Conductive agent and preparation method thereof, composite electrode material and secondary battery

By etching the vapor-grown carbon fiber and doping heteroatoms, a surface defect structure is formed, which improves the electrical properties of the conductive agent, solves the problem of low electrical properties of the existing carbon fiber conductive agent, and achieves efficient electron transmission and environmental protection. preparation process.

CN118727432APending Publication Date: 2024-10-01SHENZHEN DYNANONIC INNOVAZONE NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410724023.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-05
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The electrical properties of existing carbon fiber conductive agents are low and cannot be compared with carbon materials such as carbon nanotubes and graphene.

Method used

By etching the vapor-grown carbon fiber, a surface defect structure is formed, increasing its specific surface area and resistivity, introducing non-carbon heteroatoms to improve conductivity, and preparing a conductive agent with excellent conductive properties.

Benefits of technology

The contact effect between the conductive agent and the electrode material and the electron transmission efficiency are improved, the resistivity is reduced, and the preparation method is environmentally friendly and avoids harmful gas emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118727432A_ABST
    Figure CN118727432A_ABST
Patent Text Reader

Abstract

The invention provides a conductive agent and a preparation method thereof, a composite electrode material and a secondary battery, the conductive agent can be used in the electrode material, the conductive agent comprises carbon fiber with a defect structure formed on the surface, compared with the carbon fiber in the prior art, the surface defects of the conductive agent are increased, so that the specific surface area of the material is increased, and the specific surface area of the material is increased. And when being used as a conductive agent, the conductive agent can obtain a better contact effect and higher electron transmission efficiency with other electrode materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of secondary batteries, and in particular to a conductive agent and a preparation method thereof, a composite electrode material and a secondary battery. Background Art

[0002] Carbon fiber is a carbon material with electrical conductivity and mechanical strength. Compared with other carbon materials, carbon fiber has high structural stability, so carbon fiber is often used as a conductive agent in batteries. However, the electrical properties of existing carbon fiber conductive agents are still inferior to carbon nanotubes and graphene-based carbon materials, so how to provide a carbon fiber conductive agent with high electrical properties has become the key. Summary of the invention

[0003] The purpose of the present invention is to provide a conductive agent and a preparation method thereof, a composite electrode material and a secondary battery, so as to solve the problem that the existing carbon fiber conductive agent has poor electrical properties.

[0004] To achieve the purpose of the present invention, the present invention provides the following technical solutions:

[0005] In a first aspect, the present invention provides a conductive agent comprising carbon fibers, wherein a defect structure is formed on the surface of the carbon fibers.

[0006] The present invention provides a conductive agent, which can be used in electrode materials (including positive electrode materials and negative electrode materials). The conductive agent includes carbon fibers with surface defects. Compared with the carbon fibers in the prior art, the conductive agent has more surface defects, thereby increasing the specific surface area of ​​the material and lowering its resistivity. When used as a conductive agent, it can obtain better contact effects and higher electron transfer efficiency with other electrode materials.

[0007] In one embodiment, the carbon fiber is a vapor-grown carbon fiber, and the surface of the vapor-grown carbon fiber has depressions and / or holes to form the defect structure.

[0008] In one embodiment, the depth of the defect structure on the surface of the carbon fiber ranges from 10 nm to 100 nm.

[0009] In one embodiment, the pore volume of the carbon fiber is 0.03 g / cm 3 ~0.5g / cm 3 .

[0010] In one embodiment, the carbon fibers are further doped with non-carbon heteroatoms.

[0011] In one embodiment, the aspect ratio of the carbon fiber is 10-100.

[0012] In one embodiment, the length of the carbon fiber is 5 μm to 50 μm.

[0013] In one embodiment, the diameter of the carbon fiber is 100 nm to 200 nm.

[0014] In one embodiment, the specific surface area of ​​the carbon fiber is 15m 2 / g~100m 2 / g

[0015] In one embodiment, in the Raman spectrum of the carbon fiber, the peak intensity ratio of the D band to the G band is R≥0.8.

[0016] In one embodiment, the resistivity of the carbon fiber is less than or equal to 1.35 mΩ·m.

[0017] In a second aspect, the present invention also provides a method for preparing a conductive agent, comprising: providing carbon fiber and placing the carbon fiber under an inert atmosphere; heating the carbon fiber and introducing an etchant into the inert atmosphere so that the etchant etches the carbon fiber to obtain a carbon fiber having a defective structure formed on the surface.

[0018] The present invention provides a method for preparing a conductive agent, and the preparation method is used to prepare carbon fibers with surface defects. Compared with the carbon fibers in the prior art, the conductive agent has more surface defects, thereby increasing the specific surface area of ​​the material and lowering its resistivity. When used as a conductive agent, it can obtain better contact effect and higher electron transfer efficiency with other electrode materials. In addition, the preparation method does not use harmful reagents in the process of preparing the conductive agent, and uses water etching and high-temperature treatment, without the need to treat waste gas, which can reduce the emission of harmful gases and has high environmental friendliness.

