Method for efficiently extracting scattered metal indium and germanium from zinc leaching residues

By combining side-blown smelting and fuming pyrometallurgical processes with acid leaching and replacement, the problem of indium and germanium being difficult to recover efficiently from zinc leaching residue has been solved, achieving efficient extraction and high recovery rate of indium ingots and crude germanium dioxide production.

CN118726772APending Publication Date: 2024-10-01CINF ENG CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410736407.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-07
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In existing zinc smelting processes, the recovery and utilization of rare dispersed metals indium and germanium in zinc leaching residue are not very effective, and they are difficult to extract efficiently.

Method used

Zinc leaching residue is treated using a side-blown smelting + fuming pyrometallurgical process. Indium and germanium are enriched by acid leaching, neutralization and iron powder replacement processes. Indium and germanium are then extracted through extraction, back-extraction, electrolysis and casting. Finally, germanium is refined to obtain crude germanium dioxide product.

Benefits of technology

It improves the recovery rate of indium and germanium, reduces processing costs, has high added value, and achieves a comprehensive recovery rate of over 72%, resulting in significant economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118726772A_ABST
    Figure CN118726772A_ABST
Patent Text Reader

Abstract

The invention discloses a method for efficiently extracting scattered metal indium and germanium from zinc leaching residues. The method comprises the following steps: (1) treating the zinc leaching residues by adopting a side-blowing smelting and fuming converting fire process to obtain zinc oxide smoke dust; (2) zinc oxide smoke dust is subjected to acid leaching, and zinc oxide smoke dust acid leaching liquid is obtained; zinc oxide neutralization, iron powder reduction and iron powder replacement are carried out on the pickle liquor, and indium and germanium are enriched into indium-rich slag; (3) performing two-stage acid leaching on the indium-rich slag; (4) extracting indium from the first-section leachate to obtain an indium-rich organic phase and indium raffinate; after the indium-rich organic phase is subjected to acid pickling, indium is subjected to reverse extraction, and indium reverse extraction liquid is obtained; after the indium strip liquor is deoiled, neutralizing and replacing to obtain sponge indium; casting sponge indium into an indium anode plate; performing indium anode plate electrolysis and ingot casting to obtain an indium ingot product; (5) after the indium raffinate is deoiled, germanium is extracted, and a germanium-rich organic phase is obtained; the germanium-rich organic phase is subjected to multi-stage acid pickling and germanium reverse extraction, and germanium reverse extraction liquid is obtained; and germanium refining is carried out after the germanium strip liquor is subjected to oil removal, and a crude germanium dioxide product is obtained. The comprehensive recovery rate of main metal is high, the comprehensive recovery rate of indium is larger than 72%, the comprehensive recovery rate of germanium is larger than 65%, and the overall process is high in economic benefit.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nonferrous metal smelting, and in particular relates to a method for efficiently extracting rare metals indium and germanium from zinc leaching slag. Background Art

[0002] Indium is a typical rare metal with good mechanical and physical and chemical properties. It is widely used in high-tech and military fields such as indium tin oxide targets, electronic semiconductors, photovoltaic cells, etc. It is an important multi-purpose strategic resource. Indium can be divided into primary indium and recycled indium according to its extraction raw materials. Primary indium is indium extracted from indium-containing minerals. In the process of non-ferrous smelting and blast furnace ironmaking, indium will be enriched in certain intermediate products and by-products, such as slag, leaching slag, electrolyte, smoke, etc. The indium extracted from these raw materials belongs to primary indium. Recycled indium is generally recovered from secondary resources, such as ITO waste targets, discarded liquid crystal displays and various indium-containing alloys. At present, indium recovered from zinc hydroprocessing in my country accounts for 80% to 90% of the primary indium production.

[0003] Germanium is also a rare metal with many special properties. It has extensive and important applications in semiconductors, aerospace measurement and control, nuclear physics detection, fiber optic communications, infrared optics, solar cells, chemical catalysts, biomedicine and other fields. It is an important strategic resource. Germanium has a low content in most rocks and can only form a limited number of independent minerals. It is even more difficult to form independent deposits. It only exists as an associated element in other elements. It is commonly found in copper- and zinc-rich polymetallic sulfide deposits and coal mines, and is produced as a co-associated mineral. The production of germanium worldwide mainly comes from sulfide lead-zinc deposits and germanium-rich lignite deposits, which constitute the two most important types of known germanium deposits.

[0004] At present, most zinc smelting enterprises at home and abroad adopt the wet process, and their zinc production accounts for more than 85% of the global total production. Usually, for every ton of zinc produced by the wet process, 1.0 to 1.2 tons of zinc leaching slag will be produced. In 2023, my country's refined zinc production will be 6.623 million tons, and a large amount of zinc leaching slag will also be produced. In addition to containing valuable metals such as zinc, indium, and gallium, these zinc leaching slags are also a hazardous waste. At present, the main pyrometallurgical process is used to treat zinc leaching slag. The specific treatment methods are: rotary kiln volatilization method, fuming furnace volatilization method, Ausmelt method, oxygen-enriched side blowing method, electric heating method, sulfuric acid roasting method, chlorinated sulfuric acid roasting method, vortex furnace smelting method, etc. Pyrometallurgical treatment is to reduce and volatilize zinc, lead and scattered metals at high temperature. The flue gas is cooled and dusted, and finally zinc oxide smoke is obtained, which is sent to the zinc smelting system for recovery. Although the existing zinc smelting system can efficiently recover the valuable metal zinc in the zinc oxide dust, it is not very effective in recovering the rare metal indium and germanium. Therefore, it is urgent to develop a method for efficiently extracting metal indium and germanium from zinc leaching slag. Summary of the invention

[0005] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a method for efficiently extracting rare metal indium and germanium from zinc leaching residue.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] The method provided by the present invention for efficiently extracting rare metal indium and germanium from zinc leaching residue comprises the following steps:

[0008] 1) The zinc leaching slag is treated by side-blowing smelting + fuming blowing pyrometallurgy process to obtain zinc oxide dust;

[0009] 2) Indium and germanium enrichment:

[0010] The zinc oxide dust obtained in step 1) is subjected to acid leaching treatment, and after leaching, is subjected to filter pressing to obtain a zinc oxide dust acid leaching solution and a zinc oxide dust leaching residue;

[0011] Adding zinc oxide fume and iron powder to the zinc oxide fume acid leaching solution, adjusting the pH to a suitable range, and then adding iron powder to replace indium and germanium in the solution to obtain indium-rich slag;

[0012] 3) Acid leaching of indium-rich slag:

[0013] The indium-rich slag obtained in step 2) is subjected to a two-stage acid leaching treatment, specifically comprising:

[0014] The indium-rich slag is subjected to a low-acid leaching step, and after the leaching step is completed, the leaching solution and the leaching slag are obtained by filter pressing, wherein the leaching solution is sent to a subsequent indium extraction process;

[0015] The first stage leaching residue is slurried and then subjected to the second stage high acid leaching. After the leaching is completed, the second stage leaching liquid and the second stage leaching residue are obtained by filter pressing. The second stage leaching liquid is returned to the first stage low acid leaching. The second stage leaching residue is returned to step 1) for side blowing smelting + fuming blowing pyrometallurgical process treatment.

