Rock wool decorative plate manufacturing method
By using water-based glue and cyclone spraying technology in the processing of rock wool decorative boards, the problems of powder glue waste and safety hazards are solved, efficient and environmentally friendly board production is achieved, and the strength and aesthetics of the boards are improved.
Patent Information
- Application Number
- CN202410748476.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-01
AI Technical Summary
The use of powder glue in the processing of existing rock wool decorative boards is costly and easy to waste, and there are potential safety hazards. Traditional boards have low strength and are easy to deform.
Water-based glue is used for spraying and sizing. Water containing hydrophobic agent, dispersant, wetting agent and coupling agent is sprayed through the nozzle. Combined with the design of cyclone cylinder and sizing pipe, uniform paving and layered paving are achieved, and Heat curing and shaping through a continuous press to avoid the production of powder glue.
It reduces processing costs, improves safety, enhances the strength and durability of the board, and achieves resource conservation and environmental protection. The processing process is mechanized and labor intensity is reduced.
Smart Images

Figure CN118727261A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of plate processing, and in particular to a method for manufacturing a rock wool decorative plate. Background Art
[0002] Most of the decorative panels used in buildings are density boards, integrated boards, adhesive boards, etc. The fireproof, moisture-proof, waterproof and strength of the above-mentioned boards are poor. The strength of density boards, integrated boards and adhesive boards is low. Due to its low strength, density boards are difficult to fix. Due to its low strength, integrated boards are prone to unevenness; adhesive boards are prone to deformation due to its low strength. Rock wool boards, as a new decorative board, avoid the defects of the above-mentioned traditional boards. The exterior wall rock wool composite board is made of rock wool fibers produced by high-temperature melting of natural rocks through stacking, compacting, curing and other steps. Powder glue is applied during the processing of existing rock wool decorative boards to facilitate molding; however, the cost of powder glue is high, and it is easy to cause waste due to the blowing and suction of the fan during the application process. In addition, the small amount of powder glue that enters the bag dust collector due to the suction of the fan is easy to cause fire, increasing safety hazards. Summary of the invention
[0003] The purpose of the present invention is to provide a method for manufacturing rock wool decorative panels to solve the problems existing in the above-mentioned prior art. Water-based glue is used, which has low cost and does not produce powder during the gluing process, thereby avoiding waste and improving safety.
[0004] To achieve the above object, the present invention provides the following solutions:
[0005] The present invention provides a method for manufacturing a rock wool decorative board, comprising the following steps:
[0006] Step 1: rock wool pretreatment. The rock wool after the initial scattering and crushing is transported to the cotton shredder to be crushed into fibers of a set length and then transported to the pipeline. A nozzle is provided in the pipeline. Water containing a hydrophobic agent, a dispersant, a wetting agent and a coupling agent is sprayed and mixed by the pipeline water spraying method. The purpose of spraying the wetting agent is to prevent the material from being too dry and to facilitate transportation and mixing.
[0007] Step 2: The mixed materials are transported to the cyclone through a pipeline and then transported to the next step through the bottom of the cyclone;
[0008] Step 3: The material is broken up and measured. The material enters the breaking roller through the bottom of the cyclone and then enters the measuring bin for weighing.
[0009] Step 4: The weighed material enters the glue application pipeline, and the nozzle in the glue application pipeline applies atomized water-based glue. A moisture detector is installed in the metering bin to detect the moisture content of the material. If the moisture content is too much, it can be heated to remove the excess moisture before gluing; the material after gluing enters the second cyclone, and enters the sorting machine for impurity removal through the second cyclone. A fan and a heater are installed on one side of the sorting machine to remove impurities such as slag balls in the material. At the same time, the moisture content in the material can be detected by the moisture detector. If the moisture content is too much, the excess moisture can be removed by high-temperature heating of the heater; the material enters the third cyclone through the sorting machine;
[0010] Step five, the mixed material after spraying glue enters the paving mechanism through the third cyclone, is evenly paved into a slab, and is weighed; the paving mechanism can evenly spread the material, place good quality fibers on the surface layer, and poor quality fibers on the core layer; the principle is that the two layers of paving rollers are inclined with different inclination directions, the bottom of the upper paving roller is arranged above the lower paving roller, and a negative pressure fan is arranged above the paving roller. The limit weight of the better quality fibers is light, and they are adsorbed by the suction of the negative pressure fan during the paving process. The weight of the fibers with poor quality is heavy, and they are less adsorbed by the negative pressure fan, so they fall to the lower paving roller first, and the lighter fibers are more adsorbed, and they fall later, thereby realizing the above-mentioned layered laying function.