[0019] In a third aspect, the present invention further provides a composite electrode material, comprising an electrode material and the conductive agent as described in the first aspect, or comprising a conductive agent obtained by the preparation method of the conductive agent as described in the second aspect.

[0020] In a fourth aspect, the present invention further provides a secondary battery, comprising a positive electrode, a negative electrode and a separator disposed between the positive electrode and the negative electrode, wherein the positive electrode and / or the negative electrode comprises the composite electrode material as described in the third aspect. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0022] Figure 1is a schematic diagram of the appearance of a conductive agent according to an embodiment;

[0023] Figure 2 is a schematic diagram of the appearance of a conductive agent according to another embodiment;

[0024] Figure 3 is a SEM image of a conductive agent according to an embodiment;

[0025] Figure 4 is a flow chart of a method for preparing a conductive agent according to an embodiment;

[0026] Figure 5 is the Raman image of the carbon fiber of Example 1;

[0027] Figure 6 This is the Raman image of the carbon fiber of Comparative Example 1. DETAILED DESCRIPTION

[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used in the present invention includes any and all combinations of one or more of the related listed items.

[0030] Some embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.

[0031] The present invention provides a conductive agent, please refer to Figures 1 to 3 The conductive agent can be used to mix with the positive electrode material or the negative electrode material. The conductive agent includes carbon fiber 100, and a defective structure is formed on the surface of the carbon fiber 100.

[0032] Specifically, the conductive agent can be mixed with the positive electrode material or the negative electrode material to improve the electronic conductivity of the battery, accelerate the movement of electrons, and reduce the contact resistance.

[0033] Optionally, the carbon fiber 100 is vapor grown carbon fiber (Vapor Grown Carbon Fiber, VGCF), which is a fibrous carbon-based material generated by high-temperature pyrolysis of low-carbon hydrocarbon raw materials under the action of a transition metal catalyst, and usually has the form of irregular short fibers.

[0034] The present invention uses vapor-grown carbon fiber as a conductive agent, which has the following advantages: 1) high conductivity. VGCF has very good conductivity, and its conductivity effect far exceeds that of ordinary carbon black, carbon nanotubes, etc.; 2) high strength and corrosion resistance. VGCF exhibits high strength and good chemical stability and can withstand the erosion of electrolyte.

[0035] Furthermore, the carbon fiber 100 provided by the present invention has surface defects. Among them, the surface defects mainly include point defects, line defects and surface defects; point defects refer to the absence or replacement of atoms in the carbon fiber 100; line defects refer to edge defects or lattice dislocations in the carbon fiber 100; surface defects are manifested as holes or cracks in the carbon fiber 100.

[0036] Optionally, the surface defects of the carbon fiber 100 can be obtained by high-temperature water vapor etching. In a specific embodiment, the carbon fiber 100 without surface defects can be placed in a high temperature environment, and then a mixed gas of inert gas and water vapor is introduced, and the oxygen element in the water vapor reacts with the carbon fiber 100, so that part of the carbon element on the surface of the carbon fiber 100 is separated, thereby obtaining the carbon fiber 100 with surface defects.

[0037] Optionally, in other specific embodiments, the carbon fiber 100 without surface defects may be soaked in an etchant so that the etchant can adhere to the surface of the carbon fiber 100, and then the carbon fiber 100 is placed in a high-temperature ring of an inert atmosphere so that deionized water or an etching solution can etch the carbon fiber 100. The etchant may be deionized water, acid, alkali, organic solvent or other etching solution.

[0038] The present invention provides a conductive agent, which can be used in electrode materials (including positive electrode materials and negative electrode materials). The conductive agent includes carbon fiber 100 with surface defects. Compared with the carbon fiber 100 in the prior art, the conductive agent has more surface defects, so that the specific surface area of ​​the material is increased and the resistivity is lower. When used as a conductive agent, it can obtain better contact effect and higher electron transmission efficiency with other electrode materials.

[0039] In one implementation, please refer to Figure 1, the surface of the vapor-grown carbon fiber has depressions and / or holes to form a defect structure 10. Specifically, the surface defect structure of the carbon fiber 100 is formed by etching, so the defect structure 10 on the surface of the carbon fiber 100 can be divided into depressions or holes based on the degree of etching; wherein the deeper etching part is the hole, and the shallower etching part is the depression.

[0040] It should be explained that the surface of the existing carbon fiber 100 is smooth and flat, so the specific surface area of ​​the existing carbon fiber 100 is small, resulting in poor contact between the material and the electrode material and poor conductivity. The present invention can obtain a carbon fiber 100 with a rough surface by etching the existing carbon fiber 100. And the etching process can be controlled to form the desired depressions or holes on the surface of the carbon fiber 100.