[0016] 4) Indium extraction, stripping, replacement, electrolysis and casting:

[0017] The first section of the leachate obtained in step 3) is sent to an indium extraction box, and indium extraction, acid washing, and stripping are performed in sequence, specifically: the first section of the leachate is subjected to indium extraction to obtain an indium-rich organic phase and an indium raffinate; then the indium-rich organic phase is subjected to acid washing, and then stripping of indium is performed to obtain an indium stripping solution and a lean organic phase;

[0018] After the indium stripping solution is deoiled, it is sent to a neutralization tank, a neutralizing agent is added to the tank for a neutralization reaction, and after the reaction is completed, a displacement agent is added to the solution for a displacement reaction to obtain sponge indium;

[0019] The sponge indium is washed, melted, and impurity-removed before being cast into an indium anode plate;

[0020] Transferring the indium anode plate to an electrolytic cell for electrolysis and ingot casting to obtain an indium ingot product;

[0021] 5) Extraction, stripping and refining of germanium:

[0022] After deoiling the indium raffinate obtained in step 4), adjusting its pH to a set range, and then sending it to a multi-stage countercurrent centrifugal extraction device to extract germanium to obtain a germanium-rich organic phase;

[0023] The germanium-rich organic phase is sent to a germanium extraction box for multi-stage acid washing and stripping of germanium to obtain a germanium stripping solution;

[0024] The germanium stripping solution is deoiled and then refined to obtain a crude germanium dioxide product.

[0025] The present invention adopts the existing mature side-blowing smelting + fuming blowing pyrometallurgical process to treat zinc leaching slag. The produced vitrified fuming slag can achieve the harmlessness of zinc leaching slag and obtain zinc oxide smoke. The zinc oxide smoke is treated by the process of the present invention to recover indium and germanium, and finally electrolytic indium ingots and crude germanium dioxide products are produced.

[0026] In some embodiments, according to the difference in components in the zinc leaching slag, the mass contents of the main element chemical components in the zinc oxide smoke obtained in step 1) are: Zn 45.00% to 65.00%, In 0.015% to 0.15%, Ge0 to 0.03%, Pb10.00% to 18.00%, Ag 0.04% to 0.15%, Fe 1.50% to 3.50%, and As0.04% to 0.60%.

[0027] Since the content of indium and germanium in zinc oxide dust is low, the concentration of indium and germanium in the zinc oxide dust acid leaching solution is also at a low level. If the acid leaching solution is directly extracted, the extractant occupies a large amount and is consumed, and a large amount of wastewater is produced, and the treatment cost is high. Therefore, the zinc oxide dust acid leaching solution is treated with zinc oxide neutralization + iron reduction + iron powder replacement to enrich indium and germanium into indium-rich slag, and then the indium-rich slag is acid-leached. The concentration of indium and germanium in the indium-rich slag acid leaching solution is greatly improved, and the concentration of other metal ions is reduced, which is conducive to the subsequent extraction and recovery of indium and germanium.

[0028] Preferably, in step 2), the process of acid leaching the zinc oxide dust is: leaching the zinc oxide dust with sulfuric acid, controlling the liquid-solid ratio to 3-5 mL:1 g, the leaching temperature to 90-95° C., the reaction time to 3-5 h, and the final acid concentration not exceeding 25 g / L.

[0029] In step 2), zinc oxide smoke + iron powder is added to the zinc oxide smoke acid leaching solution (zinc oxide smoke is used to adjust the pH value, and the iron powder is added here to reduce the Fe 3+ Reduction to Fe 2+ , keep the solution pH no higher than 5 during operation, Fe 2 + It will not precipitate into indium-rich, and the mass of iron powder added is relative to Fe+2Fe 3+ =3Fe 2+ The indium-rich slag is prepared by adding iron powder to replace indium and germanium in the solution, wherein the amount of iron powder added is 1.0 to 1.05 times the mass of iron powder required for the complete reaction), and after adjusting the pH not to exceed 5, iron powder is added to replace indium and germanium in the solution to obtain indium-rich slag, wherein the iron powder addition coefficient (the amount of iron powder added relative to the mass of iron powder required to completely replace indium and germanium in the solution) is 1.0 to 1.05, and the mass content of In in the indium-rich slag is 0.6% to 3.0%, and the mass content of Ge is 0.06% to 0.2%.

[0030] The zinc oxide smoke leaching slag obtained in step 2) is sent to a zinc smelting system for treatment.

[0031] Preferably, in step 3), the process of the first stage low-acid leaching is: controlling the initial acid concentration of leaching to 60-85 g / L, the leaching temperature to 90-95° C., the liquid-solid ratio to 3-5 mL:1 g, and the final acid concentration not exceeding 25 g / L; the process of the second stage high-acid leaching is: controlling the initial acid concentration to 130-180 g / L, the leaching temperature to 90-95° C., the liquid-solid ratio to 4-6 mL:1 g, and the leaching time to 4-5 h.

[0032] Preferably, step 4) is specifically:

[0033] The first-stage leaching solution is sequentially subjected to indium extraction, acid washing and stripping, with an operating temperature of 35°C to 40°C and a mixing time of 5 to 10 minutes; the organic phase for indium extraction is P204+sulfonated kerosene, wherein the volume fraction of P204 is 25% to 30%, the relative ratio O / A=1:(1 to 4), and the extraction level is 3 to 5; the indium-rich organic phase is acid washed with a 120 to 150 g / L sulfuric acid solution, the relative ratio O:A=(4 to 6):1, and the acid washing level is 2 to 3; indium is stripped with a 4 to 6 mol / L hydrochloric acid solution, the relative ratio O / A=(14 to 20):1, and the stripping level is 3 to 5;

[0034] After the indium stripping solution is deoiled by ultrasonic wave and activated carbon, it is sent to a neutralization tank, sodium hydroxide is added as a neutralizing agent in the tank to carry out a neutralization reaction, the reaction temperature is controlled at 35-40°C, the reaction time is 1-2h, and the pH at the reaction end is 1-2. After the reaction is completed, zinc plate or zinc powder is added to the solution as a replacement agent to carry out a replacement reaction, the reaction temperature is controlled at 30-40°C, and the reaction time is 4-6h to obtain sponge indium;

[0035] The sponge indium is washed, melted at 200-300°C, and cast into an indium anode plate after adding sodium hydroxide to remove impurities;

[0036] Transfer the indium anode plate to the electrolytic cell and control the current density to 80-140A / m 2 The cell voltage is 0.35±0.05V, the center distance of the same pole is 70-90mm, the electrolysis cycle is 6-9 days for the cathode, the electrolyte is controlled at room temperature, electrolysis is carried out to obtain electrolytic indium, and then the electrolytic indium is cast at 300-350℃ to obtain an indium ingot product with a smooth and flat surface.

