Ceramic-based monofilament composite material preparation device and method and component mechanical and electrical parameter testing method
By designing the preparation device and testing method of ceramic-based single-filament composite materials, the problem of difficulty in measuring the electrical and mechanical parameters of the components of ceramic-based composite materials has been solved, and the precise preparation of ceramic-based single-filament composite materials and the measurement of the mechanical and electrical parameters of the components have been achieved. , improving the comparability and cost efficiency of experimental data.
Patent Information
- Application Number
- CN202410712682.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-04
- Publication Date
- 2024-10-01
AI Technical Summary
Existing technology cannot effectively test the interface, matrix in-situ resistivity and electromechanical coupling characteristics of ceramic matrix composites, making it difficult to obtain the electrical and mechanical parameters of key components, affecting the accuracy of structural damage monitoring.
A device and method for preparing ceramic-based monofilament composite materials is designed. The fiber monofilaments are fixed through positioning bolts and gaskets, and interface or matrix component materials are prepared on their surfaces. Combined with electronic tensile tests and scanning electron microscope measurements, calculations Resistivity and modulus properties of components.
It achieves the precise preparation of ceramic-based single-filament composite materials and the measurement of component electroelectric parameters, simplifies the damage mode, improves the comparability of experimental data, and reduces material consumption and experimental costs.
Smart Images

Figure CN118730648A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of composite material performance testing, and in particular, relates to a ceramic-based monofilament composite material preparation device and method, and a component electromechanical parameter testing method. Background Art
[0002] Ceramic matrix composites (CMCs) have broad application prospects in advanced aero engines, high-speed aircraft and other fields due to their high specific modulus, high specific strength, high temperature resistance and low density. At the same time, because their component materials usually have a certain conductivity, there is a certain correspondence between their structural resistance and damage. Monitoring the structural damage of ceramic matrix composites using resistivity changes is becoming a potential damage monitoring technology. CMCs, as a composite material, contains a variety of component materials. There are significant differences in the mechanical and electrical properties of different components. It is for this reason that the performance of composite materials has obvious advantages over traditional single-component materials. Obtaining the electrical and mechanical parameter characteristics of CMCs component materials is of great significance for using resistors to monitor the structural strength and life health of CMCs.
[0003] There is no in-situ resistivity test of CMCs interface and matrix, as well as in-situ electromechanical coupling characteristic test method of fiber, interface and matrix in the currently disclosed technical data, so it is impossible to obtain the key interface, matrix resistivity and component electromechanical response characteristics. The main reason is that the current CMCs samples, even fiber bundle composite samples, are still relatively complex in components and structure, and it is difficult to accurately obtain parameters such as the cross-sectional area, length and damage mode of each component, and it is difficult to extract the performance parameters of a single component. There is only a test device and method for testing the online electromechanical response of silicon carbide monofilaments through a single fiber strength meter proposed by Xie Chuyang and others from Nanjing University of Aeronautics and Astronautics, which is used to test the electromechanical response characteristics of only fiber monofilaments (a fiber monofilament electromechanical response online test device and test method, CN114486525A). At the same time, the size of the fiber monofilament is very small, with a diameter of only 10 to 15 microns, and a breaking load of only 0.02 to 0.05 Newtons. The small size and low strength make it even more difficult to prepare measurable interface and matrix components based on the fiber monofilament.
[0004] Therefore, it is necessary to design a method for preparing ceramic-based monofilament composite materials, prepare monofilament composite materials with only a single fiber as the reinforcement phase, an interface, and a matrix, and design matching resistivity and electromechanical response test methods for the fiber, interface, and matrix components. This method can accurately measure the cross-sectional area and length of the fiber, interface, and matrix while keeping the damage mode simple, and thus accurately obtain the resistivity and elastic modulus characteristics of the components. Summary of the invention
[0005] In view of the problems existing in the prior art, the present invention provides a device and method for preparing a ceramic-based monofilament composite material and a method for testing the mechanical and electrical parameters of its components.
[0006] In order to achieve the above technical purpose, the technical solution adopted by the present invention is:
[0007] A device for preparing ceramic-based monofilament composite materials comprises a base plate, positioning bolts and gaskets. The positioning bolts are arranged in groups of two and are fixed on the base plate. A plurality of gaskets are sleeved on each positioning bolt. In the same group, the number of gaskets and the installation height of the gaskets on the two positioning bolts are the same. The two ends of a fiber monofilament used to prepare the ceramic-based monofilament composite material are respectively placed between the upper and lower gaskets of the two positioning bolts in the same group, and the gaskets clamp and fix the ends of the fiber monofilament.
