Hydrophobic composite material as well as preparation method and application thereof
By using electrospinning technology to prepare thermoplastic polyurethane/titanium dioxide/cetyltrimethoxysilane composite nanofiber membranes in functional wearable fabrics, the problems of fabric surface contamination and insufficient performance are solved, and efficient hydrophobic, UV protection and breathability improve the overall performance and use experience of the fabric.
Patent Information
- Application Number
- CN202411000796.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-01
AI Technical Summary
The surface of functional wearable fabrics is easily infiltrated by sweat or secretions, leading to pollution and bacterial growth. Existing superhydrophobic materials cannot have good UV protection, breathability and antifouling properties, affecting the user experience.
A hydrophobic composite material including a fiber membrane and microspheres embedded in the fiber membrane is used. It is composed of a mixture of thermoplastic polyurethane, titanium dioxide and cetyltrimethoxysilane. The nanofiber membrane is formed through electrospinning technology to realize the integration of microspheres and fibers. The coexisting structure enhances the hydrophobic, UV-resistant and breathable properties of the material.
It improves the super-hydrophobicity, UV resistance and breathability of the material, enhances the mechanical properties and chemical stability, significantly improves the anti-fouling performance and usage experience of the fabric, and is suitable for a variety of application scenarios.
Smart Images

Figure CN118727265A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hydrophobic materials, and in particular relates to a hydrophobic composite material and a preparation method and application thereof. Background Art
[0002] With the development of science and technology, the application field of functional wearable fabrics has expanded rapidly, but functional wearable fabrics still face the problem of surface contamination. Sweat or secretions produced on the skin surface can easily infiltrate fabrics, breed bacteria, and contaminate the fabric surface. In order to reduce the occurrence of this situation, researchers combine functional fabrics with superhydrophobic materials. Superhydrophobic materials are materials that repel water. They refer to functional materials with a static contact angle of water droplets on a solid surface greater than 150° and a rolling angle less than 10°. The traditional methods for preparing superhydrophobic materials mainly include template method, spraying method, etching method, phase separation method, gas phase sublimation and deposition method. With the rapid development of microscopic imaging and micro-nano manufacturing technology, inspired by the superhydrophobic structure of the lotus leaf surface in nature, two new methods for preparing superhydrophobic materials have been studied: one is to construct a suitable micro-nano rough structure on the surface of the hydrophobic material, and the other is to coat the rough surface with low surface energy substances. The superhydrophobic material prepared according to the existing method has good oil-water separation performance, and its contact angle is 150-170°. However, the existing hydrophobic material cannot have good UV protection, breathability and anti-fouling properties, and has a poor experience when used in functional wearable fabrics. Summary of the invention
[0003] In view of this, the present invention provides a hydrophobic composite material and a preparation method and application thereof. The hydrophobic composite material provided by the present invention not only has super hydrophobic properties, but also has excellent UV protection, air permeability and anti-fouling properties. It can be used in functional wearable fabrics to enhance the wearing experience.
[0004] In order to solve the above technical problems, the present invention provides a hydrophobic composite material, including a fiber membrane and microspheres embedded in the fiber membrane;
[0005] The fiber membrane and microspheres are respectively composed of a mixture of thermoplastic polyurethane, titanium dioxide and hexadecyltrimethoxysilane.
[0006] Preferably, the average diameter of the microspheres is 0.5 to 1.9 μm;
[0007] The mass percentage of the microspheres in the hydrophobic composite material is 40-75%.
[0008] Preferably, the diameter of the fibers in the fiber membrane is 100 to 300 nm.
[0009] Preferably, the mass ratio of the thermoplastic polyurethane to titanium dioxide is 6-12:0.5-1.5;
[0010] The mass ratio of the thermoplastic polyurethane to hexadecyltrimethoxysilane is 6-12:2.5-3.5.
[0011] The present invention also provides a method for preparing the hydrophobic composite material described in the above technical solution, comprising the following steps:
[0012] Firstly mixing titanium dioxide, hexadecyltrimethoxysilane and an organic solvent to obtain a dispersion; the organic solvent is a mixed solvent of N,N-dimethylformamide and tetrahydrofuran;
[0013] secondly mixing the dispersion and thermoplastic polyurethane to obtain a spinning solution;
[0014] The spinning solution is used for electrostatic spinning to obtain the hydrophobic composite material; the voltage of the electrostatic spinning is 8-16 kV; the ambient temperature of the electrostatic spinning is 18-30° C., and the relative humidity is 45-65%.
[0015] Preferably, the receiving distance of the electrospinning is 15 to 18 cm, the spinning rate is 0.6 to 1.2 mL / h, and the rotation speed of the drum is 50 to 120 r / min.
[0016] Preferably, the titanium dioxide is titanium dioxide nanoparticles, and the average particle size of the titanium dioxide nanoparticles is 5 to 10 nm;
[0017] The volume ratio of N,N-dimethylformamide to tetrahydrofuran in the organic solvent is 1:1-4;
[0018] The first mixing is performed under ultrasonic conditions, the power of the ultrasound is 300-400W, the frequency of the ultrasound is 35-45kHz, and the time is 1.5-2.5h.
[0019] Preferably, the thermoplastic polyurethane is thermoplastic polyurethane particles, and the average particle size of the thermoplastic polyurethane particles is 1.8 to 2.2 mm;
[0020] The second mixing is performed under stirring conditions, the stirring is magnetic stirring, and the stirring time is 5 to 7 hours.
[0021] Preferably, the mass percentage of thermoplastic polyurethane in the spinning solution is 6-12%, the mass percentage of titanium dioxide is 0.5-1.5%, and the mass percentage of hexadecyltrimethoxysilane is 2.5-3.5%.
[0022] The present invention also provides the use of the hydrophobic composite material described in the above technical solution or the hydrophobic composite material prepared by the preparation method described in the above technical solution as a super-hydrophobic film.
[0023] The present invention provides a hydrophobic composite material, comprising a fiber membrane and microspheres embedded in the fiber membrane; the components of the fiber membrane and the microspheres are respectively a mixture of thermoplastic polyurethane, titanium dioxide and hexadecyltrimethoxysilane. The structure of the coexistence of microspheres and fibers in the hydrophobic composite material of the present invention plays a key role in improving the performance of the material. First, thermoplastic polyurethane (TPU) provides basic elasticity and plasticity, which makes the hydrophobic composite material have good deformation ability. TiO 2 Nano-microspheres enhance the mechanical strength and durability of the material, and at the same time, due to their high refractive index and ultraviolet absorption characteristics, they give the hydrophobic composite material excellent anti-ultraviolet performance. The morphology of nanofibers is conducive to the formation of a porous structure, which increases the surface area of the material while also allowing the surface to have more voids, thereby improving the hydrophobicity and air permeability of the material. The addition of hexadecyltrimethoxysilane (HDTMS) further enhances the hydrophobicity. HDTMS is a hydrophobic silane coupling agent that can form a hydrophobic layer on the surface of the fiber and microspheres. This hydrophobic layer makes it difficult for water molecules to adhere to the surface of the material, thereby significantly improving the super hydrophobicity and anti-fouling properties of the hydrophobic composite material. The TPU / TiO 2 The / HDTMS composite nanofiber membrane material achieves a synergistic enhancement of deformation ability, superhydrophobicity and UV resistance through its unique coexistence structure of microspheres and fibers. This structure and combination not only improves mechanical properties and chemical stability, but also optimizes its surface properties through nano-level surface engineering, making it perform well in a variety of application scenarios.