[0037] Step 4) also includes: washing the lean organic phase with iron and pickling in sequence, and the organic phase after pickling is returned for recycling. The lean organic phase iron washing liquid adopts 7% oxalic acid solution, with a relative O / A of (20-25):1, and the iron washing level is 2-3 levels; the organic phase after iron washing is pickled with a 120-150g / L sulfuric acid solution, with a relative O / A of (20-25):1, and the pickling level is 2-3 levels.

[0038] Step 4) also includes: adding sodium hydroxide to the liquid after indium replacement to precipitate zinc, controlling the end point pH to 12-13, sending the zinc slag obtained after pulp pressure filtration to the zinc smelting system for treatment, and sending the filtrate to wastewater treatment.

[0039] Step 5) is specifically as follows: after the indium raffinate is deoiled by ultrasound and activated carbon, sodium hydroxide is added to adjust its pH to 2-3, and then the raffinate is sent to a multi-stage countercurrent centrifugal extraction device for germanium extraction, wherein the organic phase for germanium extraction is YW100+P204+sec-octanol+sulfonated kerosene, the volume fraction of YW100 is 1%-3%, the volume fraction of P204 is 10%-15%, the volume fraction of sec-octanol is 1%-5%, the ratio O / A is 1: (10-15), and the extraction stage is 4-6;

[0040] The germanium-rich organic phase is sent to a germanium extraction box for multi-stage acid washing and stripping of germanium: the operating temperature is 30-35°C, and the mixing time is 10-15min; 10-20g / L sulfuric acid is used for multi-stage acid washing, the ratio O / A is (4-6): 1, and the number of acid washing stages is 2-3; 1.5-3.0mol / L NH4F solution is used for stripping of germanium, the ratio O / A is (8-20): 1, and the number of stripping stages is 3-5;

[0041] The germanium stripping solution is deoiled and then subjected to germanium refining, wherein the germanium refining includes germanium precipitation, chlorination distillation, and hydrolysis of germanium tetrachloride, specifically including:

[0042] The germanium stripping solution is subjected to ultrasonic and activated carbon deoiling, and then sent to a germanium precipitation tank, where liquid ammonia is introduced to precipitate germanium, and the pH of the germanium precipitation endpoint is controlled to be 9-10, and the reaction time is 2-4 hours. After the reaction is completed, the slurry is filtered to obtain filter residue and filtrate, and the filtrate is returned to the extraction section. The filter residue is the germanium concentrate, which is dried at 120-200°C and sent to the chlorination distillation process;

[0043] The germanium concentrate is added to the chlorination distillation reactor, and hydrochloric acid is added at the same time. After the liquid chlorine passes through the chlorine buffer tank, it is quantitatively added to the reactor for chlorination distillation, and the initial acid concentration of the chlorination distillation process is controlled not to exceed 8 mol / L, the final acid is 7.0-7.4 mol / L, and the liquid-solid ratio is 3-5 mL:1g. Steam is used for indirect heating, and the chlorine is controlled to pass for 30 minutes at a low temperature of less than 50° C., pass for 40-60 minutes at a medium temperature of 50-60° C., pass for 40-60 minutes at a high temperature of 83-90° C., and pass for 25-30 minutes at a high temperature of 90-115° C. to obtain distilled volatile germanium tetrachloride gas;

[0044] The germanium tetrachloride gas is condensed by ice-salt water, and the condensation temperature is controlled to be lower than -10°C. After condensation, hydrolysis is performed, specifically, the condensed germanium tetrachloride is added into a hydrolysis tank, pure water is used as a hydrolysis mother liquor, and is quantitatively added into the hydrolysis tank, and the volume ratio of pure water to germanium tetrachloride is controlled to be 6-7:1 during hydrolysis, and the hydrolysis reaction temperature is controlled to be no more than 0°C by ice-salt water, and a GeO2 mixed liquid is obtained by hydrolysis, and the GeO2 mixed liquid is separated from the solid by vacuum filtration to obtain solid GeO2, and the solid GeO2 is dried by microwave, and the drying temperature is controlled to be 120-140°C, and a crude germanium dioxide product is obtained after drying.

[0045] In step 5), the germanium raffinate obtained after germanium extraction is subjected to ultrasonic and activated carbon degreasing and then sent to the zinc smelting system for treatment;

[0046] The organic phase obtained after stripping germanium is acidified with sulfuric acid having a concentration not exceeding 100 g / L and then returned for recycling, with a relative ratio of O / A = (4-6): 1 and an acidification level of 2-3 levels;

[0047] In the chlorination distillation process, when the temperature of the distillation residue is lower than 70°C, it is sent to filtration, the filter residue is sent to the rotary kiln for volatilization treatment, and the filtrate is returned to the chlorination distillation. When the impurity content is high, it is sent to evaporation and drying treatment in an open circuit;

[0048] The waste gas discharged from the chlorination distillation and condensation absorption devices is absorbed by the alkali liquid absorption device to meet the standards;

[0049] Most of the solution after liquid-solid separation of the GeO2 mixed solution is returned to the hydrolysis mother liquor tank, and a part of it is added with alkali and calcium chloride for open circuit treatment of germanium precipitation, and then sent to sewage treatment after germanium precipitation.

[0050] The beneficial effects of the present invention are as follows:

[0051] (1) In view of the low content of indium and germanium in the zinc oxide smoke obtained from the pyrometallurgical treatment of zinc leaching slag, the process of acid leaching → neutralization + replacement is used to enrich indium and germanium into indium-rich slag, and then the indium-rich slag acid leaching liquid is extracted. In this process flow, the concentration of indium and germanium in the extraction liquid is improved, and the concentration of other ions is reduced. The extraction treatment volume is small, the effect is good, the extraction rate is high, the selected extraction box is small, the extraction agent occupancy and consumption are small, the output wastewater is small, and the overall consumption cost is low.

[0052] (2) The products of this process are electrolytic indium ingots and crude germanium dioxide, which have high added value. The comprehensive recovery rate of major metals is high, with the comprehensive recovery rate of indium exceeding 72% (zinc leaching slag → indium ingots) and the comprehensive recovery rate of germanium exceeding 65% (zinc leaching slag → crude germanium dioxide), and the overall process has high economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] Figure 1 The present invention is a simplified process flow diagram for efficiently extracting rare metal indium and germanium from zinc leaching residue. DETAILED DESCRIPTION

[0054] Example 1

[0055] The zinc leaching slag is treated by side-blowing smelting + fuming blowing pyrometallurgy process to obtain zinc oxide fume, wherein the main chemical composition contents of the zinc oxide fume are: Zn 46.54%, In 0.123%, Ge 0.014%.