[0041] In one implementation, please refer to Figure 1 , the defect structure 10 of the carbon fiber 100 has a plurality of depressions and holes.

[0042] In one embodiment, the depth of the defect structure on the surface of the carbon fiber 100 ranges from 10nm to 100nm. Optionally, the depth of the defect structure on the surface of the carbon fiber 100 can be 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm. It should be explained that the depth of the defect structure on the surface of the carbon fiber 100 includes the depth of depressions and holes. The depth of the depressions or holes of the carbon fiber 100 can be regulated by controlling the parameters of the etching process.

[0043] When the depth of the defect structure on the surface of the carbon fiber 100 is within the above range, the carbon fiber 100 with a higher specific surface area can be obtained, and the structural stability of the carbon fiber 100 is ensured. When the depth of the defect structure of the carbon fiber 100 is less than the above range, the specific surface area of ​​the carbon fiber 100 is limited, and the improvement of the conductive effect is not obvious; when the depth of the defect structure of the carbon fiber 100 is greater than the above range, the structural stability of the carbon fiber 100 is not ideal, and the carbon fiber 100 is easily damaged.

[0044] In one embodiment, the pore volume of the carbon fiber 100 is 0.03 g / cm 3 ~0.5g / cm 3 The pore volume is also called the pore volume, which is the total volume of pores per unit mass of a porous solid. Optionally, the pore volume of the carbon fiber 100 can be 0.03 g / cm 3 , 0.05g / cm 3 , 0.07g / cm 3 , 0.09g / cm 3 , 0.1g / cm 3 , 0.2g / cm 3, 0.3g / cm 3 , 0.4g / cm 3 , 0.5g / cm 3 It is understandable that the pore volume of the carbon fiber 100 can be adjusted by controlling the parameters of the etching process.

[0045] When the pore volume of the carbon fiber 100 is within the above range, a carbon fiber 100 with a higher specific surface area can be obtained, so that the carbon fiber 100 has a better contact effect with the electrode material, improves the transmission efficiency of electrons, and reduces the resistivity of the material. When the pore volume of the carbon fiber 100 is less than the above range, the specific surface area of ​​the carbon fiber 100 is limited, which may cause the electrical properties of the carbon fiber 100 to decrease; when the pore volume of the carbon fiber 100 is greater than the above range, the structural stability of the carbon fiber 100 deteriorates, and the carbon fiber 100 is easily damaged or cracked, which may cause the battery to pulverize and slag.

[0046] In one implementation, please refer to Figure 2 The surface of the carbon fiber 100 also has a plurality of convex points 20, and the convex points 20 protrude from the outer surface of the carbon fiber 100. Specifically, based on the above embodiment, under the water etching process, a portion of the original carbon fiber 100 can be thinned (the fiber diameter is reduced), so that a plurality of convex points 20 can be obtained on the surface of the carbon fiber 100.

[0047] It should be explained that the position of the protrusion 20 is the diameter of the original carbon fiber 100. After water etching, part of the carbon fiber 100 is thinned, and the unthinned part is retained to form the protrusion 20. It can be understood that by forming a plurality of protrusions 20 on the surface of the carbon fiber 100, the surface roughness of the carbon fiber 100 can be increased, thereby increasing the specific surface area of ​​the carbon fiber 100.

[0048] In one embodiment, the carbon fiber 100 is also doped with non-carbon heteroatoms. Specifically, the surface defect type of the carbon fiber 100 also includes non-carbon heteroatom doping, and the introduction of heteroatoms can improve the electronic conductivity of the carbon fiber 100; since heteroatoms are more electronegative than carbon atoms, the doped carbon fiber 100 has better electronic conductivity.

[0049] Moreover, the heteroatom-doped carbon fiber 100 as a material for lithium-ion batteries can improve electron mobility and lithium ion mobility. In addition, by doping heteroatoms, such as sulfur atoms, the carbon spacing of the carbon fiber 100 can be significantly enlarged, defects and active sites can be increased, and thus its electrochemical performance can be improved.

[0050] Optionally, the preparation method of the heteroatom-doped carbon fiber 100 can be: before the inert gas is introduced into the carbon fiber 100, the inert gas can be introduced into an etching solution containing heteroatoms, and then a small amount of heteroatom-containing etching solution mixed in the inert gas is introduced into the carbon fiber 100; as the ambient temperature increases, the heteroatom etching solution reacts with the surface of the carbon fiber, and allows the heteroatoms to be incorporated into the carbon fiber 100 to form surface defects.