[0024] The present invention also provides a method for preparing the hydrophobic composite material described in the above technical solution, comprising the following steps: first mixing titanium dioxide, hexadecyltrimethoxysilane and an organic solvent to obtain a dispersion; the organic solvent is a mixed solvent of N,N-dimethylformamide and tetrahydrofuran; second mixing the dispersion and thermoplastic polyurethane to obtain a spinning solution; using the spinning solution for electrostatic spinning to obtain the hydrophobic composite material; the voltage of the electrostatic spinning is 8 to 16 kV; the ambient temperature of the electrostatic spinning is 18 to 30 ° C, and the relative humidity is 45 to 65%. The present invention uses electrostatic spinning technology to form a phenomenon in which microspheres and fiber structures coexist in nanofiber membranes, which is mainly attributed to the characteristics of the spinning solution and the parameter control during the spinning process. In electrostatic spinning, high voltage causes the solution containing polymers to spray out filaments, and the rapid volatilization of the solvent leads to the formation of polymer fibers. If the viscosity of the solution is low or the surface tension is small, or the voltage is low and the flow rate is high during the spinning process, the Coulomb repulsion of the charged droplets is slightly greater than their surface tension, and a special structure (beaded structure) of spindle-shaped or round microspheres and fibers coexisting will be produced. After the solution is squeezed out of the needle and before it reaches the receiving plate, the beaded or microsphere solvent formed by the solution under the stretching of the electric field under the specific conditions specified in the present invention is solidified after the solvent evaporates, so this structure can stably exist in the fiber membrane finally formed. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 Schematic diagram of the process of preparing a hydrophobic composite material, wherein A is a schematic diagram of the process of preparing a spinning solution, and B is a schematic diagram of the process of electrospinning;
[0026] Figure 2 TPU / TiO 2 Schematic diagram of the multifunctionality of / HDTMS composite membrane;
[0027] Figure 3 The SEM images, fiber diameter distribution and particle size distribution of the materials prepared in Example 1 and Comparative Examples 1-2 are shown in Figure 1, where (a) is a 5000x FE-SEM image of pure TPU nanofiber membrane; (b) is a 5000x FE-SEM image of TPU / TiO 2 1500 times FE-SEM image of composite nanofiber membrane; (c) TPU / TiO 2 200 times FE-SEM image of the / HDTMS composite nanofiber membrane; (d) is the fiber diameter distribution and fitting curve of the pure TPU nanofiber membrane; (e) is the TPU / TiO 2 Fiber diameter distribution and fitting curve of composite nanofiber membrane; (f) TPU / TiO 2 / HDTMS composite membrane fiber diameter distribution and fitting curve; (g) TPU / TiO 2Microsphere diameter distribution and fitting curve in composite film; (h) TPU / TiO 2 / HDTMS composite film microsphere diameter distribution and fitting curve; (i) TPU / TiO 2 Schematic diagram of the super-hydrophobic structure of / HDTMS composite membrane;
[0028] Figure 4 The infrared spectra of the film materials prepared in Example 1 and Comparative Examples 1-2, wherein (a) is the FTIR spectrum and (b) is the Raman spectrum;
[0029] Figure 5 The XRD spectra of the membrane materials prepared in Example 1 and Comparative Examples 1-2 are shown;
[0030] Figure 6 The TPU / TiO prepared in Example 1 2 / XPS graph of HDTMS;
[0031] Figure 7 The TPU / TiO prepared in Example 1 2 / HDTMS thermolysis weight loss analysis results;
[0032] Figure 8 The TPU / TiO prepared in Example 1 2 DSC curves of the / HDTMS composite nanofiber membrane and the pure TPU membrane prepared in Comparative Example 1;
[0033] Fig. 9 The TPU / TiO prepared in Example 1 2 / HDTMS isothermal adsorption and desorption results, where (a) is the isothermal adsorption and desorption curve, (b) is the cumulative pore volume diagram, (c) is the surface structure diagram, and (d) is the three-dimensional morphology diagram;
[0034] Fig.10 The hydrophobicity test results are shown in Figure 1, where (a) is TPU / TiO 2 Photos of different droplets on the surface of TPU / TiO / HDTMS composite nanofiber membranes. (b) and (c) are photos of different droplets on the surface of TPU / TiO / HDTMS composite nanofiber membranes. 2 The appearance of the / HDTMS composite nanofiber membrane forced into water, (d) TPU / TiO 2 FE-SEM images and static contact angle images of the / HDTMS composite nanofiber membrane, (e) and (f) are pure TPU membrane and TPU / TiO 2 The contact angle diagram of the composite nanofiber membrane with time (g) is TPU / TiO 2 Sliding angle test diagram of / HDTMS composite nanofiber membrane;
[0035] Fig.11 TPU / TiO 2 / HDTMS composite nanofiber membrane water droplet adhesion behavior test results;
[0036] Fig.12 TPU / TiO 2 / HDTMS composite nanofiber membrane anti-pollution performance test results;
[0037] Fig.13 For pure TPU film and TPU / TiO 2 / HDTMS composite nanofiber membrane stress-strain curve;
[0038] Fig.14 TPU / TiO 2 Schematic diagram of the anti-ultraviolet and self-cleaning principle of / HDTMS composite film;
[0039] Fig.15 It is a columnar comparison chart of the moisture permeability and air permeability of the membrane materials prepared in Example 1 and Comparative Examples 1-2. DETAILED DESCRIPTION
[0040] The present invention provides a hydrophobic composite material, comprising a fiber membrane and microspheres embedded in the fiber membrane;
[0041] The fiber membrane and microspheres are respectively composed of a mixture of thermoplastic polyurethane, titanium dioxide and hexadecyltrimethoxysilane.
[0042] The hydrophobic composite material provided by the present invention includes a fiber membrane. In the present invention, the diameter of the fiber in the fiber membrane is preferably 100 to 300 nm, and more preferably 179.28 nm. In the present invention, the component of the fiber membrane is a mixture of thermoplastic polyurethane, titanium dioxide and hexadecyltrimethoxysilane; the mass ratio of the thermoplastic polyurethane to titanium dioxide is preferably 6 to 12: 0.5 to 1.5, and more preferably 8 to 10: 1; the mass ratio of the thermoplastic polyurethane to hexadecyltrimethoxysilane is preferably 6 to 12: 2.5 to 3.5, and more preferably 8 to 10: 3.