[0011] Step 6: pre-pressing the slab. The pre-pressing machine pre-presses the slab and heats it at the same time, controlling the degree of heating to remove excess moisture.
[0012] Step 7: Sheet forming: the sheet blank after removing metal impurities is transported to a continuous press for thermal curing and shaping;
[0013] Step 8: Remove defective products. After the defective products are removed, the plates are trimmed and the surface is polished before storage. The waste after polishing is recovered and can be recycled. The recycled waste can be melted at a high temperature of 1450 degrees and then recycled.
[0014] Optionally, step seven includes metal impurity removal, a first conveyor belt is provided at the front end of the continuous press, a second conveyor belt is provided at the rear end of the pre-press, and the pre-pressed slab can be transferred to the first conveyor belt via the second conveyor belt; an impurity storage box is provided below between the first conveyor belt and the second conveyor belt, a tensioning wheel and a support wheel are provided at one end of the second conveyor belt close to the first conveyor belt, and the support wheel can drive the end of the second conveyor belt to move downward; a metal detector is provided on the second conveyor belt.
[0015] Optionally, a fan is provided at one end of the glue application pipeline to increase the flow rate in the glue application pipeline; a moisture detector is provided at the glue application pipeline, and a heater is provided at one end of the glue application pipeline close to the fan, and the heater can heat 100°~120°; two universal glue mixing joints are provided between the glue application pipeline and the third cyclone, which can further mix the water-based glue and the material.
[0016] Optionally, in step 1, the length of the fibers after being crushed is 300um to 1500um.
[0017] Optionally, the pipeline in step one includes a corrugated pipe and an elbow pipe, a fan is provided at one end of the pipeline, and the other end of the pipeline is connected to a cyclone, and the cyclone is connected to a negative pressure fan and a bag dust collector; the nominal diameter of the pipeline is 150-200 mm, the glue application pipeline has the same structure as the pipeline, the pipeline diameter is small, the fan wind force is strong, and the corrugated inner wall structure in the pipeline makes the material flow rate in the pipeline fast, between 60m and 140m per second, and the material will not gather and block the pipeline.
[0018] Optionally, the water-based glue uses a water-soluble phenolic resin with a content of 40% to 50%.
[0019] Optionally, the moisture content of the material is detected and adjusted to a set range before paving the slab; in step six, the longitudinal edge of the slab is cut off before weighing the slab.
[0020] Optionally, the water-based glue is prepared by mixing MDI with 100% solid content and water in a ratio of 1:3.
[0021] The surface of the board is easily over-cured due to high temperature, with low strength and poor smoothness. After grinding off the 0.3-0.8mm over-cured layer, it is painted and laminated with melamine layer, PP film and aluminum skin.
[0022] In step 1, the content of water sprayed is 1-8% of the fiber raw material; the content of water repellent in water is 3‰-5%, which is sprayed on the surface of the material to make the board waterproof. Since the fiber is easy to clump, which affects the use, in order to avoid its agglomeration, a dispersant content of 1-5% and a coupling agent content of 3‰-1% are added, which can increase the bonding viscosity between glue and glue when spraying, and then increase the strength of the board when the board is cured.
[0023] Compared with the prior art, the present invention has achieved the following technical effects:
[0024] The present invention adopts water-based glue to make the board, which avoids the generation of glue powder, has high safety and saves cost; uses rock wool fiber to make the board, is pollution-free, can be recycled, and saves resources. The entire processing and manufacturing process adopts mechanical integration, which reduces the labor intensity of operators and has high work efficiency. After the board is sprayed with paint and film-laminated, a surface of various patterns can be formed, which is beautiful and durable. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0026] Figure 1 This is a schematic diagram of the process of manufacturing the rock wool decorative board of the present invention;
[0027] Figure 2 This is a schematic diagram of the pipeline structure of the present invention;
[0028] Explanation of the reference numerals: 1-cotton shredder, 2-nozzle, 3-pipeline, 4-cyclone, 5-fan, 6-negative pressure fan, 7-bag dust collector, 8-heater, 9-sorter, 10-breaking roller, 11-metering bin, 12-glue application pipeline, 13-universal glue mixing joint, 14-moisture detector, 15-paving mechanism, 16-edge saw, 17-pre-pressure steam heating system, 18-continuous press, 19-first conveyor belt, 20-second conveyor belt, 21-metal detector, 22-impurity storage box, 23-tensioning wheel, 24-support wheel, 25-bubble detection device, 26-double-sided grinding device, 27-cooling machine. DETAILED DESCRIPTION
[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] The purpose of the present invention is to provide a method for manufacturing rock wool decorative panels to solve the problems existing in the above-mentioned prior art. Water-based glue is used, which has low cost and does not produce powder during the gluing process, thereby avoiding waste and improving safety.