[0056] The zinc oxide dust was leached with sulfuric acid, the liquid-solid ratio was controlled to be 4ml:1g, the reaction time was 4h, the leaching temperature was 90℃, the final leaching acid was 22g / L, the leached pulp was filtered through a filter press to obtain the zinc oxide dust acid leaching solution; zinc oxide dust and iron powder were added to the zinc oxide dust acid leaching solution, and the amount of iron powder added was to reduce the Fe content in the solution to 1. 3+ Reduction to Fe 2+ The required theoretical amount, after adjusting pH=5, iron powder is added to replace indium and germanium to obtain indium-rich slag, and the amount of iron powder added is the amount of iron powder required to completely replace indium and germanium; wherein the obtained indium-rich slag contains In1.12% and Ge0.11%.

[0057] The indium-rich slag is treated by two-stage acid leaching with sulfuric acid: the indium-rich slag is added to the first leaching tank, the initial leaching acid is controlled to be 60g / L, the leaching temperature is 90°C, the liquid-solid ratio is 4ml:1g, the final acid is 19g / L, the leached slurry is filtered through a chamber filter press to obtain a first-stage leaching liquid and a first-stage leaching slag; the first-stage leaching liquid is sent to the indium extraction process for treatment, and the indium concentration in the solution is 2.58g / L and the germanium concentration is 0.24g / L; the first-stage leaching slag is slurried and sent to the second-stage leaching tank;

[0058] Sulfuric acid was added to the second-stage leaching tank, the initial acid was controlled at 155 g / L, the leaching temperature was 90°C, the liquid-solid ratio was 6 ml:1 g, the leaching time was 4 h, and the leached slurry was filtered through a chamber filter press to obtain the second-stage leaching liquid and the second-stage leaching residue; the second-stage leaching liquid was returned to the first-stage leaching process, and the second-stage leaching residue was returned to the side-blowing smelting + fuming blowing pyrometallurgical process for treatment.

[0059] A section of leaching liquid is pumped into the indium extraction box, and 3-stage indium extraction, 2-stage acid washing, 3-stage stripping, 2-stage iron washing, and 2-stage acid washing are set up in sequence, with an operating temperature of 35°C and a mixing time of 5 minutes. The indium raffinate is sent to recover germanium after ultrasonic and activated carbon oil removal; the indium stripping liquid is sent to recover indium after ultrasonic and activated carbon oil removal. The organic phase for indium extraction is P204+sulfonated kerosene, and the volume fraction of P204 is 25%. Compared with O / A=1:2, when the content of sulfuric acid does not exceed 20g / L, P204 can only remove In in the solution. 3+ , Fe 3+ Extraction into the organic phase can thus 3+ Enrichment and purification; 150g / L sulfuric acid solution is used for pickling, and O:A=5:1. The purpose of pickling is to wash away a small amount of raffinate mixed in the organic phase and reduce the entry of other ions into the stripping solution; 6mol / L hydrochloric acid solution is used to strip indium, and O:A=14:1; 7% oxalic acid solution is used for the poor organic phase iron washing solution, and O:A=20:1. Due to C2O4 2- with Fe 3+ The complexation of Fe 3+ Completely stripping off is an important step in the recycling of the organic phase; the organic phase after iron washing is pickled with a 150g / L sulfuric acid solution, and the organic phase after pickling is returned for recycling, with a ratio of O:A=20:1.

[0060] The obtained indium stripping solution has an indium concentration of 68.6 g / L, which is pumped into a neutralization tank, and sodium hydroxide is added into the tank for neutralization reaction, the reaction temperature is controlled at 35°C, the reaction time is 1 hour, and the reaction end point pH is 1.5; the neutralized solution is replaced with a zinc plate / zinc powder, the reaction temperature is controlled at 30°C, the reaction time is 6 hours, and sponge indium is obtained; the sponge indium is washed, melted at 300°C, and sodium hydroxide is added to remove impurities and then cast into an indium anode plate; sodium hydroxide is added to the solution after the indium is replaced to precipitate zinc, and the end point pH is controlled to be 13, and the zinc slag obtained after pulp filtration is sent to a zinc smelting system for treatment, and the filtrate is sent to wastewater treatment.

[0061] Transfer the indium anode plate to the electrolytic cell and control the current density to 90A / m 2 , the cell voltage is 0.36V, the electrolyte is controlled at 25°C, the electrolysis cycle is 7d, and electrolytic indium is obtained; the electrolytic indium is cast at 300°C to obtain an indium ingot product with a smooth and flat surface.

[0062] After adding sodium hydroxide to adjust the deoiled indium raffinate to pH=2.5, it is sent to a 6-stage countercurrent centrifugal extraction device. The organic phase for extracting germanium is 1% YW100+15% P204+1% octanol+sulfonated kerosene, the operating temperature is 35°C, the mixing time is 15min, the phase ratio is O:A=1:10, and the extraction level is 6. The germanium in the solution is enriched and purified into the organic phase through extraction. The germanium-rich organic phase obtained after extraction is sent to the germanium extraction box, and multi-stage acid washing, stripping, and acidification are set in sequence, the operating temperature is 35°C, and the mixing time is 15min. The germanium raffinate is sent to the zinc smelting system for treatment after ultrasonic and activated carbon deoiling; the germanium stripping solution is sent to the germanium refining section after ultrasonic and activated carbon deoiling. 15g / L sulfuric acid was used for pickling, with O:A=5:1 and pickling level 2; 2.5mol / L NH4F solution was used for stripping germanium, with O:A=18:1 and stripping level 5; the organic phase after stripping germanium was acidified with 100g / L sulfuric acid and returned for recycling, with O:A=5:1 and acidification level 2.

[0063] The germanium concentration in the obtained germanium stripping solution is 41.1g / L. It is sent to the germanium precipitation tank, and liquid ammonia is introduced to precipitate germanium. The pH value of the germanium precipitation endpoint is controlled to be 9.5. The reaction time is 3h. The germanium precipitation slurry is filtered by a chamber filter press, and the filtrate is returned to the extraction section. The filter residue is the germanium concentrate, which is dried at 150°C and sent to the chlorination distillation process.

[0064] In order to further purify the germanium concentrate into germanium products, the germanium concentrate is added to the chlorination distillation reactor, and hydrochloric acid is added at the same time. After the liquid chlorine passes through the chlorine buffer tank, it is quantitatively added to the reactor for chlorination distillation. The initial acid of leaching is controlled to be 8mol / L, the final acid is 7.2mol / L, and the liquid-solid ratio is 5ml:1g. Steam is used for indirect heating, and the chlorine is passed for 30 minutes at low temperature (less than 50℃), 50 minutes at medium temperature (50-60℃), 50 minutes at medium and high temperature (83-90℃), and 30 minutes at high temperature (90-115℃) to obtain the distillation volatiles, namely, germanium tetrachloride gas; the germanium tetrachloride gas is condensed with ice brine, and the condensation temperature is controlled to be lower than -10℃. After condensation, it is collected and sent to the hydrolysis process. When the temperature of the distillation residue is lower than 70℃, it is sent to filtration, the filter residue is sent to the rotary kiln for volatilization treatment, and the filtrate is returned to the chlorination distillation. When the impurity content is high, it is sent to open circuit for evaporation and drying treatment. The waste gas emitted by the chlorination distillation and condensation absorption devices is absorbed by the alkaline solution absorption device to meet the standards.