[0043] The hydrophobic composite material provided by the present invention also includes microspheres embedded in the fiber membrane. In the present invention, the components of the microspheres are a mixture of thermoplastic polyurethane, titanium dioxide and hexadecyltrimethoxysilane; the mass ratio of the thermoplastic polyurethane and titanium dioxide is preferably 6 to 12:0.5 to 1.5, more preferably 8 to 10:1; the mass ratio of the thermoplastic polyurethane and hexadecyltrimethoxysilane is preferably 6 to 12:2.5 to 3.5, more preferably 8 to 10:3. In the present invention, the average diameter of the microspheres is preferably 0.5 to 1.9 μm, more preferably 1.5 to 1.75 μm. In the present invention, the mass percentage of the microspheres in the hydrophobic composite material is preferably 40 to 75%, more preferably 46 to 65%.
[0044] In the present invention, the hydrophobic composite material contains an irregular pore structure, and the average pore size of the pore structure in the hydrophobic composite material is preferably 2 to 25 nm, more preferably 10.31 to 15 nm; the specific surface area of the hydrophobic composite material is preferably 0.5 to 3 m 2 / g, more preferably 1.339 to 2m 2 / g; the surface energy of the hydrophobic composite material is preferably <25mN / m, more preferably 9.18mN / m.
[0045] The present invention also provides a method for preparing the hydrophobic composite material described in the above technical solution, comprising the following steps:
[0046] Firstly mixing titanium dioxide, hexadecyltrimethoxysilane and an organic solvent to obtain a dispersion; the organic solvent is a mixed solvent of N,N-dimethylformamide and tetrahydrofuran;
[0047] secondly mixing the dispersion and thermoplastic polyurethane to obtain a spinning solution;
[0048] The spinning solution is used for electrostatic spinning to obtain the hydrophobic composite material; the voltage of the electrostatic spinning is 8-16 kV; the ambient temperature of the electrostatic spinning is 18-30° C., and the relative humidity is 45-65%.
[0049] The present invention first mixes titanium dioxide, hexadecyltrimethoxysilane and an organic solvent to obtain a dispersion. In the present invention, the titanium dioxide is preferably titanium dioxide nanoparticles, and the average particle size of the titanium dioxide nanoparticles is preferably 5 to 10 nm, more preferably 6 to 8 nm. In the present invention, the molecular formula of the hexadecyltrimethoxysilane is C 19 H 42 SiO 3 , molecular weight is 364.62, and it is a colorless liquid. In the present invention, the purity of the hexadecyltrimethoxysilane is preferably ≥85%, more preferably 90-95%.
[0050] In the present invention, the organic solvent is a mixed solvent of N,N-dimethylformamide (DMF) and tetrahydrofuran (THF); the volume ratio of N,N-dimethylformamide to tetrahydrofuran in the organic solvent is preferably 1:1-4, more preferably 1:2-4, and further preferably 1:4. In the present invention, the organic solvent has a small surface energy and a volatilization rate suitable for the production of TPU / TiO 2 Fiber-microsphere structure of / HDTMS composite membrane.
[0051] In the present invention, the first mixing is preferably carried out under ultrasonic conditions, the power of the ultrasound is preferably 300-400 W, more preferably 360 W; the frequency of the ultrasound is preferably 35-45 kHz, more preferably 40 kHz; the time of the ultrasound is preferably 1.5-2.5 h, more preferably 2 h.
[0052] After obtaining the dispersion, the present invention secondly mixes the dispersion and thermoplastic polyurethane to obtain a spinning solution. In the present invention, the thermoplastic polyurethane is preferably thermoplastic polyurethane particles, and the average particle size of the thermoplastic polyurethane particles is preferably 1.8 to 2.2 mm, more preferably 2 mm; the molecular weight of the thermoplastic polyurethane is preferably 100K. In the present invention, the thermoplastic polyurethane particles are preferably spindle-shaped transparent particles.
[0053] In the present invention, the second mixing is preferably carried out under stirring conditions, and the stirring is preferably magnetic stirring; the stirring time is preferably 5 to 7 hours, more preferably 6 hours; the present invention has no special requirements on the stirring speed, as long as the thermoplastic polyurethane can be completely dissolved.
[0054] In the present invention, the mass percentage of thermoplastic polyurethane in the spinning solution is preferably 6-12%, more preferably 8-10%; the mass percentage of titanium dioxide is preferably 0.5-1.5%, more preferably 1%; the mass percentage of hexadecyltrimethoxysilane is preferably 2.5-3.5%, more preferably 3%.
[0055] In the present invention, the viscosity of the spinning solution is determined by the concentration of thermoplastic polyurethane in the solution, the solubility of the organic solvent, and the ambient temperature. When the concentration of thermoplastic polyurethane increases, the interaction between thermoplastic polyurethane molecules in the solution is enhanced, resulting in an increase in the overall viscosity of the solution. High-concentration thermoplastic polyurethane solutions are usually more viscous because the entanglement and interaction between molecular chains are more significant. The solvent's ability to dissolve the polymer directly affects the degree of dispersion of the polymer molecules in the solvent. Solvents with good solubility can more effectively disperse polymer molecules, reduce intermolecular aggregation and interaction, and thus reduce viscosity. If the solubility is insufficient, polymer molecules may form local aggregations, thereby increasing viscosity. An increase in ambient temperature usually leads to a decrease in the viscosity of the polymer solution because high temperature increases the thermal motion of the molecules and reduces the mutual attraction between the molecules. In the present invention, the conductivity of the spinning solution is mainly affected by the ion concentration in the solution and the TiO 2 The present invention can ensure that the viscosity and conductivity of the spinning solution are conducive to spinning by limiting the concentration of thermoplastic polyurethane in the spinning solution, the type of organic solvent, and the temperature and relative humidity of the spinning environment.
[0056] After obtaining the spinning solution, the present invention uses the spinning solution for electrostatic spinning to obtain the hydrophobic composite material. In the present invention, the voltage of the electrostatic spinning is 8 to 16 kV, preferably 10 to 15 kV; the ambient temperature of the electrostatic spinning is 18 to 30 ° C, preferably 20 to 25 ° C; the relative humidity of the electrostatic spinning environment is 45 to 65%, preferably 50 to 60%. In the present invention, the receiving distance of the electrostatic spinning is preferably 15 to 18 cm, more preferably 16 to 17 cm; the spinning rate of the electrostatic spinning is preferably 0.6 to 1.2 mL / h, more preferably 0.8 to 1 mL / h; the rotation speed of the electrostatic spinning drum is preferably 50 to 120 r / min, more preferably 100 r / min.
[0057] The preparation method provided by the present invention is simple and easy to operate. The nanofiber membrane with microspheres is prepared by controlling the voltage, ambient temperature and relative humidity, thereby realizing a structure in which microspheres and nanofibers coexist. The TPU / TiO 2 / HDTMS composite nanofiber membrane has the characteristics of low surface energy and high roughness.