[0031] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0032] The present invention provides a method for manufacturing a rock wool decorative board, comprising the following steps:
[0033] Step 1: rock wool pretreatment. The rock wool after the initial breaking and crushing is transported to the cotton shredder 1 and crushed to the set length of the fiber and then transported to the pipeline 3. The fiber length after crushing is 300um-1500um. The pipeline 3 is provided with a nozzle 2. The pipeline water spraying method is used to spray water containing a hydrophobic agent, a dispersant, a wetting agent and a coupling agent, and the mixture is mixed. The content of the sprayed water is 1-8% of the fiber raw material amount; the content of the hydrophobic agent in the water is 3‰-5%, which is sprayed on the surface of the material to make the board waterproof. Since the fiber is easy to agglomerate, which affects the use, in order to avoid its agglomeration, a dispersant content of 1-5% and a coupling agent content of 3‰-1% are added, which can increase the bonding viscosity between the glue and the glue when spraying the glue, and then increase the strength of the board when the board is solidified; the wetting agent is sprayed to prevent the material from being too dry, which is convenient for transportation and mixing;
[0034] Step 2: The mixed material is transported to the cyclone 4 through the pipeline 3. A fan 5 is provided at one end of the pipeline 3. A negative pressure fan 6 is connected to one side of the cyclone 4. Under the high-pressure blowing force of the fan 5 and the suction action of the negative pressure fan 6, the crushed and water-sprayed mixed material can be transported to the cyclone 4. A bag dust collector 7 is provided on one side of the negative pressure fan 6, which can absorb smaller impurities such as rock wool debris. At the same time, the impurities in the bag dust collector 7 can be recycled, melted and reused to avoid waste, and then transported to the next step through the bottom of the cyclone 4;
[0035] Step 3: the material is broken up and measured. The material enters the breaking roller 10 through the bottom of the cyclone 4 and then enters the measuring bin 11 for weighing.
[0036] Step 4: The weighed material enters the glue application pipeline 12, and the nozzle in the glue application pipeline 12 applies atomized water-based glue. The water-based glue uses a water-soluble phenolic resin with a content of 40% to 50%; or the water-based glue is made of MDI with a solid content of 100% and water in a ratio of 1:3. MDI is a general term for diphenylmethane diisocyanate, a mixture containing a certain proportion of pure MDI and polyphenyl polymethylene polyisocyanate, and a modified product of pure MDI and polymerized MDI. A fan 5 is provided at one end of the glue application pipeline 12 to increase the flow rate in the glue application pipeline; a moisture detector 14 is provided at the glue application pipeline 12, and a heater 8 is provided at one end of the glue application pipeline 12 close to the fan 5. The heater 8 can heat 100° to 120° to remove excess moisture. Two universal glue mixing joints 13 are provided between the glue application pipeline 12 and the third cyclone 4 to further mix the water-based glue and the material. A moisture detector 14 is provided in the metering bin 11, which can detect the moisture content of the material. If the moisture content is too much, it can be heated to remove the excess moisture before gluing; the material after gluing enters the second cyclone 4, enters another breaking roller 10 through the second cyclone 4, and then enters the sorting machine 9. A fan 5 and a heater 8 are provided on one side of the sorting machine 9 to remove impurities such as slag balls in the material. At the same time, the moisture content in the material can be detected by the moisture detector 14. If the moisture content is too much, the heater 8 can be used to heat the excess moisture at high temperature to remove it. A bag dust collector 7 is provided on the other side of the sorting machine 9 to recover impurities; the impurity-removed material enters the third cyclone 4 through the sorting machine 9;
[0037] Step five, the mixed material after spraying glue enters the paving mechanism 15 through the third cyclone 4, is evenly paved into a slab, and is weighed; the paving mechanism 15 can evenly spread the material, place the fiber of good quality on the surface layer, and place the fiber of poor quality on the core layer; the principle is that the two layers of paving rollers of the paving mechanism 15 are both inclined with different inclination directions, the bottom end of the paving roller of the upper layer is arranged above the paving roller of the lower layer, and a negative pressure fan 6 is arranged above the paving roller. The limit weight of the fiber with better quality is light, and it is adsorbed by the suction of the negative pressure fan 6 during the paving process. The fiber with poor quality is heavy and is less adsorbed by the negative pressure fan 6. It falls to the paving roller of the lower layer first, and the lighter fiber is greatly adsorbed, and then falls, thereby realizing the above-mentioned layered laying function. Before paving the slab, the moisture content of the material needs to be detected by a moisture detector 14 and the moisture content needs to be adjusted to a set range; in order to ensure that the final size of the board is qualified, the paving slab is wider than the set board, and the longitudinal edge of the slab needs to be cut off by a trim saw 16 before weighing the paving slab to make its width within the set range;