[0065] The condensed germanium tetrachloride is added to the hydrolysis tank, and pure water is used as the hydrolysis mother liquor, which is quantitatively added to the hydrolysis tank. The volume ratio of pure water to germanium tetrachloride is controlled to be 7:1 during hydrolysis, and the hydrolysis reaction temperature is controlled not to exceed 0°C by ice brine. The GeO2 mixed solution obtained by hydrolysis is separated by vacuum filtration for liquid-solid separation. The separated solid is GeO2, which is dried by microwave, and the drying temperature is controlled at 130°C. After drying, the crude germanium dioxide product is obtained and stored for sale; most of the separated solution is returned to the hydrolysis mother liquor tank, and a part of it is added with alkali and calcium chloride for open circuit treatment of germanium precipitation, and the precipitation of germanium is sent to sewage treatment.

[0066] Example 2

[0067] The zinc leaching slag is treated by side-blowing smelting + fuming blowing pyrometallurgy process to obtain zinc oxide fume, wherein the main chemical composition of the zinc oxide fume is: Zn57.91%, In0.073%, Ge0.007%.

[0068] The zinc oxide fume is leached with sulfuric acid, the liquid-solid ratio is controlled to be 4ml:1g, the leaching temperature is 95°C, the reaction time is 4h, the final leaching acid is 20g / L, and the leached slurry is filtered through a filter press to obtain a zinc oxide fume acid leaching solution; zinc oxide fume and iron powder are added to the zinc oxide fume acid leaching solution, the iron powder excess coefficient is 1.02, and after adjusting the pH to 5, iron powder is added to replace indium and germanium, and the iron powder excess coefficient is 1.0 to obtain indium-rich slag, wherein the indium-rich slag contains 0.77% In and 0.064% Ge.

[0069] The indium-rich slag is treated by two-stage acid leaching with sulfuric acid: the indium-rich slag is added to the first leaching tank, the initial leaching acid is controlled to be 72g / L, the leaching temperature is 95°C, the liquid-solid ratio is 3ml:1g, the final acid is 20g / L, and the leached slurry is filtered through a chamber filter press to obtain a first-stage leaching liquid and a first-stage leaching slag; the first-stage leaching liquid is sent to the indium extraction process for treatment, and the concentrations of indium and germanium in the solution are 2.36g / L and 0.19g / L respectively; the first-stage leaching slag is slurried and sent to the second-stage leaching tank.

[0070] Sulfuric acid was added to the second-stage leaching tank, the initial acid was controlled at 170 g / L, the leaching temperature was 95°C, the liquid-solid ratio was 5 ml:1 g, the leaching time was 4 h, and the leached slurry was filtered through a chamber filter press to obtain the second-stage leaching liquid and the second-stage leaching residue; the second-stage leaching liquid was returned to the first-stage leaching process, and the second-stage leaching residue was returned to the side-blowing smelting + fuming blowing pyrometallurgical process for treatment.

[0071] A section of leachate is pumped into the indium extraction box, and 3-stage indium extraction, 2-stage pickling, 3-stage stripping, 2-stage iron washing, and 2-stage pickling are set up in sequence, with an operating temperature of 38°C and a mixing time of 6 minutes. The indium raffinate is sent to recover germanium after ultrasonic and activated carbon degreasing; the indium stripping solution is sent to recover indium after ultrasonic and activated carbon degreasing. The organic phase for indium extraction is P204+sulfonated kerosene indium extraction, and the volume fraction of P204 is 30%, with a relative O / A=1:2; 150g / L sulfuric acid solution is used for pickling, with a relative O:A=5:1; 6mol / L hydrochloric acid solution is used to strip indium, with a relative O:A=16:1; 7% oxalic acid solution is used for poor organic phase iron washing liquid, with a relative O:A=25:1; 150g / L sulfuric acid solution is used to pickle the organic phase after iron washing, and the organic phase after pickling is returned for recycling, with a relative O:A=25:1.

[0072] The obtained indium stripping solution has an indium concentration of 71.1 g / L, which is pumped into a neutralization tank, and sodium hydroxide is added into the tank for neutralization reaction, the reaction temperature is controlled at 38°C, the reaction time is 1 hour, and the reaction end point pH is 2; the neutralized solution is replaced with a zinc plate / zinc powder, the reaction temperature is controlled at 30°C, the reaction time is 6 hours, and sponge indium is obtained; the sponge indium is washed, melted at 300°C, and sodium hydroxide is added to remove impurities and then cast into an indium anode plate; sodium hydroxide is added to the solution after the indium is replaced to precipitate zinc, and the end point pH is controlled to be 12, and the zinc slag obtained after pulp filtration is sent to a zinc smelting system for treatment, and the filtrate is sent to wastewater treatment.

[0073] Transfer the indium anode plate to the electrolytic cell and control the current density to 120A / m 2 , the cell voltage is 0.35V, the electrolyte is controlled at 25°C, the electrolysis cycle is 6d, and electrolytic indium is obtained; the electrolytic indium is cast at 300°C to obtain an indium ingot product with a smooth and flat surface.

[0074] After adding sodium hydroxide to adjust the deoiled indium raffinate to pH=2, it is sent to a 6-stage countercurrent centrifugal extraction device. The organic phase for extracting germanium is 2% YW100+15% P204+3% sec-octanol+sulfonated kerosene, the operating temperature is 30°C, the mixing time is 15min, the phase ratio is O:A=1:15, and the extraction level is 6. The germanium-rich organic phase obtained after extraction is sent to the germanium extraction box, and multi-stage acid washing, stripping, and acidification are set in sequence, the operating temperature is 30°C, and the mixing time is 15min. The germanium raffinate is sent to the zinc smelting system for treatment after ultrasonic and activated carbon deoiling; the germanium stripping solution is sent to the germanium refining section after ultrasonic and activated carbon deoiling. 20g / L sulfuric acid was used for pickling, with O:A=5:1 and pickling level 2; 2.5mol / L NH4F solution was used for stripping germanium, with O:A=15:1 and stripping level 5; the organic phase after stripping germanium was acidified with 100g / L sulfuric acid and returned for recycling, with O / A=5:1 and acidification level 2.

[0075] The germanium concentration in the obtained germanium stripping solution is 40.6g / L, which is sent to the germanium precipitation tank, and liquid ammonia is introduced to precipitate germanium. The pH value of the germanium precipitation endpoint is controlled to be 10, and the reaction time is 4h. The germanium precipitated slurry is filtered by a chamber filter press, and the filtrate is returned to the extraction section. The filter residue is the germanium concentrate, which is dried at 180°C and sent to the chlorination distillation process.