[0058] Figure 1 Schematic diagram of the process for preparing hydrophobic composite materials. Figure 1 A is a schematic diagram of the process of preparing the spinning solution, specifically, titanium dioxide nanoparticles are dispersed in a mixed solvent of N,N-dimethylformamide and tetrahydrofuran with a volume ratio of 1:4, and then hexadecyltrimethoxysilane is dropped into it, ultrasonically treated, and then thermoplastic polyurethane is added and stirred to obtain the spinning solution. Figure 1 Figure B is a schematic diagram of the electrospinning process, which specifically involves filling 5 mL of spinning solution into a syringe, connecting the positive electrode of a high-voltage power supply to a metal needle (with an inner diameter of 0.4 mm) of a syringe containing the spinning solution, and covering the drum collector with a layer of tin foil for electrospinning.
[0059] The present invention adopts electrospinning technology to prepare a new type of TPU / TiO 2 / HDTMS composite nanofiber membrane. This method is simple and easy to operate, with low cost, and is very suitable for large-scale production at room temperature. The core advantage of the electrospinning method lies in its simplicity and environmental friendliness. The raw materials used are all environmentally friendly materials, which are not only beneficial to environmental protection, but also reduce the potential risks in the production process. In addition, the prepared composite nanofiber membrane has excellent deformation ability and can adapt to various use environments and needs. In particular, the composite membrane material also has super hydrophobicity and excellent UV resistance, especially in outdoor protection applications. It has significant advantages, such as covering materials for protective clothing and outdoor equipment, which effectively extends its service life and provides continuous protection. The development of this technology not only promotes innovation and functionality in the field of materials, but also proposes a cost-effective and efficient solution strategy, opening up new development prospects for related application fields.
[0060] In the present invention, Figure 2 TPU / TiO 2 Schematic diagram of the multifunctional / HDTMS composite membrane. Figure 2 It can be seen that TPU / TiO 2 / HDTMS composite film has excellent UV resistance, super hydrophobicity, moisture permeability and air permeability.
[0061] The present invention also provides the use of the hydrophobic composite material described in the above technical solution or the hydrophobic composite material prepared by the preparation method described in the above technical solution as a super hydrophobic film. In the present invention, the super hydrophobic film is preferably used in functional wearable fabrics.
[0062] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0063] The sources of the raw materials used in the examples are as follows: thermoplastic polyurethane particles (TPU 1185K) with a molecular weight of 100K, transparent particles, purchased from BASF, Germany; titanium dioxide nanoparticles (TiO 2NPs) with a particle size of 5 nm, analytical grade, purchased from MacLean; hexadecyltrimethoxysilane with a purity of 90% was purchased from MacLean; N,N-dimethylformamide (DMF) with analytical grade was purchased from Tianjin Fuyu Fine Chemical Co., Ltd.; tetrahydrofuran (THF) with analytical grade was purchased from Tianjin Fuyu Fine Chemical Co., Ltd.
[0064] Example 1
[0065] Titanium dioxide nanoparticles with a particle size of 5 nm, hexadecyltrimethoxysilane, and a mixed solvent of N,N-dimethylformamide and tetrahydrofuran (the volume ratio of N,N-dimethylformamide to tetrahydrofuran is 1:4) are ultrasonicated for 2 h at a power of 360 W and a frequency of 40 kHz to obtain a dispersion;
[0066] Thermoplastic polyurethane particles with an average particle size of 2 mm and a molecular weight of 100K and a dispersion are mixed and stirred for 6 hours under magnetic stirring to obtain a spinning solution; the mass percentage of titanium dioxide in the spinning solution is 1wt%, the mass percentage of hexadecyltrimethoxysilane is 3wt%, and the mass percentage of thermoplastic polyurethane is 10wt%;
[0067] The spinning solution was filled into a syringe, and the positive electrode of the high-voltage power supply was connected to the metal needle (with an inner diameter of 0.4 mm) of the syringe needle tube containing the spinning solution. A layer of tin foil was covered on the drum collector for electrospinning to obtain a hydrophobic composite material, which was recorded as TPU / TiO 2 / HDTMS; the spinning voltage was 15 kV, the receiving distance was 15 cm, the spinning rate was 0.8 mL / h, the rotation speed of the drum was 100 r / min, the ambient temperature was 25° C., and the relative humidity was 50±5%.
[0068] Comparative Example 1
[0069] Thermoplastic polyurethane particles with an average particle size of 2 mm were magnetically stirred in a mixed solvent of N,N-dimethylformamide and tetrahydrofuran (the volume ratio of N,N-dimethylformamide to tetrahydrofuran was 1:4) for 6 hours to obtain a spinning solution;
[0070] Electrospinning was performed using the spinning solution according to the method of Example 1 to obtain a fiber membrane material, which was recorded as TPU.
[0071] Comparative Example 2
[0072] Titanium dioxide nanoparticles with an average particle size of 8 nm and a mixed solvent of N,N-dimethylformamide and tetrahydrofuran (the volume ratio of N,N-dimethylformamide and tetrahydrofuran is 1:4) are ultrasonically treated at a power of 360 W and a frequency of 40 kHz for 2 hours, and then thermoplastic polyurethane particles with an average particle size of 2 mm are added, and stirred for 6 hours under magnetic stirring to obtain a spinning solution; the mass percentage of titanium dioxide in the spinning solution is 1wt%, and the mass percentage of thermoplastic polyurethane is 10wt%;
[0073] According to the method of Example 1, electrospinning was performed using the spinning solution to obtain a fiber membrane material, which was recorded as TPU / TiO 2 .
[0074] The performance of the materials prepared in Example 1 and Comparative Examples 1-2 was tested according to the following method:
[0075] 1. The surface microstructure of the nanofiber membrane was observed using a field emission scanning electron microscope (FE-SEM, sigma500, Germany). It is worth noting that the sample needs to be treated with gold spraying before observation. The diameters of 100 fibers were randomly selected for measurement using ImageJ software, and Origin software was used to draw the graph to obtain the SEM image, fiber diameter distribution map and particle size distribution map, as shown in Figure 1. Figure 3 As shown, (a), (b) and (c) are TPU, TPU / TiO 2 、TPU / TiO 2 FE-SEM images of (d), (e) and (f) are TPU, TPU / TiO 2 、TPU / TiO 2 Distribution diagram of fiber diameter in / HDTMS, (g) and (h) are TPU / TiO 2 、TPU / TiO 2 / Distribution diagram of the diameter of microspheres on the HDTMS surface. Figure 3 It can be seen from (a), (b) and (c) that the distribution of nanofiber diameters of pure TPU film has a high consistency, indicating that TPU, TiO 2 The components such as TPU / TiO2 and HDTMS are highly evenly mixed in the spinning solution. 2 The surface of the composite nanofiber membrane has more fibers and a small amount of microspheres, which do not completely cover the membrane surface. 2 Fibers and microspheres coexist on the surface of the / HDTMS composite nanofiber membrane, and the microspheres cover the entire surface.
