Aluminum alloy

By using aluminum alloy powder containing titanium, iron and chromium in additive manufacturing, the problems of low process stability and poor economic feasibility of existing aluminum alloys in additive manufacturing are solved, and a high-strength and efficient processing process is achieved. Anisotropy is reduced and process stability and economic efficiency are improved.

CN118726796AInactive Publication Date: 2024-10-01GF CASTING SOLUTIONS NOVAZZANO SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410366449.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-28
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing high-strength aluminum alloys for additive manufacturing suffer from low process stability, insufficient hardening potential and poor economic feasibility during processing, especially due to the evaporation of magnesium and the use of expensive scandium and zirconium elements.

Method used

Aluminum alloy powder containing 1 to 6% titanium, 0.05 to 2% iron, 0.5 to 1.5% chromium and the balance aluminum is used. It is rapidly cooled through laser powder bed fusion technology to avoid segregation of alloy elements and utilize high titanium and Solid solution formation of chromium and intermetallic precipitates of iron significantly reduce anisotropy and increase process stability and strength.

Benefits of technology

Achieving greater process stability and strength, reducing anisotropy, improving the economic efficiency and sustainability of additive manufacturing, avoiding the use of expensive elements, and achieving high yield strengths without the need for subsequent heat treatment and elongation at break.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118726796A_ABST
    Figure CN118726796A_ABST
Patent Text Reader

Abstract

The invention relates to an aluminum alloy. Aluminum alloy for additive manufacturing in powder form, containing the following alloy components: 1 to 6% by weight of titanium, 0.05 to 2% by weight of iron, 0.5 to 2.5% by weight of chromium, and as the remainder aluminum and production-related impurities.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to aluminum alloys in powder form for additive manufacturing.

[0002] In the prior art, several high-strength alloys are known, however these are mainly from the 4xxx or 5xxx Al series and in which Mg is used as an alloying element for precipitation hardening in subsequent heat treatment to achieve the strengthening potential. However, these alloys are not ideal solutions for use in additive manufacturing because, for example, magnesium, among other things, tends to evaporate during additive processing. This leads to reduced process stability and lower material quality, as well as reduced hardening potential due to the loss of Mg.

[0003] Furthermore, other drawbacks of such conventional Al alloys are the anisotropic mechanical behavior caused by their microstructure and driven by specific processing conditions and alloy manufacturing concepts.

[0004] DE 102020131823 A1 discloses an aluminum alloy for additive manufacturing. The alloy contains scandium and zirconium, whereby increased solid solution formation occurs, and in addition, the high required strength is achieved by the necessary subsequent heat treatment.

[0005] The disadvantage is that scandium and zirconium are very expensive to purchase and are elements that are criticized in demand sourcing due to sustainability aspects. In addition, subsequent heat treatment is often necessary to achieve the required strength.

[0006] Various aluminum alloys for additive manufacturing are also sold by Constellium, APWorks, EOS and Elementum 3D, among others, including alloys from the 2xxx, 4xxx and 5xxx series. However, in order to achieve the yield strength of high-strength aluminum alloys, these alloys must be subsequently heat treated, which in turn reduces the economic viability of the alloys.

[0007] The object of the present invention is to propose a high strength aluminium alloy which is tailor-made for additive manufacturing and which is economical and sustainable to produce and which provides a more robust additive manufacturing processing compared to conventional alloys used in additive manufacturing.

[0008] According to the invention, this object is achieved by an aluminum alloy for additive manufacturing in powder form, which contains the following alloying components: 1 to 6% by weight of titanium, 0.05 to 2% by weight of iron, 0.5 to 1.5% by weight of chromium and, as the remainder, aluminum and production-related impurities.

[0009] These high titanium, chromium and iron contents, present in total weight concentrations exceeding the equilibrium solubility in aluminum, are particularly suitable for aluminum alloys used in additive manufacturing. Because the laser is used to melt and cool very quickly during LPBF (laser powder bed fusion), and because the aluminum alloy is applied only in a thin layer, heat can flow down to the massive build platform and previously built structures. Due to this rapid cooling and solidification, the alloying elements can be kept in solid solution and segregation of the alloying elements can be avoided.

[0010] Due to the specific composition of the aluminum alloy of the present invention, the anisotropy tendency of the alloy can be significantly reduced to about half the anisotropy value of competing high-strength alloys (such as Scalalloy), corresponding to about 1 / 10 of the 4XXX alloy.