[0076] Add germanium concentrate to the chlorination distillation reactor, add hydrochloric acid at the same time, and after the liquid chlorine passes through the chlorine buffer tank, add it quantitatively to the reactor for chlorination distillation. Control the initial acid of the chlorination distillation process to be 8mol / L, the final acid to be 7.2mol / L, and the liquid-solid ratio to be 4ml:1g. Use steam for indirect heating, control the low temperature (less than 50℃) to pass chlorine for 30min, the medium temperature (50-60℃) to pass chlorine for 50min, the medium and high temperature (83-90℃) to pass chlorine for 50min, and the high temperature (90-115℃) to pass chlorine for 30min to obtain the distillation volatiles, namely germanium tetrachloride gas; condense the germanium tetrachloride gas with ice and brine, control the condensation temperature to be lower than -10℃, collect it after condensation and send it to the hydrolysis process. When the temperature of the distillation residue is lower than 70℃, send it to the filter, send the filter residue to the rotary kiln for volatilization treatment, and return the filtrate to the chlorination distillation. When the impurity content is high, open the circuit and send it to evaporation and drying treatment. The waste gas discharged by the chlorination distillation and condensation absorption device is absorbed by the alkali absorption device to meet the standards.

[0077] The condensed germanium tetrachloride is added to the hydrolysis tank, and pure water is used as the hydrolysis mother liquor, which is quantitatively added to the hydrolysis tank. The volume ratio of pure water to germanium tetrachloride is controlled to be 6:1 during hydrolysis, and the hydrolysis reaction temperature is controlled not to exceed 0°C by ice brine. The GeO2 mixed solution obtained by hydrolysis is separated by vacuum filtration. The separated solid is GeO2, which is dried by microwave, and the drying temperature is controlled at 140°C. After drying, the crude germanium dioxide product is obtained and stored for sale; most of the separated solution is returned to the hydrolysis mother liquor tank, and a part of it is added with alkali and calcium chloride to precipitate germanium for open circuit treatment, and the precipitation of germanium is sent to sewage treatment.

[0078] Example 3

[0079] The zinc leaching slag is treated by side-blowing smelting + fuming blowing pyrometallurgy process to obtain zinc oxide fume, wherein the main chemical composition of the zinc oxide fume is: Zn 62.15%, In 0.145%, Ge 0.018%.

[0080] The zinc oxide fume is leached with sulfuric acid, the liquid-solid ratio is controlled to be 3ml:1g, the leaching temperature is 90°C, the reaction time is 4h, the final leaching acid is 18g / L, and the leached slurry is filtered through a filter press to obtain a zinc oxide fume acid leaching solution; zinc oxide fume and iron powder are added to the zinc oxide fume acid leaching solution, the iron powder excess coefficient is 1.0, and after adjusting the pH to 5, iron powder is added to replace indium and germanium, the iron powder excess coefficient is 1.05, and indium-rich slag is obtained, wherein the indium-rich slag contains 1.85% In and 0.2% Ge.

[0081] The indium-rich slag is treated by two-stage acid leaching with sulfuric acid: the indium-rich slag is added to the first leaching tank, the initial leaching acid is controlled to be 63g / L, the leaching temperature is 95°C, the liquid-solid ratio is 3.5ml:1g, the final acid is 20g / L, and the leached slurry is filtered through a chamber filter press to obtain a first-stage leaching liquid and a first-stage leaching slag; the first-stage leaching liquid is sent to the indium extraction process for treatment, and the concentrations of indium and germanium in the solution are 4.86g / L and 0.55g / L respectively; the first-stage leaching slag is slurried and sent to the second-stage leaching tank.

[0082] Sulfuric acid was added to the second-stage leaching tank, the initial acid was controlled at 140 g / L, the leaching temperature was 95°C, the liquid-solid ratio was 6 ml:1 g, the leaching time was 4 h, and the leached slurry was filtered through a chamber filter press to obtain the second-stage leaching liquid and the second-stage leaching residue; the second-stage leaching liquid was returned to the first-stage leaching process, and the second-stage leaching residue was returned to the side-blowing smelting + fuming blowing pyrometallurgical process for treatment.

[0083] A section of leachate is pumped into the indium extraction box, and 4-stage indium extraction, 2-stage pickling, 4-stage stripping, 2-stage iron washing, and 2-stage pickling are set up in sequence, with an operating temperature of 35°C and a mixing time of 8 minutes. The indium raffinate is sent to recover germanium after ultrasonic and activated carbon degreasing; the indium stripping solution is sent to recover indium after ultrasonic and activated carbon degreasing. The organic phase for indium extraction is P204+sulfonated kerosene, and the volume fraction of P204 is 30%, with an O / A ratio of 1:3; 150g / L sulfuric acid solution is used for pickling, with an O:A ratio of 6:1; 6mol / L hydrochloric acid solution is used to strip indium, with an O:A ratio of 14:1; 7% oxalic acid solution is used for poor organic phase iron washing liquid, with an O:A ratio of 25:1; 150g / L sulfuric acid solution is used to pickle the organic phase after iron washing, and the organic phase after pickling is returned for recycling, with an O:A ratio of 25:1.

[0084] The obtained indium stripping solution has an indium concentration of 66.3 g / L, which is pumped into a neutralization tank, and sodium hydroxide is added into the tank for neutralization reaction, the reaction temperature is controlled at 35°C, the reaction time is 2 hours, and the reaction end point pH is 1.5; the neutralized solution is replaced with a zinc plate / zinc powder, the reaction temperature is controlled at 35°C, the reaction time is 6 hours, and sponge indium is obtained; the sponge indium is washed, melted at 300°C, and sodium hydroxide is added to remove impurities and then cast into an indium anode plate; sodium hydroxide is added to the solution after the indium is replaced to precipitate zinc, and the end point pH is controlled to be 12, and the zinc slag obtained after pulp filtration is sent to a zinc smelting system for treatment, and the filtrate is sent to wastewater treatment.

[0085] Transfer the indium anode plate to the electrolytic cell and control the current density to 100A / m 2 , the cell voltage is 0.38V, the electrolyte is controlled at 25°C, the electrolysis cycle is 8d, and electrolytic indium is obtained; the electrolytic indium is cast at 300°C to obtain an indium ingot product with a smooth and flat surface.

[0086] After adding sodium hydroxide to adjust the deoiled indium raffinate to pH=2.5, it is sent to a 6-stage countercurrent centrifugal extraction device. The germanium organic phase is 3% YW100+15% P204+5% sec-octanol+sulfonated kerosene, the operating temperature is 30°C, the mixing time is 15min, the phase ratio is O:A=1:10, and the extraction level is 6. The germanium-rich organic phase obtained after extraction is sent to the germanium extraction box, and multi-stage acid washing, stripping, and acidification are set in sequence, the operating temperature is 30°C, and the mixing time is 15min. The germanium raffinate is sent to the zinc smelting system for treatment after ultrasonic and activated carbon deoiling; the germanium stripping solution is sent to the germanium refining section after ultrasonic and activated carbon deoiling. 20g / L sulfuric acid was used for pickling, with O:A=5:1 and pickling level 2; 3.0mol / L NH4F solution was used for stripping germanium, with O:A=8:1 and stripping level 5; the organic phase after stripping germanium was acidified with 100g / L sulfuric acid and returned for recycling, with O / A=5:1 and acidification level 2.

