061] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.
Claims
1. A method for separating and recovering molybdenum and nickel from molybdenum-nickel ore, characterized in that: include: Mixing molybdenum-nickel ore and a calcifying agent, and first roasting to obtain calcified molybdenum roasted sand; The calcified molybdenum roasted sand and carbonate are mixed and granulated to obtain green balls; The green balls are subjected to a second roasting to obtain roasted balls, and the roasted balls are crushed and ground to obtain roasted clinker; The roasted clinker is mixed with water for leaching, and a leaching solution and a leaching residue are obtained after solid-liquid separation; The leachate is purified and impurities removed to obtain a pure potassium molybdate solution; The leached slag is subjected to reduction smelting to obtain a low-grade nickel matte product; The carbonate includes potassium carbonate.
2. The method for separating and recovering molybdenum and nickel from molybdenum-nickel ore according to claim 1, characterized in that: The calcifying agent includes one or more of slaked lime, quicklime and limestone.
3. The method for separating and recovering molybdenum and nickel from molybdenum-nickel ore according to claim 2, characterized in that: The dosage of the calcifying agent is 1 to 3 times of the theoretical amount calculated based on the sulfur content.
4. The method for separating and recovering molybdenum and nickel from molybdenum-nickel ore according to claim 1, characterized in that: The temperature of the first calcination is 400° C.-600° C., and the calcination time is 1 h-3 h.
5. The method for separating and recovering molybdenum and nickel from molybdenum-nickel ore according to claim 1, characterized in that: The mass ratio of the carbonate to the calcified molybdenum roasted sand is (0.2-1.5):
1.
6. The method for separating and recovering molybdenum and nickel from molybdenum-nickel ore according to claim 1, characterized in that: The second calcination temperature is 150° C.-300° C., and the calcination time is 1 h-3 h.
7. The method for separating and recovering molybdenum and nickel from molybdenum-nickel ore according to claim 1, characterized in that: The leaching includes normal pressure leaching, and the solid-liquid ratio of the normal pressure leaching is (0.1 kg-0.5kg):1L.
8. The method for separating and recovering molybdenum and nickel from molybdenum-nickel ore according to claim 7, characterized in that: The temperature of the atmospheric pressure leaching is 30° C.-90° C., and the stirring time is 1 h-3 h.
9. The method for separating and recovering molybdenum and nickel from molybdenum-nickel ore according to claim 1, characterized in that: The finely ground particle size is 50 meshes to 300 meshes.
10. The method for separating and recovering molybdenum and nickel from molybdenum-nickel ore according to any one of claims 1 to 9, characterized in that: The molybdenum content of the molybdenum-nickel ore is 2%-10%, and the nickel content is 2%-10%.
Citation Information
Patent Citations
Alkali breakdown process of molybdenum-vanadium multi-metal metallurgy smelting materials
CN101333601A
Method for preparing sodium molybdate from nickel-molybdenum ore
CN103952534A
Method for separating and recovering vanadium and molybdenum from vanadium-containing waste residues
CN115161480A
Method for separating and extracting molybdenum and nickel from carbon-containing nickel-molybdenum ore
CN116590524A
Process for recovering chromium, vanadium, molybdenum and tungsten values from a feed material
US4298581A