[0076] Depend on Figure 3From (d), (e) and (f), it can be seen that the average diameter of the nanofibers in the pure TPU film is 481 nm, and the distribution range is between 300 and 800 nm. 2 The average diameter of the surface fibers of the composite nanofiber membrane is 313 nm, and the distribution range is between 100 and 500 nm. 2 The fiber diameter of the / HDTMS composite nanofiber membrane is 179.28 nm, and the fiber diameter distribution is between 100 and 300 nm. 2 With the addition of HDTMS, the fiber diameter gradually decreased, the pore size of the membrane became smaller, and the porosity became larger.
[0077] Depend on Figure 3 As can be seen from (g) and (h), TPU / TiO 2 The average diameter of microspheres in the composite nanofiber membrane is 2.78 μm. 2 The average diameter of microspheres in the TPU / TiO / HDTMS composite nanofiber membrane is 1.75 μm. 2 / HDTMS composite nanofiber membrane surface microsphere diameter is much smaller than TPU / TiO 2 The diameter of microspheres on the surface of the composite nanofiber membrane. This indicates that TPU / TiO 2 The presence of this micro-nano rough structure on the surface of the HDTMS composite nanofiber membrane significantly increases the roughness of the fiber membrane surface, and thus further enhances the hydrophobic properties of the nanofiber membrane.
[0078] Figure 3 (i) is TPU / TiO 2 Schematic diagram of the super-hydrophobic structure of the TPU / TiO composite film. The coexistence of fibers and microspheres in the rough structure increases the air in the film, and the low surface energy of the fibers and microspheres makes the TPU / TiO 2 / HDTMS composite film achieves super hydrophobic effect.
[0079] 2. The chemical composition of the membrane materials prepared in Example 1 and Comparative Examples 1 to 2 was analyzed by Fourier transform infrared spectrometer (FTIR, Bruker Tensor 37, Germany) and Raman spectrometer (Raman, Horiba-Lab RAM HR Evolution, Japan) to obtain infrared spectra, as shown in FIG. Figure 4 As shown, (a) is the FTIR spectrum and (b) is the Raman spectrum. Figure 4 From (a), we can see that 1230cm -1 The peak at represents the O-Ti-O bond angle vibration, which is the TiO 2An important characteristic peak in the infrared spectrum, the position and intensity of this peak are also affected by the crystal structure and coordination conditions. 2 The existence of. At 771cm -1 The characteristic absorption peaks observed at 2852 cm-1 are attributed to the antisymmetric and symmetric stretching vibrations of the Si-OC group, thus verifying the existence of HDTMS. -1 and 2927cm -1 The absorption peaks at 1 and 2 represent the -CH 3 and -CH 2 The asymmetric and symmetric stretching vibrations of the membrane significantly improve its hydrophobicity. -1 and 1732cm -1 The absorption peaks at 3350cm -1 The absorption peak near indicates the stretching vibration of the aliphatic -NH group in TPU. Figure 4 From the analysis in (b), we can see that at 144cm -1 、399cm -1 、514cm -1 and 635cm -1 The observation of the characteristic peak at 2 The crystal form is anatase.
[0080] 3. The crystallization behavior of the fiber membrane was investigated using an X-ray polycrystalline diffractometer (XRD, Rigaku-SmartLab SE, Japan) to obtain the XRD spectrum, such as Figure 5 As shown. Figure 5 It can be seen that a wide diffraction peak appears at a diffraction angle of about 20° in the test results of TPU, which indicates that the crystal area of the TPU soft segment is small and the crystal integrity is not high, resulting in TPU having lower hardness and good elasticity and flexibility. 2 In the XRD spectrum of the / HDTMS composite film, obvious diffraction peaks appear at diffraction angles 2θ of 16.7°, 24.8°, 44.5°, and 64.9°, which correspond to the anatase nano-TiO 2 With the TiO 2 With the addition of TiO 2The uneven dispersion of HDTMS affects the polymer chain arrangement and crystal formation behavior inside the material. The uneven distribution may make it difficult for the polymer chains in the local area to form an ordered crystal structure, which in turn leads to a decrease in the overall crystallinity of the composite film, an increase in the amorphous area, and a decrease in the hardness of the material. At the same time, the toughness and impact resistance of the material are improved.
[0081] 4. X-ray photoelectron spectrometer (XPS, Thermo Fisher Scientific-ESCALAB250Xi, USA) was used to analyze the TPU / TiO prepared in Example 1 using an Al target. 2 / HDTMS surface element information is accurately analyzed to obtain XPS graphs, such as Figure 6 A 3D optical profiler (Bruker Contour GT-K, Germany) was used to characterize the roughness and 3D morphology of the film surface. Figure 6 The functional groups of C1s, O1s and Si2p are shown in the figure. The C1s spectrum consists of C-Si (284.2eV), CC (285eV), CONH (285.3eV) and CO (286.3eV) signals. The peak at 530.6eV is due to the presence of OH, and the peaks at 531.8eV, 532.5eV and 533.3eV belong to CONH, Si-OC and OCOO, respectively. The Si-OC peak is located at 102.33eV. From XPS, it can be seen that TiO 2 The addition of HDTMS is just physical mixing and does not generate new chemical bonds, which is consistent with the infrared results.
[0082] 5. The TPU / TiO prepared in Example 1 was analyzed by a thermogravimetric analyzer (TG, 209F1Iris, Germany). 2 The thermal stability and composition of HDTMS during pyrolysis weight loss were studied. The sample mass was between 3 and 6 mg and placed in an 80 μL NETZSCH ceramic crucible. The sample was heated to 500°C at a heating rate of 10°C / min under a nitrogen atmosphere. The thermal weight loss (TG) curve and differential thermal weight loss (DTG) curve were obtained as shown in Figure 2. Figure 7As shown. According to the TG and DTG curves, in the initial stage of heating, the thermal gravimetric differential curve (DTG) shows a fluctuating characteristic. The main components of the sample begin to decompose at 218°C, and at 372°C, the decomposition rate reaches a maximum value, and then the decomposition rate decreases. At 426°C, the decomposition rate is relatively slow, and then the decomposition rate gradually increases. At 485°C, the decomposition rate reaches a small peak during the second accelerated decomposition process, and then gradually decreases. At room temperature to 218°C, the ups and downs of the curve may be caused by the difference in the decomposition rates of different components in the composite film and the volatilization of a small amount of THF and water. At 218-262°C, water and a small amount of THF are completely volatilized. At 262-426°C, it is the decomposition process of the main components such as HDTMS and TPU, and the mass loss is fastest at 372°C. At 426°C, TiO 2 Begins to decompose, at 485℃ TiO 2 The decomposition rate reaches the maximum. These components have different decomposition rates. For example, THF evaporates faster, while HDTMS decomposes relatively slowly. At a specific temperature point, the decomposition rate of HDTMS may reach the maximum. As the heating process proceeds, the organic components in HDTMS will decompose or volatilize, among which -OCH 3 The melting or softening of TPU may be accompanied by the volatilization of solvent or water and the chemical decomposition of HDTMS. The overlap of these processes may be manifested in the DTG curve as multiple rising and falling fluctuations between room temperature and 218°C.