[0087] The germanium concentration in the obtained germanium stripping solution is 42.9g / L. It is sent to the germanium precipitation tank, and liquid ammonia is introduced to precipitate germanium. The pH value of the germanium precipitation endpoint is controlled to be 10, and the reaction time is 4h. The germanium precipitation slurry is filtered by a chamber filter press, and the filtrate is returned to the extraction section. The filter residue is the germanium concentrate, which is dried at 180°C and sent to the chlorination distillation process.

[0088] Add germanium concentrate to the chlorination distillation reactor, add hydrochloric acid at the same time, and after the liquid chlorine passes through the chlorine buffer tank, add it quantitatively to the reactor for chlorination distillation. Control the initial acid of the chlorination distillation process to be 8mol / L, the final acid to be 7.0mol / L, and the liquid-solid ratio to be 4ml:1g. Use steam for indirect heating, control the low temperature (less than 50℃) to pass chlorine for 30min, the medium temperature (50-60℃) to pass chlorine for 50min, the medium and high temperature (83-90℃) to pass chlorine for 50min, and the high temperature (90-115℃) to pass chlorine for 30min to obtain the distillation volatiles, namely germanium tetrachloride gas; condense the germanium tetrachloride gas with ice and brine, control the condensation temperature to be lower than -10℃, collect it after condensation and send it to the hydrolysis process. When the temperature of the distillation residue is lower than 70℃, send it to the filter, send the filter residue to the rotary kiln for volatilization treatment, and return the filtrate to the chlorination distillation. When the impurity content is high, open the circuit and send it to evaporation and drying treatment. The waste gas discharged by the chlorination distillation and condensation absorption device is absorbed by the alkali absorption device to meet the standards.

[0089] The condensed germanium tetrachloride is added to the hydrolysis tank, and pure water is used as the hydrolysis mother liquor, which is quantitatively added to the hydrolysis tank. The volume ratio of pure water to germanium tetrachloride is controlled to be 6:1 during hydrolysis, and the hydrolysis reaction temperature is controlled not to exceed 0°C by ice brine. The GeO2 mixed solution obtained by hydrolysis is separated by vacuum filtration. The separated solid is GeO2, which is dried by microwave, and the drying temperature is controlled at 140°C. After drying, the crude germanium dioxide product is obtained and stored for sale; most of the separated solution is returned to the hydrolysis mother liquor tank, and a part of it is added with alkali and calcium chloride to precipitate germanium for open circuit treatment, and the precipitation of germanium is sent to sewage treatment.

Claims

1. A method for efficiently extracting rare metal indium and germanium from zinc leaching residue, comprising the following steps: 1) The zinc leaching slag is treated by side-blowing smelting + fuming blowing pyrometallurgy process to obtain zinc oxide dust; 2) Indium and germanium enrichment: The zinc oxide dust obtained in step 1) is subjected to acid leaching treatment, and after leaching, is subjected to filter pressing to obtain a zinc oxide dust acid leaching solution and a zinc oxide dust leaching residue; Adding zinc oxide fume and iron powder to the zinc oxide fume acid leaching solution, adjusting the pH to a suitable range, and then adding iron powder to replace indium and germanium in the solution to obtain indium-rich slag; 3) Acid leaching of indium-rich slag: The indium-rich slag obtained in step 2) is subjected to a two-stage acid leaching treatment, specifically comprising: The indium-rich slag is subjected to a low-acid leaching step, and after the leaching step is completed, the leaching solution and the leaching slag are obtained by filter pressing, wherein the leaching solution is sent to a subsequent indium extraction process; The first stage leaching residue is slurried and then subjected to the second stage high acid leaching. After the leaching is completed, the second stage leaching liquid and the second stage leaching residue are obtained by filter pressing. The second stage leaching liquid is returned to the first stage low acid leaching. The second stage leaching residue is returned to step 1) for side blowing smelting + fuming blowing pyrometallurgical process treatment. 4) Indium extraction, stripping, replacement, electrolysis and casting: The first section of the leachate obtained in step 3) is sent to an indium extraction box, and indium extraction, acid washing, and stripping are performed in sequence, specifically: the first section of the leachate is subjected to indium extraction to obtain an indium-rich organic phase and an indium raffinate; then the indium-rich organic phase is subjected to acid washing, and then stripping of indium is performed to obtain an indium stripping solution and a lean organic phase; After the indium stripping solution is deoiled, it is sent to a neutralization tank, a neutralizing agent is added to the tank for a neutralization reaction, and after the reaction is completed, a displacement agent is added to the solution for a displacement reaction to obtain sponge indium; The sponge indium is washed, melted, and impurity-removed before being cast into an indium anode plate; Transferring the indium anode plate to an electrolytic cell for electrolysis and ingot casting to obtain an indium ingot product; 5) Extraction, stripping and refining of germanium: After deoiling the indium raffinate obtained in step 4), adjusting its pH to a set range, and then sending it to a multi-stage countercurrent centrifugal extraction device to extract germanium to obtain a germanium-rich organic phase; The germanium-rich organic phase is sent to a germanium extraction box for multi-stage acid washing and stripping of germanium to obtain a germanium stripping solution; The germanium stripping solution is deoiled and then refined to obtain a crude germanium dioxide product.

2. The method according to claim 1, characterized in that: According to the difference in components in zinc leaching slag, the mass contents of the main element chemical components in the zinc oxide smoke obtained in step 1) are: Zn 45.00% ~ 65.00%, In 0.015% ~ 0.15%, Ge 0 ~ 0.03%, Pb 10.00% ~ 18.00%, Ag 0.04% ~ 0.15%, Fe 1.50% ~ 3.50%, As 0.04% ~ 0.60%.

3. The method according to claim 1, characterized in that In step 2), the process of acid leaching the zinc oxide dust is as follows: leaching the zinc oxide dust with sulfuric acid, controlling the liquid-solid ratio to 3-5 mL:1 g, the leaching temperature to 90-95° C., the reaction time to 3-5 h, and the final acid concentration to not exceed 25 g / L.

4. The method according to claim 1, characterized in that In step 2), zinc oxide fume and iron powder are added to the zinc oxide fume acid leaching solution, and the mass of iron powder added is relative to Fe+2Fe 3+ =3Fe 2+ The method comprises the following steps: adding 1.0 to 1.05 times the mass of iron powder required for the complete reaction, adjusting the pH value not to exceed 5, and then adding iron powder to replace indium and germanium in the solution, wherein the addition coefficient of the iron powder is 1.0 to 1.05, and obtaining indium-rich slag; wherein the mass content of In in the indium-rich slag is 0.6% to 3.0%, and the mass content of Ge is 0.06% to 0.2%.