[0038] Step 6, pre-pressing the slab, the pre-pressing machine of the pre-pressing steam heating system 17 pre-presses the slab, the pre-pressing machine can use the pressing rollers arranged up and down to realize the pre-pressing of the slab, and the steam engine is used to apply steam heating during the pre-pressing process, the steam penetrates from the bottom surface to the core layer, and then penetrates to the surface, increasing the temperature of the core layer, facilitating the curing of the core layer, and reducing the curing time; increasing the temperature of the core layer, facilitating the subsequent heating and curing;
[0039] Step seven, sheet forming, a first conveyor belt 19 is provided at the front end of the continuous press 18, a second conveyor belt 20 is provided at the rear end of the pre-press, a metal detector 21 is provided on the second conveyor belt 20, and the pre-pressed sheet can be transferred to the first conveyor belt 19 via the second conveyor belt 20; an impurity storage box 22 is provided below between the first conveyor belt 19 and the second conveyor belt 20, a tensioning wheel 23 and a supporting wheel 24 are provided at one end of the second conveyor belt 20 close to the first conveyor belt 19, the second conveyor belt 20 is sequentially wound around the supporting wheel 24 and the tensioning wheel 23, and is used to support the second conveyor belt 20, and the supporting wheel 24 can drive the end of the second conveyor belt 20 to move downward, so that the end of the second conveyor belt 20 is inclined The slab containing metal impurities can be transported to the impurity storage box 22 below, and the support wheel 24 moves upward, driving the second conveyor belt 20 to move to a horizontal position. At this time, the slab without metal impurities can be transferred to the first conveyor belt 19, and the slab after removing the metal impurities is transported to the continuous press 18. The continuous press 18 controls the heating temperature and removes excess moisture. The continuous press 18 is provided with two closed steel belts arranged symmetrically up and down. The slab is located between the two steel belts. The upper and lower steel belts squeeze the slab for thermal curing and shaping. The sheet forming process is connected to the bag dust collector at the paving step to recover the impurities and dust generated in the process to ensure the safety of the processing environment.
[0040] Step eight, rejecting defective products, trimming the boards after rejecting defective products, when the core layer curing quality is poor, the boards are prone to bubbling, so a bubbling detection device 25 is needed to detect whether the boards have bubbles, the bubbling detection device 25 can use an infrared detector or a level meter, etc., if there are bubbles, it will be set as a defective product to be rejected, the genuine boards without bubbles are cooled by the cooling machine 27, and then conveyed to the double-sided grinding device 26 to grind the upper and lower surfaces and then stored, the double-sided grinding device can use two grinding devices to grind the two sides of the board respectively, the ground material can be melted and reused after being recovered by the recovery device to avoid waste, the recovery device includes a cyclone 4, a negative pressure fan 6 and a bag dust collector 7, and the various components are used together to recover impurities generated during the grinding process; the surface of the board is prone to over-curing due to excessive temperature, low strength and poor smoothness, after grinding off the over-cured layer of 0.3 to 0.8 mm, it is painted, and the melamine layer, PP film and aluminum skin are attached.
[0041] Further preferably, Figure 2As shown, in step one, the pipeline 3 includes a corrugated pipe and an elbow pipe, a fan 5 is provided at one end of the pipeline 3, and the other end of the pipeline 3 is connected to a cyclone 4, and the cyclone 4 is connected to a negative pressure fan 6 and a bag dust collector 7; the nominal diameter of the pipeline 3 is 150-200 mm, the glue application pipeline 12 has the same structure as the pipeline 3, the diameter of the pipeline 3 is small, the wind force of the fan 5 is large, and the corrugated inner wall structure of the pipeline 3 makes the material flow rate in the pipeline 3 fast, between 60m and 140m per second, and the material will not gather and block the pipeline 3.