[0083] 6. The TPU / TiO prepared in Example 1 was quantified using a differential scanning calorimeter (DSC, TA Discovery 25, USA). 2 / HDTMS and the pure TPU film prepared in Example 1 were tested to explore the thermal properties and phase change characteristics of the material. The temperature was raised to 170°C at 10°C / min, maintained for 1 min, then dropped to 40°C at 10°C / min, and then raised to 170°C again to ensure the accuracy of the experiment. The obtained TPU / TiO 2 The differential scanning calorimetry (DSC) curves of the / HDTMS composite nanofiber membrane and the pure TPU membrane are shown in Figure 8 As shown in the figure, although the exothermic peak of pure TPU film at 95.27℃ exists, it is not significant. The reason may be that TPU itself is a thermoplastic polyurethane with specific crystallization properties. When the temperature reaches 95.27℃, the TPU molecular chains will rearrange to form a more ordered structure. 2 / HDTMS composite nanofiber membrane, the exothermic peak at 74.36 °C is more significant, which may be attributed to the addition of TiO 2After the addition of HDTMS, the crystallization kinetics of the composite nanofibrous membrane changed. These nanofillers acted as nucleating agents, thus promoting the crystallization of TPU at an earlier stage, so the exothermic peak was observed at a relatively low temperature (74.36 °C).
[0084] 7. The TPU / TiO prepared in Example 1 2 / HDTMS isothermal adsorption and desorption experiments (the adsorption gas is nitrogen (N 2 ), the test temperature is -195.85℃, the degassing temperature is 150℃, and the degassing time is 6h), and the result is Fig. 9 , where (a) is the isothermal adsorption-desorption curve, (b) is the cumulative pore volume diagram, (c) is the surface schematic diagram, and (d) is the three-dimensional morphology diagram. Fig. 9 In (a), it can be seen that the hysteresis loop isotherm does not have an obvious saturated adsorption platform, indicating that the pore structure is very irregular and is a narrow pore formed by the accumulation of flake particles. It does not show adsorption saturation in the higher relative pressure area. In the SEM image of the TPU composite nanofiber membrane, it can also be clearly seen that there are pores between the fibers. Fig. 9 As shown in (b), the average pore size is 10.31 nm, and the specific surface area measured by multi-point BET is 1.339 m 2 / g. TPU / TiO 2 The / HDTMS composite membrane has a low surface energy of 9.18 mN / m, which is also conducive to hindering the infiltration of water molecules into the fiber membrane. The diameter of water vapor is 4 nm, and the diameter of liquid water is usually greater than 2.0×10 4 nm, indicating that the TPU composite nanofiber membrane allows water vapor molecules to pass freely but prevents liquid water from penetrating, that is, it has waterproof and moisture permeability. Fig. 9 As shown in (d), TPU / TiO 2 The roughness of the / HDTMS composite nanofiber membrane is 13.507 μm. In Example 1, TiO 2 Nanoparticles, TiO2 is evenly distributed inside and on the surface of each fiber. 2 Nanoparticles, compared with pure TPU film, TPU / TiO 2 The surface roughness structure of the HDTMS / HDTMS composite nanofibers increased significantly, which increased the overall surface roughness of the fiber membrane and increased the hydrophobicity of the composite nanofiber membrane.
[0085] 8. The TPU / TiO prepared in Example 1 was measured using a water contact angle meter (OCA20, Germany). 2The static contact angle and rolling angle of the / HDTMS composite nanofiber membrane were measured to evaluate the wetting properties of the fiber membrane surface, and the drop volume was 10μL. The surface energy of the composite membrane was quantitatively analyzed using a surface tension tester (Dataphysics-OCA20, Germany). The specific surface area of TPU / TiO 2 The specific surface area of the / HDTMS composite nanofiber membrane was measured. The adsorbed gas was nitrogen (N 2 ), the test temperature is -196.15°C, the degassing temperature is 150°C, and the degassing time is 6h. The BET nitrogen adsorption specific surface area calculation formula is shown in formula 2-1:
[0086]
[0087] Where V represents the total volume of the adsorbed gas at the equilibrium pressure P; V m It refers to the volume of gas required to achieve a monolayer coverage state on the catalyst surface; P represents the pressure of the adsorbed gas when it reaches an equilibrium state under specific adsorption temperature conditions during the adsorption process; P 0 refers to the corresponding saturated vapor pressure; while C is a specific constant related to the adsorption process.
[0088] Fig.10 (a) is TPU / TiO 2 Photos of different droplets on the surface of the TPU / TiO composite nanofiber membrane. Water, iced black tea, jasmine tea, cola, milk, and cherry juice droplets can all stay on the membrane surface. 2 / HDTMS composite nanofiber membrane exhibits excellent superhydrophobicity. Fig.10 As shown in (b) and (c), when TPU / TiO 2 When the / HDTMS composite nanofiber membrane was immersed in water, a mirror phenomenon was observed from the surface of the membrane. This is because the air trapped by the layered structure on the fabric surface and the surrounding environment forms a solid-liquid-air interface to prevent water from penetrating into the superhydrophobic surface. The Laplace-Young differential circle method was used to fit the measurement to obtain the TPU / TiO 2 The static contact angle of the / HDTMS composite nanofiber membrane is 166.2°. Fig.10 As shown in (d). TPU / TiO 2 The excellent super-hydrophobicity of the / HDTMS composite nanofiber membrane is attributed to the fact that the rough structure stores a large amount of air, which greatly improves the super-hydrophobicity of the coated fabric. TPU material is originally a hydrophilic substance. The addition of HDTMS provides the TPU composite nanofiber membrane with excellent hydrophobicity, allowing the membrane material to block moisture while maintaining good moisture permeability and breathability, increasing wearing comfort.
[0089] Fig.10 (e) and (f) are pure TPU film and TPU / TiO 2 Contact angle diagram of the / HDTMS composite nanofiber membrane changing with time. Fig.10 In (e), the contact angle of a 10 μL water droplet on the pure TPU membrane is 103.1°, indicating that the water droplet gradually wets the pure TPU membrane, and after 30 seconds, the water droplet has penetrated into the membrane. Fig.10 In (f), the water droplets are still nearly round after 40 seconds. This indicates that TPU / TiO 2 The / HDTMS composite nanofiber membrane has excellent sustained hydrophobicity. The water droplet remained spherical on the coated fabric for 40 seconds without obvious change in the hydrophobic angle, indicating that the coated fabric has excellent superhydrophobic stability.
[0090] TPU / TiO 2 The sliding angle test results of the / HDTMS composite nanofiber membrane are as follows Fig.10 As shown in (g), a 10 μL water droplet appears nearly circular on the membrane surface, and slides off the membrane surface when tilted 3.5°. This indicates that TPU / TiO 2 / HDTMS composite nanofiber membrane has excellent hydrophobicity.