[0051] Optionally, in other embodiments, the preparation method of the heteroatom-doped carbon fiber 100 may also be: calcining the carbon fiber 100 together with a carbon material (or precursor) containing heteroatoms, so that the heteroatoms can enter into the atomic defects formed by the carbon fiber 100.

[0052] In one embodiment, the heteroatoms doped on the carbon fiber 100 include one or more of nitrogen (N), phosphorus (P), and sulfur (S).

[0053] In one embodiment, the aspect ratio of the carbon fiber 100 is 10 to 100. Optionally, the aspect ratio of the carbon fiber 100 may be 10, 20, 30, 40, 50, 60, 70, 80, 90, or 100.

[0054] When the aspect ratio of the carbon fiber 100 is within the above range, it is possible to avoid the carbon fiber 100 being too thin or too thick and too large to affect the specific surface area of ​​the carbon fiber 100, and it is also possible to reduce the difficulty of preparing the carbon fiber 100. When the aspect ratio of the carbon fiber 100 is less than the above range, the carbon fiber 100 is too thick, which will cause the specific surface area to decrease, and the softness of the carbon fiber 100 will decrease, making it difficult to fully mix with the electrode material. When the aspect ratio of the carbon fiber 100 is greater than the above range, the carbon fiber 100 is too thin, which will easily cause the carbon fibers 100 to be entangled in balls, and the dispersibility of the carbon fiber 100 will deteriorate.

[0055] In one embodiment, the length of the carbon fiber 100 is 5 μm to 50 μm. Optionally, the length of the carbon fiber 100 may be 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, or 50 μm.

[0056] Meeting the length of the carbon fiber 100 within the above range can prevent the volume of the carbon fiber 100 from being too large and affecting the proportion of the electrode material, and can also ensure the mechanical properties of the carbon fiber 100. When the length of the carbon fiber 100 is less than the above range, the carbon fiber 100 is too short, and the ability of the carbon fiber 100 to transfer stress is weakened, affecting the overall mechanical properties of the carbon fiber 100. When the length of the carbon fiber 100 is greater than the above range, the volume of the carbon fiber 100 per unit gram weight increases, which will cause the proportion of the electrode material per unit volume to decrease; and when the carbon fiber 100 is too long, the contact points between the carbon fibers 100 are reduced, resulting in a decrease in the conductivity of the carbon fiber 100 in the electrode.

[0057] In one embodiment, the diameter of the carbon fiber 100 is 100nm to 200nm. Optionally, the diameter of the carbon fiber 100 can be 100nm, 110nm, 120nm, 130nm, 140nm, 150nm, 160nm, 170nm, 180nm, 190nm, 200nm. Satisfying that the diameter of the carbon fiber 100 is within the above range can also avoid the volume of the carbon fiber 100 being too large and affecting the proportion of the electrode material, and can also reduce the difficulty of preparing the carbon fiber 100.

[0058] In one embodiment, the specific surface area of ​​the carbon fiber 100 is 15 m 2 / g~100m 2 / g. Optionally, the specific surface area of ​​the carbon fiber 100 can be 15m 2 / g, 20m 2 / g, 30m 2 / g, 40m 2 / g, 50m 2 / g, 60m 2 / g, 70m 2 / g, 80m 2 / g, 90m 2 / g、100m 2 / g.

[0059] It can be understood that the specific surface area of ​​the carbon fiber 100 provided by the present invention is positively correlated with the amount of the above-mentioned surface defects, so the specific surface area of ​​the carbon fiber 100 that meets this range can refer to the effect of the above-mentioned pore volume, which will not be elaborated here.

[0060] In one embodiment, in the Raman spectrum of the carbon fiber 100, the peak intensity ratio of the D band to the G band is R≥0.8. Specifically, G and D refer to two types of carbon in the carbon material, and their ratio ID / IG can reflect which type of carbon accounts for a larger proportion. In a specific embodiment, Figure 5 As shown, at 1350cm 1 A peak called D band (Dband) was found near 1580cm1 A peak called the G band (Gband) is found near Figure 6 The ID / IG ratio can be used to describe the parameter of the degree of carbon defects in the carbon material. It is the ratio of the D peak and the G peak intensities in the Raman spectrum. Therefore, when the peak intensity ratio of the D band to the G band (ID / IG) is larger, it means that there are more defects in the carbon material, and vice versa. Therefore, the ratio of the D peak and the G peak intensities of the carbon fiber 100 is within the above range, which can ensure that there are enough defects on the carbon fiber 100.

[0061] Among them, the D peak is usually related to defects or disordered structures in carbon materials, which is caused by the A1g breathing mode in the carbon atom crystal. The appearance of the D peak often means that there are defects in the material, such as vacancies, grain boundaries or other amorphous structures. The G peak is related to the in-plane vibration mode E2g of carbon atoms and usually represents the order of the material. The G peak is a typical feature of carbon materials, and its high intensity indicates that the material has high crystallinity and structural integrity.