5. The method according to claim 1, characterized in that In step 3), the process of the first stage low-acid leaching is as follows: the initial acid concentration of the leaching is controlled to be 60-85 g / L, the leaching temperature is 90-95° C., the liquid-solid ratio is 3-5 mL:1 g, and the final acid concentration does not exceed 25 g / L; the process of the second stage high-acid leaching is as follows: the initial acid concentration is controlled to be 130-180 g / L, the leaching temperature is 90-95° C., the liquid-solid ratio is 4-6 mL:1 g, and the leaching time is 4-5 h.

6. The method according to claim 1, characterized in that Step 4) is specifically as follows: The first-stage leaching solution is sequentially subjected to indium extraction, acid washing and stripping, with an operating temperature of 35°C to 40°C and a mixing time of 5 to 10 minutes; the organic phase for indium extraction is P204+sulfonated kerosene, wherein the volume fraction of P204 is 25% to 30%, the relative ratio O / A=1:(1 to 4), and the extraction level is 3 to 5; the indium-rich organic phase is acid washed with a 120 to 150 g / L sulfuric acid solution, the relative ratio O:A=(4 to 6):1, and the acid washing level is 2 to 3; indium is stripped with a 4 to 6 mol / L hydrochloric acid solution, the relative ratio O / A=(14 to 20):1, and the stripping level is 3 to 5; After the indium stripping solution is deoiled by ultrasonic wave and activated carbon, it is sent to a neutralization tank, sodium hydroxide is added as a neutralizing agent in the tank to carry out a neutralization reaction, the reaction temperature is controlled at 35-40°C, the reaction time is 1-2h, and the pH at the reaction end is 1-2. After the reaction is completed, zinc plate or zinc powder is added to the solution as a replacement agent to carry out a replacement reaction, the reaction temperature is controlled at 30-40°C, and the reaction time is 4-6h to obtain sponge indium; The sponge indium is washed, melted at 200-300°C, and cast into an indium anode plate after adding sodium hydroxide to remove impurities; Transfer the indium anode plate to the electrolytic cell and control the current density to 80-140A / m 2 The cell voltage is 0.35±0.05V, the center distance of the same pole is 70-90mm, the electrolysis cycle is 6-9 days for the cathode, the electrolyte is controlled at room temperature, electrolysis is carried out to obtain electrolytic indium, and then the electrolytic indium is cast at 300-350℃ to obtain an indium ingot product with a smooth and flat surface.

7. The method according to claim 1, characterized in that Step 4) also includes: washing the lean organic phase with iron and pickling in sequence, and returning the organic phase after pickling for recycling; using 7% oxalic acid solution as the iron-washing liquid for the lean organic phase, with a relative O / A ratio of (20-25):1, and an iron washing level of 2-3 levels; and pickling the organic phase after iron washing with a 120-150 g / L sulfuric acid solution, with a relative O / A ratio of (20-25):1, and an acid washing level of 2-3 levels.

8. The method according to claim 1, characterized in that Step 5) is specifically as follows: After the indium raffinate is deoiled by ultrasonic and activated carbon, sodium hydroxide is added to adjust its pH to 2-3, and then it is sent to a multi-stage countercurrent centrifugal extraction device for germanium extraction, wherein the organic phase for germanium extraction is YW100+P204+sec-octanol+sulfonated kerosene, the volume fraction of YW100 is 1%-3%, the volume fraction of P204 is 10%-15%, the volume fraction of sec-octanol is 1%-5%, the phase O / A is 1: (10-15), and the extraction stage is 4-6; The germanium-rich organic phase is sent to a germanium extraction box for multi-stage acid washing and stripping of germanium: the operating temperature is 30-35°C, and the mixing time is 10-15min; 10-20g / L sulfuric acid is used for multi-stage acid washing, the ratio O / A is (4-6): 1, and the number of acid washing stages is 2-3; 1.5-3.0mol / L NH4F solution is used for stripping of germanium, the ratio O / A is (8-20): 1, and the number of stripping stages is 3-5; The germanium stripping solution is deoiled and then subjected to germanium refining, wherein the germanium refining includes germanium precipitation, chlorination distillation, and hydrolysis of germanium tetrachloride, specifically including: The germanium stripping solution is subjected to ultrasonic and activated carbon deoiling, and then sent to a germanium precipitation tank, where liquid ammonia is introduced to precipitate germanium, and the pH of the germanium precipitation endpoint is controlled to be 9-10, and the reaction time is 2-4 hours. After the reaction is completed, the slurry is filtered to obtain filter residue and filtrate, and the filtrate is returned to the extraction section. The filter residue is the germanium concentrate, which is dried at 120-200°C and sent to the chlorination distillation process; The germanium concentrate is added to the chlorination distillation reactor, and hydrochloric acid is added at the same time. After the liquid chlorine passes through the chlorine buffer tank, it is quantitatively added to the reactor for chlorination distillation. The initial acid concentration of the chlorination distillation process is controlled not to exceed 8 mol / L, the final acid is 7.0-7.4 mol / L, the liquid-solid ratio is 3-5 mL:1g, steam is used for indirect heating, and chlorine is passed at a low temperature of less than 50° C. for 30 minutes, at a medium temperature of 50-60° C. for 40-60 minutes, at a high temperature of 83-90° C. for 40-60 minutes, and at a high temperature of 90-115° C. for 25-30 minutes to obtain distilled volatile germanium tetrachloride gas; The germanium tetrachloride gas is condensed by ice-salt water, and the condensation temperature is controlled to be lower than -10°C. After condensation, hydrolysis is performed, specifically, the condensed germanium tetrachloride is added into a hydrolysis tank, pure water is used as a hydrolysis mother liquor, and is quantitatively added into the hydrolysis tank, and the volume ratio of pure water to germanium tetrachloride is controlled to be 6-7:1 during hydrolysis, and the hydrolysis reaction temperature is controlled to be no more than 0°C by ice-salt water, and a GeO2 mixed liquid is obtained by hydrolysis, and the GeO2 mixed liquid is separated from the solid by vacuum filtration to obtain solid GeO2, and the solid GeO2 is dried by microwave, and the drying temperature is controlled to be 120-140°C, and a crude germanium dioxide product is obtained after drying.

9. The method according to claim 1, characterized in that: In step 5), the germanium raffinate obtained after germanium extraction is subjected to ultrasonic and activated carbon deoiling and then sent to the zinc smelting system for treatment.

10. The method according to claim 1, characterized in that In step 5), the organic phase obtained after stripping germanium is acidified with sulfuric acid at a concentration not exceeding 100 g / L and then returned for recycling, with a relative ratio of O / A = (4-6): 1 and an acidification level of 2-3 levels.

Citation Information

Cited By

  • Method for efficiently recovering strategic metal indium from secondary zinc oxide smoke dust

    CN121472604A

  • A process for recovering indium and germanium from low indium germanium dross

    CN123005110A