[0042] In the description of the present invention, it should be noted that the terms "center", "top", "bottom", "left", "right", "vertical", "horizontal", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, which are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.
[0043] The present invention uses specific examples to illustrate the principles and implementation methods of the present invention. The above examples are only used to help understand the method and core ideas of the present invention. At the same time, for those skilled in the art, according to the ideas of the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting the present invention.
Claims
1. A method for manufacturing a rock wool decorative board, characterized in that: The steps include: Step 1: rock wool pretreatment, the rock wool after the initial breaking and crushing is transported to the cotton shredder to be crushed into fibers of a set length and then transported to the pipeline. A nozzle is provided in the pipeline, and water containing a hydrophobic agent, a dispersant, a wetting agent and a coupling agent is sprayed and mixed by the pipeline water spraying method; Step 2: The mixed materials are transported to the cyclone through a pipeline and then transported to the next step through the bottom of the cyclone; Step 3: The material is broken up and measured. The material enters the breaking roller through the bottom of the cyclone to be broken up, and then enters the measuring bin for weighing; Step 4: the weighed material enters the glue application pipeline, and the nozzle in the glue application pipeline applies atomized water-based glue; then it enters the second cyclone, and enters the sorting machine through the second cyclone; after the impurities are removed by the sorting machine, it enters the third cyclone; Step 5, the mixed material after spraying glue enters the paving mechanism through the third cyclone, is evenly paved into a slab, and is weighed; Step 6: pre-pressing the slab, the pre-pressing machine pre-presses the slab and heats it at the same time; Step 7: Sheet forming: the sheet blank after removing metal impurities is transported to a continuous press for thermal curing and shaping; Step 8: Remove defective products. After the defective products are removed, the boards are trimmed and the surface is polished before storage.
2. The method for manufacturing a rock wool decorative board according to claim 1, characterized in that: Step seven includes metal impurity removal. A first conveyor belt is provided at the front end of the continuous press, and a second conveyor belt is provided at the rear end of the pre-press. The pre-pressed slab can be transferred to the first conveyor belt via the second conveyor belt. An impurity storage box is provided below between the first conveyor belt and the second conveyor belt. A tensioning wheel and a support wheel are provided at one end of the second conveyor belt close to the first conveyor belt. The support wheel can drive the end of the second conveyor belt to move downward. A metal detector is provided on the second conveyor belt.
3. The method for manufacturing a rock wool decorative board according to claim 1, characterized in that: After grinding off the over-cured layer of 0.3 to 0.8 mm on the surface of the board, it is sprayed with paint and the melamine layer is attached.
4. The method for manufacturing a rock wool decorative board according to claim 1, characterized in that: A fan is provided at one end of the glue application pipeline to increase the flow rate in the glue application pipeline; a moisture detector is provided at the glue application pipeline, and a heater is provided at one end of the glue application pipeline close to the fan, and the heater can heat 100°~120°. Two universal glue mixing joints are provided between the glue application pipeline and the third cyclone, which can further mix the water-based glue and the material.
5. The method for manufacturing a rock wool decorative board according to claim 1, characterized in that: In step 1, the length of the fiber after being broken is 300um to 1500um.
6. The method for manufacturing a rock wool decorative board according to claim 1, characterized in that: The pipeline in step one includes a corrugated pipe and an elbow pipe, a fan is provided at one end of the pipeline, and the other end of the pipeline is connected to a cyclone, and the cyclone is connected to a negative pressure fan and a bag dust collector; the nominal diameter of the pipeline is 150 to 200 mm, and the glue application pipeline has the same structure as the pipeline.
7. The method for manufacturing a rock wool decorative board according to claim 1, characterized in that: The water-based glue uses a water-soluble phenolic resin with a content of 40% to 50%.
8. The method for manufacturing a rock wool decorative board according to claim 1, characterized in that: Before paving the slab, the moisture content of the material is detected and adjusted to the set range; in step six, the longitudinal edge of the slab is cut off before weighing the slab.
9. The method for manufacturing a rock wool decorative board according to claim 1, characterized in that: The water-based glue is prepared by mixing MDI with a solid content of 100% and water in a ratio of 1:3.
Citation Information
Patent Citations
Inorganic fiber thermal insulation material and construction method
CN104926212A
Method for manufacturing fireproof density plate
CN110341216A
Manufacturing method of enhanced ultra-high density fiberboard
CN117021280A
Rock wool fiber board and preparation method thereof
CN117700152A
Woody fiber board producing process
CN1887549A