[0062] In one embodiment, in the Raman spectrum of the carbon fiber 100, the peak intensity ratio R of the D band to the G band satisfies the range: 0.8≤R≤5. Optionally, the peak intensity ratio R of the D band to the G band may be in the range of 0.8≤R≤2. Specifically, the peak intensity ratio R of the D band to the G band may be 0.8, 0.85, 0.9, 0.95, 1, 1.05, 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, 1.4, 1.45, 1.5, 1.55, 1.6, 1.65, 1.7, 2, 3, 4, 5.

[0063] It should be noted that, based on the structural stability of carbon fiber, the degree of defects inside the carbon fiber needs to be controlled within an appropriate range. Because when there are too many carbon defects inside the carbon fiber (i.e., when the ID / IG value is too large), the structural stability of the carbon fiber will deteriorate, resulting in a decrease in material performance. However, it is understandable that, in the case of providing a suitable initial carbon fiber structure (for example, when the initial structural strength of the carbon fiber is high), as many carbon defects as possible can be made on the carbon fiber, and the ID / IG can also exceed the above upper limit.

[0064] In one embodiment, the present invention also provides a method for preparing a conductive agent, please refer to Figure 4 , specifically including the following steps:

[0065] Step S11, providing carbon fibers, and placing the carbon fibers under an inert atmosphere.

[0066] Step S12, heat-treating the carbon fiber, and introducing an etchant into an inert atmosphere so that the etchant etches the carbon fiber to obtain a carbon fiber with a defective structure formed on the surface.

[0067] Optionally, before step S11, the method further includes step S10: preparing carbon fiber.

[0068] In a specific embodiment, the prepared carbon fiber is vapor-grown carbon fiber, and the preparation method of vapor-grown carbon fiber includes: preparing nano-sized metal catalyst particles, and depositing the metal catalyst particles on a substrate for carbon fiber growth; then exposing the metal catalyst particles to a carbon source gas under high temperature conditions, such as methane, benzene, acetylene or carbon monoxide; under the action of the catalyst, the carbon source gas decomposes and forms carbon filaments on the surface of the metal catalyst particles to obtain vapor-grown carbon fiber.

[0069] Optionally, in step S11, the carbon fiber is placed under an inert atmosphere, specifically comprising: taking a certain mass of carbon fiber in a porcelain boat and placing it in a tubular furnace, and then introducing an inert gas into the tubular furnace to exhaust the air in the tubular furnace.

[0070] Optionally, in step S11, the mass of the carbon fiber may be 1 g to 10 g. In a specific embodiment, the mass of the carbon fiber may be 1 g, 2 g, 3 g, 4 g, 5 g, 6 g, 7 g, 8 g, 9 g, or 10 g.

[0071] Optionally, in step S11, the inert gas may be at least one of argon, helium, and nitrogen.

[0072] Optionally, in step S12, the carbon fiber is treated at high temperature and an etchant is introduced into an inert atmosphere, specifically including: heating the tubular furnace and switching the gas flow, and passing the inert gas introduced into the tubular furnace through a washing bottle filled with water in advance so that the inert gas can carry part of the water vapor into the tubular furnace.

[0073] Optionally, in step S12, the temperature of high temperature treatment of carbon fiber may be 500°C to 1000°C. In a specific embodiment, the temperature of high temperature treatment of carbon fiber may be 500°C, 600°C, 700°C, 800°C, 900°C, or 1000°C.

[0074] Optionally, in step S12, the inert gas flow rate may be 100 mL / min to 1000 mL / min. In a specific embodiment, the inert gas flow rate may be 100 mL / min, 200 mL / min, 400 mL / min, 600 mL / min, 800 mL / min, or 1000 mL / min.

[0075] Optionally, in step S12, the etching time may be 15 min to 2 h. In a specific embodiment, the etching time may be 15 min, 30 min, 45 min, 1 h, 1 h 15 min, 1 h 30 min, 1 h 45 min, or 2 h.

[0076] The present invention provides a method for preparing a conductive agent. The preparation method is used to prepare carbon fibers with surface defects. Compared with the carbon fibers in the prior art, the conductive agent has more surface defects, thereby increasing the specific surface area of ​​the material and lowering its resistivity. When used as a conductive agent, it can obtain better contact effect and higher electron transfer efficiency with other electrode materials, and exhibits lower resistivity. In addition, the preparation method does not use harmful reagents in the process of preparing the conductive agent, and uses water etching and high-temperature treatment, without the need to treat waste gas, which can reduce the emission of harmful gases and has high environmental friendliness.

[0077] In one embodiment, the present invention further provides a composite electrode material, which includes an electrode material and the conductive agent provided in the above embodiment.