[0091] Water drop adhesion tests were performed to study the adhesion behavior of the coated fabrics and the results were as follows Fig.11 As shown. Fig.11 8 μL water droplet was observed moving away from TPU / TiO 2 / HDTMS composite nanofiber membrane was stretched, and then the water droplet was discharged from the coated fabric without any residue, indicating that the coated fabric has excellent water repellency. 2 The surface energy of the TPU / HDTMS composite nanofiber membrane is 9.18 mN / m. The addition of HDTMS reduces the surface energy of the TPU membrane and can more effectively resist the attraction between water molecules, thereby preventing water diffusion and wetting. Water droplets on the membrane are not easy to spread into a liquid film, but maintain an almost perfect spherical shape, which increases the hydrophobicity of the membrane.
[0092] Superhydrophobic fabrics will inevitably be contaminated by pollutants during use, which will seriously affect their superhydrophobic properties. Therefore, it is very important to make them have anti-fouling and self-cleaning properties to extend their service life. 2 / HDTMS composite nanofiber membrane's anti-pollution performance, we evenly distributed a certain amount of dust on the composite membrane surface, such as Fig.12 As shown, rinse with clean water afterwards. Fig.12During the flushing process, we can clearly see that the stains can be easily washed away from the surface of the membrane by the water flow without any adhesion. Fig.12 The final result further confirmed that the stains had been completely removed. This experimental result fully demonstrated the TPU / TiO 2 / HDTMS composite nanofiber membrane has excellent anti-pollution performance, which can effectively extend its service life.
[0093] 9. Mechanical properties test: The uniaxial tensile properties of the fiber membrane were tested using a mechanical properties comprehensive testing machine (YG026MD, China) using the strip method (GB / T24218.3-2010). The size of the rectangular sample was 60 mm × 10 mm, the clamping distance of the sample was 20 mm, and the tensile speed was 12 mm min. -1 , 5 tensile tests were performed, and the average strength is listed. Table 1 shows the tensile strength of pure TPU film and TPU / TiO 2 Data of 5 stretching of / HDTMS composite nanofiber membrane. Fig.13 The stress-strain curve is shown in Figure 2, where the dotted line is the stress-strain curve of pure TPU film and the solid line is the stress-strain curve of TPU / TiO 2 Stress-strain curves of / HDTMS composite nanofiber membrane.
[0094] Table 1 Mechanical properties of pure TPU film and TPU / TiO2 / HDTMS composite nanofiber membrane
[0095]
[0096]
[0097] At a clamping width of 10 mm and a clamping distance of 20 mm, the average breaking stress of the pure TPU film is 2.56 MPa and the average breaking elongation is 124.22%, indicating that it has high toughness and ductility. 2 The average breaking stress of the / HDTMS composite nanofiber membrane is 3.90MPa, which is increased by 52.34%, and the breaking elongation is 145.80%, which is increased by 17.37%. This shows that the TPU / TiO 2 The breaking stress and elongation of the / HDTMS composite nanofiber membrane are improved, which is due to the TiO 2 The addition of TPU and HDTMS not only increases the microstructural complexity of the material, but also improves the adhesion of the TPU substrate, thereby improving the overall mechanical strength and toughness of the material.
[0098] However, in terms of initial elastic modulus, TPU / TiO 2 / HDTMS composite nanofiber membrane is significantly lower. The average initial elastic modulus of pure TPU membrane is 5.10MPa, while that of TPU / TiO 2 The average initial elastic modulus of the / HDTMS composite nanofiber membrane is 1.04 MPa, indicating that the initial rigidity of the composite membrane is significantly lower than that of the pure TPU membrane, and the deformation is larger under smaller stress, which can flexibly adapt to the needs of human activities.
[0099] 10. The TPU / TiO prepared in Example 2 / HDTMS composite nanofiber membrane for wearing performance test: The anti-ultraviolet transmission performance tester (UV-2000F, USA) was used to measure the TPU / TiO 2 The UPF value and UV transmittance of the / HDTMS composite nanofiber membrane were measured three times and the average value was taken; after three scanning tests, the results are shown in Table 2. According to the national standard GB / T18830-2009 "Evaluation of UV protection performance of textiles", when the UPF value of the sample is greater than 40 and T UVA If the UPF value of a product is less than 5%, it can be called an "anti-ultraviolet product". If the UPF value of a product exceeds 50, it is marked as "UPF50+".
[0100] Table 2 TPU / TiO 2 UPF test of / HDTMS composite nanofiber membrane
[0101]
[0102] It can be seen from Table 2 that TPU / TiO 2 The average UPF value of the / HDTMS composite nanofiber membrane is 1485.7, far exceeding 50. UVA 0.41%, T UVB 0.05%, showing excellent UV protection performance. 2 It has the ability to reflect and disperse most of the ultraviolet rays, thus significantly improving the TPU / TiO 2 Anti-ultraviolet properties of / HDTMS composite nanofiber membrane.
[0103] TPU / TiO 2 / HDTMS composite nanofiber membrane contains TiO 2 The particles are composed of fibers and microspheres. When exposed to ultraviolet light, TiO 2 The particles can absorb and reflect the ultraviolet rays in sunlight.
[0104] TiO 2The particles improve the UV resistance of the composite fiber membrane by enhancing its ability to absorb UV rays. However, the introduction of these inorganic particles forms tiny discontinuous regions in the polymer matrix of TPU, which reduces the overall continuity of the material and leads to a decrease in the initial modulus and fracture stress. These discontinuous regions also help promote the deformation of the material when subjected to external forces, thereby increasing the elongation at break. On the other hand, as a highly hydrophobic substance, the addition of HDTMS can significantly enhance the surface hydrophobicity of the TPU membrane and further increase the contact angle. The enhanced hydrophobicity may also promote the UV blocking effect because it can reduce the absorption of water and the hydrolysis reaction induced by UV rays. In summary, these effects are caused by the TiO 2 and HDTMS, and their combined effects on the structure and surface properties of TPU films. 2 It also has self-cleaning properties. The TiO 2 After the particles are irradiated by ultraviolet light, they absorb enough energy to be excited, causing free electrons to move at a higher energy level. This process releases high-energy charge carriers, generates free radiation, and degrades organic pollutants into non-toxic small molecules, such as water molecules and carbon dioxide molecules. The principle diagram is shown below. Fig.14 shown.
[0105] The RL-450WVP textile moisture permeability tester (Belgium) was used to evaluate the moisture permeability of the samples. The moisture permeability calculation formula is shown in Formula 2-2:
[0106]
[0107] In formula 2-2: WVT is the moisture permeability, the unit is grams per square meter 24h [g / (m 2 ·24h)]; Δm is the difference between two weighings of the same test assembly, in grams (g); Δm′ is the difference between two weighings of the same test assembly of the blank sample, in grams (g); A is the effective test area, in square meters (m 2 );t is the test time, the unit is hour (h).