[0011] The high titanium content of 1 to 6 wt% in this alloy results in high temperature metastable cubic Al3Ti_L12 and stable tetragonal Al3Ti_D. 22 The advantage of initial precipitation is that hardening is achieved through the effect of grain refinement.

[0012] Another advantage of titanium over magnesium in the main alloy component is that titanium brings high process stability when used in additive manufacturing. This is due to the fact that the melting process in the LPBF process leads to a more stable molten pool compared to magnesium-containing aluminum alloys, because there is also no magnesium evaporation and therefore no interfering vapors that reduce the quality of the incident laser beam.

[0013] As mentioned above, a high content of 0.5 to 1.5 wt. % chromium in the additive manufacturing process brings the advantage of forming a high solid solution via subsequent particle precipitation for further strengthening.

[0014] The included iron content of 0.05 to 2 wt. % improves high temperature properties via high temperature stable intermetallic Fe-containing precipitates which also contribute to a fine grained microstructure.

[0015] Preferably, the aluminum alloy contains 2 to 4.5 wt. % titanium.

[0016] Preferably, the aluminum alloy according to the invention contains 2.5 to 4% by weight of titanium. Both of the above possible weight ranges of titanium in the aluminum alloy according to the invention bring with them the above mentioned advantages.

[0017] Preferably, the aluminum alloy of the present invention contains 0.05 to 5 wt. % copper.

[0018] Preferably, the aluminum alloy contains 1.5 to 2.5 wt. % copper.

[0019] Due to the copper content, precipitation hardening is possible in a possible subsequent heat treatment to further increase the strength.

[0020] Preferably, the aluminum alloy contains 1 to 2 wt. % chromium.

[0021] Preferably, the aluminum alloy contains 0.1 to 1.5 wt % iron.

[0022] Preferably, the aluminum alloy contains one or more of the following elements: <0.3 wt. % manganese, <0.5 wt. % silicon, <0.5 wt. % magnesium and / or <0.5 wt. % zinc, and the total wt. % of one or more of these elements is <1 wt. %.

[0023] The inclusion of the above elements has the advantage that they can be derived from recycled waste materials and can be included in the alloy, which supports the concept of sustainability in addition to economic efficiency.

[0024] Preferably, the aluminum alloy is free of scandium, zirconium and rare earth elements. Due to their rare presence, these elements are expensive and environmentally harmful to obtain, which reduces the economic viability of the alloy and increases its negative impact on the environment.

[0025] Despite the avoidance of scandium, zirconium and rare earth elements, components produced by additive manufacturing processes using the alloy according to the invention are still insensitive to hot cracking. This is achieved by a) the absence of magnesium as an alloying element and b) the promotion of grain refinement by the addition of titanium. This also leads to a much more robust process with a more stable melt pool, and a reduced risk of hot cracking. Therefore, the alloy according to the invention can be processed more quickly (build rate is up to ∼50% higher compared to Scalmalloy and even higher compared to AlSi10Mg). This further advantage increases the economic efficiency of the invention.

[0026] It is advantageous if the layer thickness in additive manufacturing by means of the LPBF process is at least 25 μm thick.

[0027] Preferably, the structure of the aluminum alloy according to the invention consists of spherical particles, which preferably have an average particle size of 15 to 75 μm. Particularly preferably, the particle size distribution parameter d 50 In the range between 25-50μm.

[0028] The aluminum alloy preferably has an increased yield strength YS in the as-processed condition. 0.2 >300MPa, and elongation at break A>5%. These mechanical properties are well above the range of HPDC cast high-strength aluminum alloys, and they are similar to the levels of wrought alloys or additively manufactured aluminum alloys with expensive alloying elements.

[0029] Preferably, the yield strength YS of the aluminum alloy is achieved without additional heat treatment. 0.2>300 MPa and elongation at failure A>5%. The aluminum alloy according to the invention therefore has the abovementioned strength and elongation values ​​immediately after having been produced by an additive manufacturing process.

[0030] The object of the present invention is to use the aluminum alloy according to the invention for the additive manufacturing of components. The advantage is that lightweight components with high strength values ​​can be produced in the same way or even better than components produced by casting processes, for example, with reduced wall thickness and weight. In addition, no molds are required, which means that small series can also be produced economically.