[0078] Optionally, the electrode material can be a positive electrode material or a negative electrode material, or the electrode material can be a positive electrode lithium replenishing material or a negative electrode lithium replenishing material; of course, the electrode material can also be a mixture of a positive electrode active material and a positive electrode lithium replenishing material, or a mixture of a negative electrode active material and a negative electrode lithium replenishing material.

[0079] Optionally, the positive electrode active material can be a phosphate positive electrode active material and a ternary positive electrode active material. In a specific embodiment, it includes one or more of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium vanadium phosphate, lithium vanadium oxyphosphate, lithium fluorovanadium phosphate, lithium titanate, lithium nickel cobalt manganese oxide, and lithium nickel cobalt aluminum oxide.

[0080] In one embodiment, the mass percentage of the conductive agent in the composite electrode material can be controlled to be 3% to 5%. In some specific embodiments, the mass percentage of the lithium supplement material in the positive electrode material can be 3%, 3.5%, 4%, 4.5%, 5%, etc.

[0081] In one embodiment, the conductive agent is coated on the outer surface of the electrode material. Specifically, the conductive agent can be coated on the surface of the electrode material to form a conductive coating layer. The electrode material can be the type provided above.

[0082] In one embodiment, the present invention further provides an electrode plate, which includes a current collector and an active material layer disposed on the current collector, wherein the active material layer includes the composite electrode material of any one of the above embodiments.

[0083] Optionally, the electrode plate is a positive electrode plate, including a positive current collector, and the positive current collector has a positive active layer, and the positive active layer includes components such as positive active materials, lithium supplement materials, and binders. The present invention does not specifically limit these materials, and suitable materials can be selected according to actual application requirements; of course, the positive active layer also includes the conductive agent provided in the above embodiment. The positive current collector includes but is not limited to any one of copper foil and aluminum foil. The types of binders include polyvinylidene chloride, soluble polytetrafluoroethylene, styrene-butadiene rubber, hydroxypropyl methylcellulose, methylcellulose, carboxymethyl cellulose, polyvinyl alcohol, acrylonitrile copolymers, sodium alginate, chitosan, and chitosan derivatives. One or more, and the content of the binder in the positive active layer is 2wt% to 4wt%.

[0084] In one embodiment, the present invention further provides a secondary battery, comprising a positive electrode, a negative electrode and a separator disposed between the positive electrode and the negative electrode, wherein the positive electrode and / or the negative electrode may be the electrode sheet described above, and the electrode sheet includes the conductive agent provided in the above embodiment.

[0085] The technical solution of the present invention is described in detail below through specific embodiments.

[0086] Example 1

[0087] This embodiment provides a conductive agent, which includes vapor-grown carbon fiber, the surface of which is formed with a defect structure, the defect structure of which is manifested as a plurality of holes, the aspect ratio of which is 50, the length is 10 μm, and the diameter is 200 nm. The depth of the defect structure is 10 nm, and the pore volume is 0.03 g / cm 3 .

[0088] The method for preparing carbon fiber in this embodiment comprises the following steps:

[0089] 1) Take 5 g of carbon fiber and place it in a porcelain boat in a tube furnace, then introduce argon gas into the tube furnace to exhaust the air in the tube furnace.

[0090] 2) The temperature of the tubular furnace was raised to 800° C., and the gas flow was switched. Argon gas at 100 mL / min passed through a gas washing bottle filled with water and then entered the tubular furnace. The carbon fiber was etched for 1 hour to obtain water-etched carbon fiber.

[0091] Example 2

[0092] This embodiment provides a conductive agent, which includes vapor-grown carbon fiber, the surface of which is formed with a defect structure, the defect structure of which is manifested as a plurality of holes, the aspect ratio of which is 50, the length is 10 μm, the diameter is 200 nm, the depth of the defect structure is 30 nm, and the pore volume is 0.1 g / cm 3 .

[0093] The preparation method of the conductive agent comprises the following steps:

[0094] 1) Take 5 g of carbon fiber and place it in a porcelain boat in a tube furnace, then introduce argon gas into the tube furnace to exhaust the air in the tube furnace.

[0095] 2) The temperature of the tubular furnace was raised to 800° C., and the gas flow was switched. Argon gas at 300 mL / min passed through a gas washing bottle filled with water and then entered the tubular furnace. The carbon fiber was etched for 1 hour to obtain water-etched carbon fiber.

[0096] Example 3

[0097] This embodiment provides a conductive agent. The difference between this embodiment and the conductive agent in embodiment 1 is that the depth of the defect structure is 50nm and the pore volume is 0.5g / cm 3 .

[0098] The preparation method of the composite catalyst and the composite lithium supplement material comprises the following steps:

[0099] 1) Take 5 g of carbon fiber and place it in a porcelain boat in a tube furnace, then introduce argon gas into the tube furnace to exhaust the air in the tube furnace.