[0108] The air permeability of the nanofiber membrane was tested using a digital fabric air permeability meter (YG(B)461N, Nantong Hongda Experimental Instrument Co., Ltd.). The air permeability test standard was based on GB / T24218.15-2018, and the test area was 20 cm 2 The circular area is set to a pressure difference of 200 Pa. The test is carried out at room temperature and each sample is tested 3 times. The air permeability calculation formula is shown in formula 2-3:
[0109]
[0110] In formula 2-3: R represents air permeability, the unit is liter per square centimeter second [L / (cm 2 s)], represents the average air permeability, in liters per second (L / s); A represents the test area, in square centimeters (cm 2 ).
[0111] The test results of moisture permeability and air permeability are as follows Fig.15 As shown, the moisture permeability of pure TPU film is 2546.35g / (m 2 24h); TPU / TiO 2 The moisture permeability of the membrane is 2983.43g / (m 2 ·24h), which is 17.16% higher than that of pure TPU film; while TPU / TiO 2 / The moisture permeability of HDTMS film is 3517.45g / (m 2 ·24h), which is 38.13% higher than that of pure TPU film. These improvements are attributed to TiO 2 The addition of TiO and HDTMS not only changes the microstructure and surface properties of the fiber membrane, but also increases the permeation path of water vapor. 2 The addition of nanoparticles formed more micropores and channels, while HDTMS as a surface modifier formed a hydrophobic layer, which increased the water vapor permeability and prevented the penetration of liquid water.
[0112] TPU / TiO 2 The air permeability of the / HDTMS composite nanofiber membrane is relatively higher than that of the pure TPU membrane and TPU / TiO 2 The composite membrane increased by 9.17% and 7.16% respectively. This composite nanofiber membrane contains fiber and bead structures. Although the increase in pores significantly improves moisture permeability, the improvement in air permeability is small because the volume of gas molecules is much smaller than that of water vapor and the gaps in the nanofiber membrane, so the air permeability is less affected.
[0113] The present invention adopts the electrospinning one-step spinning method to successfully prepare TPU / TiO in a low-cost and convenient way. 2 / HDTMS composite nanofiber membrane. The whole process of the preparation method provided by the present invention is completely carried out under room temperature, the preparation process is simple and convenient to operate, the cost is relatively low, and the materials used are environmentally friendly and suitable for large-scale production. 2 / HDTMS composite nanofiber membrane contains both fibers and microspheres, with an average fiber diameter of 481nm, an average microsphere diameter of 1.75μm, an average pore size of 10.31nm, a surface energy as low as 9.18mN / m, and a roughness of up to 13.507μm. It can resist 8μL water droplets, and the hydrophobic angle under 10μL water droplets reaches 166.2±0.5°, the sliding angle is 3.5°, and the surface energy is as low as 9.18mN / m. It not only has super hydrophobic properties, but also has excellent UV protection and moisture permeability, air permeability and anti-fouling properties. The average breaking stress is increased by 52.34% to 3.90MPa, and the breaking elongation is increased by 17.37% to 145.80%. Its UPF average is as high as 1485.7, and the moisture permeability is as high as 3517.45g / (m 2 ·24h), air permeability is 255.83±2.24L / (m 2 ·s). These outstanding properties provide it with broad application prospects in many fields, such as environmental purification, outdoor protective equipment and photocatalysts.
[0114] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A hydrophobic composite material, It is characterized in that comprising a fiber membrane and microspheres embedded in the fiber membrane; The fiber membrane and microspheres are respectively composed of a mixture of thermoplastic polyurethane, titanium dioxide and hexadecyltrimethoxysilane.
2. The hydrophobic composite material according to claim 1, It is characterized in that The average diameter of the microspheres is 0.5 to 1.9 μm; The mass percentage of the microspheres in the hydrophobic composite material is 40-75%.
3. The hydrophobic composite material according to claim 1, It is characterized in that The diameter of the fibers in the fiber membrane is 100-300 nm.
4. The hydrophobic composite material according to any one of claims 1 to 3, It is characterized in that The mass ratio of the thermoplastic polyurethane to titanium dioxide is 6-12:0.5-1.5; The mass ratio of the thermoplastic polyurethane to hexadecyltrimethoxysilane is 6-12:2.5-3.
5.
5. A method for preparing the hydrophobic composite material according to any one of claims 1 to 4, It is characterized in that The following steps are involved: Firstly mixing titanium dioxide, hexadecyltrimethoxysilane and an organic solvent to obtain a dispersion; the organic solvent is a mixed solvent of N,N-dimethylformamide and tetrahydrofuran; secondly mixing the dispersion and thermoplastic polyurethane to obtain a spinning solution; The spinning solution is used for electrostatic spinning to obtain the hydrophobic composite material; the voltage of the electrostatic spinning is 8-16 kV; the ambient temperature of the electrostatic spinning is 18-30° C., and the relative humidity is 45-65%.
6. The preparation method according to claim 5, It is characterized in that The receiving distance of the electrostatic spinning is 15-18 cm, the spinning rate is 0.6-1.2 mL / h, and the rotating speed of the drum is 50-120 r / min.
7. The preparation method according to claim 5, It is characterized in that The titanium dioxide is titanium dioxide nanoparticles, and the average particle size of the titanium dioxide nanoparticles is 5 to 10 nm; The volume ratio of N,N-dimethylformamide to tetrahydrofuran in the organic solvent is 1:1-4; The first mixing is performed under ultrasonic conditions, the power of the ultrasound is 300-400W, the frequency of the ultrasound is 35-45kHz, and the time is 1.5-2.5h.
8. The preparation method according to claim 5, It is characterized in that The thermoplastic polyurethane is thermoplastic polyurethane particles, and the average particle size of the thermoplastic polyurethane particles is 1.8 to 2.2 mm; The second mixing is performed under stirring conditions, the stirring is magnetic stirring, and the stirring time is 5 to 7 hours.
9. The preparation method according to claim 5, 7 or 8, It is characterized in that The mass percentage of thermoplastic polyurethane in the spinning solution is 6-12%, the mass percentage of titanium dioxide is 0.5-1.5%, and the mass percentage of hexadecyltrimethoxysilane is 2.5-3.5%.
10. Use of the hydrophobic composite material according to any one of claims 1 to 4 or the hydrophobic composite material prepared by the preparation method according to any one of claims 5 to 9 as a super-hydrophobic membrane.
Citation Information
Patent Citations
Ultra-hydrophobic polystyrene thin film enhanced by nano silicon dioxide particles and preparation method thereof
CN101165083A
Super-hydrophobic electrostatic spinning polydimethylsiloxane membrane and preparation method and application thereof
CN106334462A
Super-hydrophobic water-proof moisture-permeable nanometer fiber material and preparation method thereof
CN109629113A
Preparation method of super-hydrophobic membrane material
CN112442796A
Preparation method of polyetherimide nanofiber membrane
CN117026512A