[0031] Preferably, such components are used in the fields of aerospace, vehicle construction and energy technology.

[0032] All possible embodiments can be freely combined with one another.

[0033] Some embodiments of the present invention are listed, but the present invention is not limited to these embodiments.

[0034] Some examples of samples have been fabricated by additive manufacturing using the following aluminum alloy compositions Alloy A-Alloy E.

[0035] In the table below, the measured properties of the different aluminum alloys listed in the table above, produced as additively manufactured parts, are listed. It should be emphasized that the values ​​for the samples were obtained without any additional heat treatment.

[0036] The table shows that the sample of aluminum alloy AE has a breaking elongation A and a tensile yield strength YS 0.2 , and this is without any heat treatment. Of course, components manufactured from the aluminum alloy according to the invention using an additive manufacturing process can also be subjected to a heat treatment, which will further improve these values, especially if copper is contained in the aluminum alloy according to the invention.

[0037] The above-mentioned aluminum alloys enable additive manufacturing processes to be used for any component. These alloys are also preferably used in the aerospace, automotive and energy technology sectors, where lightweight components with very high strength play an important role.

[0038] Figure 1 Shows the yield strength YS from different aluminum alloys 0.2 of charts.

[0039] Figure 1 The graph in FIG. 1 shows the yield strength YS of materials known in the prior art and commercially available for additive manufacturing. 0.2 and the yield strength YS of the two aluminum alloys according to the present invention listed in the above table 0.2 .

[0040] It can be seen that the material alloys B and C for additive manufacturing according to the present invention represented by circular symbols have a yield strength YS of about 330 to 350 MPa at room temperature without heat treatment. 0.2 ("AB" means as-built). Materials known from the prior art, produced by Constellium, APWorks, EOS and Elementum 3D and represented by square symbols, have a yield strength YS in the range of about 320 to 480 MPa. 0.2 , but only with the aid of subsequent heat treatment.

[0041] Furthermore, the aluminum alloy of the present invention ensures a yield strength YS of about 220-260 MPa even in a temperature range of 250°C. 0.2 , where other aluminum alloys typically exhibit softening and thus severe strength loss, such as AlSi10Mg with a minimum of <150MPa.

Claims

1. An aluminum alloy for additive manufacturing in powder form, comprising the following alloy components: 1 to 6% by weight of titanium, 0.05 to 2% by weight of iron 0.5 to 2.5 wt% chromium and aluminum and production-related impurities as the balance.

2. The aluminum alloy according to claim 1, characterized in that The aluminum alloy contains 2 to 4.5 wt. % titanium.

3. The aluminum alloy according to claim 1, characterized in that The aluminum alloy contains 2.5 to 4 wt. % titanium.

4. The aluminum alloy according to claim 1, characterized in that The aluminum alloy contains 0.05 to 5 wt % copper.

5. The aluminum alloy according to claim 1, characterized in that The aluminum alloy contains 1.5 to 2.5 wt. % copper.

6. The aluminum alloy according to claim 1, characterized in that The aluminum alloy contains 1 to 2% by weight of chromium.

7. The aluminum alloy according to claim 1, characterized in that The aluminum alloy contains 0.1 to 1.5 wt % iron.

8. The aluminum alloy according to claim 1, characterized in that The aluminum alloy contains one or more of the following elements: <0.3 wt % manganese, <0.5 wt % silicon, <0.5 wt % magnesium and / or <0.5 wt % zinc, and the total wt % of one or more of these elements is <1 wt %.

9. The aluminum alloy according to claim 1, characterized in that The aluminum alloy does not contain scandium, zirconium and rare earth elements.

10. The aluminum alloy according to claim 1, characterized in that It consists of spherical particles, preferably having an average particle size of 15 to 75 μm.

11. The aluminum alloy according to claim 1, characterized in that The aluminum alloy has an increased yield strength YS in the initial processing state. 0.2 >300MPa, and elongation at failure A>5%.

12. The aluminum alloy according to claim 11, characterized in that The yield strength YS of the aluminum alloy is achieved without additional heat treatment. 0.2 >300MPa and elongation at failure A>5%.

13. Use of the aluminum alloy according to any one of claims 1 to 13 for the additive manufacturing of components, preferably in the fields of aerospace, vehicle construction and energy technology.