[0100] 2) The temperature of the tubular furnace was raised to 800° C., and the gas flow was switched. Argon gas at 500 mL / min passed through a gas washing bottle filled with water and then entered the tubular furnace. The carbon fiber was etched for 1 hour to obtain water-etched carbon fiber.

[0101] Example 4

[0102] This embodiment provides a conductive agent. The difference between the conductive agent in this embodiment and that in Embodiment 2 is that the carbon fiber has an aspect ratio of 100, a length of 20 μm, and a diameter of 200 nm.

[0103] The method for preparing carbon fiber in this embodiment comprises the following steps:

[0104] 1) Take 5 g of carbon fiber and place it in a porcelain boat in a tube furnace, then introduce argon gas into the tube furnace to exhaust the air in the tube furnace.

[0105] 2) The temperature of the tubular furnace was raised to 800° C., and the gas flow was switched. Argon gas at 300 mL / min passed through a gas washing bottle filled with water and then entered the tubular furnace. The etching was performed for 0.5 h to obtain water-etched carbon fiber.

[0106] Example 5

[0107] This embodiment provides a conductive agent. The difference between the conductive agent in this embodiment and that in Embodiment 2 is that the carbon fiber has an aspect ratio of 10, a length of 1 μm, and a diameter of 100 nm.

[0108] The preparation method of the composite catalyst and the composite lithium supplement material comprises the following steps:

[0109] 1) Take 5 g of carbon fiber and place it in a porcelain boat in a tube furnace, then introduce argon gas into the tube furnace to exhaust the air in the tube furnace.

[0110] 2) The temperature of the tubular furnace was raised to 800° C., and the gas flow was switched. Argon gas at 300 mL / min passed through a gas washing bottle filled with water and then entered the tubular furnace. The carbon fiber was etched for 12 hours to obtain water-etched carbon fiber.

[0111] Example 6

[0112] This embodiment provides a conductive agent. The conductive agent of this embodiment is different from that of Embodiment 1 in that the carbon fibers are further doped with N element.

[0113] The preparation method of the composite catalyst and the composite lithium supplement material comprises the following steps:

[0114] 1) Take 5 g of carbon fiber and place it in a porcelain boat in a tube furnace, then introduce argon gas into the tube furnace to exhaust the air in the tube furnace.

[0115] 2) The temperature of the tubular furnace was raised to 800° C., and the gas flow was switched. Argon gas at 300 mL / min passed through a gas washing bottle filled with water and then entered the tubular furnace. The carbon fiber was etched for 1 hour to obtain water-etched carbon fiber.

[0116] Example 7

[0117] This embodiment provides a conductive agent. The conductive agent of this embodiment is different from that of Embodiment 1 in that the carbon fiber is further doped with S element.

[0118] The preparation method of the composite catalyst and the composite lithium supplement material comprises the following steps:

[0119] 1) Take 5 g of carbon fiber and place it in a porcelain boat in a tube furnace, then introduce argon gas into the tube furnace to exhaust the air in the tube furnace.

[0120] 2) The temperature of the tubular furnace was raised to 800° C., and the gas flow was switched. Argon gas at 300 mL / min passed through a gas washing bottle filled with water and then entered the tubular furnace. The carbon fiber was etched for 1 hour to obtain water-etched carbon fiber.

[0121] Comparative Example 1

[0122] This comparative example provides a conductive agent. The conductive agent includes ordinary carbon fiber. Among them, Figure 6 This is the Raman image of the carbon fiber of Comparative Example 1.

[0123] The conductive agents provided in the above-mentioned Examples 1 to 7 and the conductive agent provided in Comparative Example 1 were tested as follows:

[0124] Surface area test: The conductive agent in each embodiment and comparative example was tested by a BET analyzer to obtain the specific surface area.

[0125] Raman test: The conductive agent in each embodiment and comparative example was tested by a Raman spectrum test platform to obtain a Raman spectrum.

[0126] Resistivity test: The resistivity of the conductive agent in each embodiment and comparative example was calculated and tested by a four-probe method.

[0127] The test results of the conductive agent are shown in Table 1 below:

[0128] Table 1. Test results of embodiments and comparative examples

[0129]

[0130]

[0131] From the test results of Examples 1 to 7 and Comparative Example 1 in Table 1, it can be seen that the conductive agents provided in the embodiments of the present invention all have large specific surface areas, high ID / IG values, and low resistivity. This indicates that the surface of the carbon fiber conductive agent prepared by the method provided by the present invention has more defect structures. Compared with the carbon fiber in the comparative document, the conductive agent in the embodiment has more surface defects, thereby increasing the specific surface area of ​​the material and lowering its resistivity. When used as a conductive agent, it can obtain better contact effects and higher electron transfer efficiency with other electrode materials.

[0132] From the test results of Examples 1 to 3 in Table 1, it can be seen that by controlling the etching gas flow rate, a carbon fiber conductive agent with a relatively suitable defect structure depth and pore volume can be obtained, so that the specific surface area and ID / IG value of the carbon fiber are both higher than those of ordinary carbon fiber (13.01 m in Comparative Example 1). 2 / g and 0.1). However, the resistivity of the conductive agent will decrease first and then increase with the increase of specific surface area and ID / IG. Because, if the etching gas flow rate is too small, insufficient etching will occur, that is, the depth and pore volume of the defect structure of the carbon fiber will be small, so the specific surface area is small; as the etching gas flow rate increases (300mL / min), the specific surface area and ID / IG value of the material will be further increased, thereby reducing the resistivity; but if the etching degree is too large, over-etching will occur, which will affect the structural stability of the material, thereby increasing the resistivity.

[0133] From the test results of Example 2, Example 4 and Example 5 in Table 1, it can be learned that by controlling the etching time, a carbon fiber conductive agent with a more suitable aspect ratio can be obtained. When the etching time is short, the appearance of the carbon fiber changes less. Under the same defect, the carbon fiber is too long, resulting in a small specific surface area of ​​the material. The corresponding ID / IG value decreases and the resistivity increases slightly. When the etching time is long, the appearance of the carbon fiber changes greatly. Under the same defect, the carbon fiber is over-etched, resulting in a length that is too short and a diameter that is too small. Although the specific surface area of ​​the material increases, the material structure is damaged, resulting in an increase in resistivity.

[0134] From the test results of Example 2, Example 6 and Example 7 and Comparative Example 1 in Table 1, it can be seen that by introducing heteroatoms into the carbon fiber conductive agent, the defects of the carbon fiber can also be increased to increase the specific surface area, and the introduced nitrogen element can further effectively reduce the resistivity of the conductive agent to 0.91 mΩ·m. The introduction of sulfur element has a weaker effect on improving the resistivity, but is still better than Comparative Example 1.

[0135] In the description of the embodiments of the present invention, it should be noted that the orientation or positional relationship of terms such as "center", "up", "down", "left", "right", "vertical", "horizontal", "inside" and "outside" are based on the orientation or positional relationship of the accompanying drawings, which are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.

[0136] What is disclosed above is only a preferred embodiment of the present invention, and it certainly cannot be used to limit the scope of rights of the present invention. Ordinary technicians in this field can understand that all or part of the processes of the above embodiment and equivalent changes made according to the claims of the present invention still fall within the scope covered by the present invention.

Claims

1. A conductive agent, It is characterized in that The invention comprises carbon fibers, and a defect structure is formed on the surface of the carbon fibers.

2. The conductive agent according to claim 1, It is characterized in that The carbon fiber is a vapor-grown carbon fiber, and the surface of the vapor-grown carbon fiber has depressions and / or holes to form the defect structure.

3. The conductive agent according to claim 2, It is characterized in that The depth of the defect structure on the carbon fiber surface ranges from 10 nm to 100 nm; and / or, The pore volume of the carbon fiber is 0.03 g / cm 3 ~0.5g / cm 3 .

4. The conductive agent according to claim 1, It is characterized in that The carbon fibers are also doped with non-carbon heteroatoms.

5. The conductive agent according to claim 1, It is characterized in that The aspect ratio of the carbon fiber is 10 to 100; and / or The length of the carbon fiber is 5 μm to 50 μm; and / or The diameter of the carbon fiber is 100nm to 200nm; and / or The specific surface area of ​​the carbon fiber is 15m 2 / g~100m 2 / g.

6. The conductive agent according to any one of claims 1 to 5, It is characterized in that In the Raman spectrum of the carbon fiber, the peak intensity ratio of the D band to the G band is R≥0.

8.

7. The conductive agent according to claim 6, It is characterized in that The resistivity of the carbon fiber is less than or equal to 1.35 mΩ·m.

8. A method for preparing a conductive agent, It is characterized in that include: Providing carbon fibers and placing the carbon fibers under an inert atmosphere; The carbon fiber is subjected to a heat treatment, and an etchant is introduced into an inert atmosphere so that the etchant etches the carbon fiber to obtain a carbon fiber with a defective structure formed on the surface.

9. A composite electrode material, It is characterized in that The composite electrode material comprises an electrode material and the conductive agent as described in any one of claims 1 to 7, or comprises a conductive agent obtained by the preparation method of the conductive agent as described in claim 8.

10. A secondary battery, It is characterized in that It comprises a positive electrode, a negative electrode and a separator arranged between the positive electrode and the negative electrode, and the positive electrode and / or the negative electrode comprises the composite electrode material as claimed in claim 9.