[0008] Furthermore, the positioning bolt is a bolt, and an even number of positioning holes matching the positioning bolts are opened on the base plate. The gasket is provided with a gasket through-hole for the positioning bolts to pass through. The lower end of the positioning bolt is inserted into the positioning hole on the base plate for fixation. A thread is provided on the gasket through-hole, and the gasket can move up and down on the positioning bolt by rotation.
[0009] Furthermore, the base plate, the positioning bolts and the gaskets are all made of high temperature resistant graphite material or ceramic material.
[0010] A method for preparing a ceramic-based monofilament composite material, using a ceramic-based monofilament composite material preparation device, comprises the following steps:
[0011] Step 1: Install the gasket on the positioning bolt, determine the number of gaskets to be assembled according to the length of the positioning bolt and the number of ceramic-based monofilament composite materials to be prepared, and assemble the positioning bolt with the gasket installed on the bottom plate;
[0012] Step 2: Take a fiber bundle that is slightly longer than twice the distance between the positioning pins in the same group, remove the sizing agent on the surface of the fiber bundle according to the required degumming process, and take out the degummed fiber monofilaments;
[0013] Step 3: Fold the fiber monofilament in half, pass it through the middle section between the two lowest gaskets on a positioning bolt, and pass the two ends of the fiber monofilament through the two lowest gaskets on another positioning bolt in the same group, and tighten the two gaskets to clamp the fiber monofilament therebetween;
[0014] Step 4: Use the method in step 3 to wind the fiber monofilament between each gasket in turn and tighten the corresponding gasket until the top group of gaskets;
[0015] Step 5: prepare the required interface or matrix component material on the surface of the fiber monofilament between the two positioning pins in the same group; after the preparation is completed, cut the fiber monofilament from the gasket to obtain a ceramic-based monofilament composite material.
[0016] In step five, the desired interface or matrix component material is prepared on the surface of the fiber monofilament by chemical vapor deposition or precursor impregnation and pyrolysis.
[0017] The fiber monofilament is carbon fiber, silicon carbide fiber, oxide fiber or glass fiber.
[0018] The interface is pyrolytic carbon, boron nitride, silicon carbide interface or multi-layer composite interface, and the matrix is silicon carbide or carbon matrix.
[0019] A method for testing mechanical and electrical parameters of components of a ceramic-based monofilament composite material, which tests the mechanical and electrical parameters of components of a ceramic-based monofilament composite material, specifically comprises the following steps:
[0020] Step S1, bonding the two ends of the ceramic-based monofilament composite material to a C-shaped paper sheet through a conductive adhesive, and bonding two wires at the two ends of the C-shaped paper sheet as electrodes, waiting for the conductive adhesive to solidify, and then coating the bonding part of the ceramic-based monofilament composite material with quick-drying adhesive to supplement the bonding strength, and the exposed part of the center of the ceramic-based monofilament composite material without glue bonding is the test section;
[0021] Step S2, using an electronic tensile testing machine to clamp the C-shaped paper piece, and after clamping, cutting off the connecting part of the C-shaped paper piece to separate it, connecting the electrode to the electrical measuring instrument, and starting the electronic tensile testing machine to gradually break the ceramic-based monofilament composite material. In this process, the electrical measuring instrument correspondingly measures the electromechanical response characteristic data of the ceramic-based monofilament composite material;
[0022] Step S3, observing the broken ceramic-based monofilament composite material after being pulled apart using a scanning electron microscope to measure the fracture morphology and the radius of each component;
[0023] Step S4: Calculate and obtain the resistivity, modulus and electromechanical response characteristic data of each component, specifically:
[0024] Calculate the interface resistivity and matrix resistivity. When the fiber single-filament resistivity ρ is known f , fiber single filament radius r f , the interface radius r is measured i , base radius r m , the length of the ceramic-based monofilament composite material test section L, the initial resistance R of the ceramic-based monofilament composite material, all components can be regarded as parallel circuits to prepare the fiber monofilament + interface ceramic-based monofilament composite material and the fiber monofilament + matrix ceramic-based monofilament composite material respectively. The specific expression is as follows:
[0025] or
[0026]
[0027] or
[0028] In the formula, R i is the interface component resistance, R m is the matrix component resistance, R r is the contact resistance between different components due to contact, ρ i is the interface resistivity, ρ m is the substrate resistivity, R f is the single fiber resistance,
[0029] Calculate the interface modulus and matrix modulus, and obtain the fiber single fiber modulus E in advance f After the initial modulus E of the ceramic-based monofilament composite material is measured experimentally, the interface modulus E can be calculated. i and matrix modulus E m , the specific expression is as follows:
[0030] E=f f E f +f i E i Or E = f f E f +f m E m
[0031] Among them, f f is the volume fraction of the fiber, f i is the interface volume fraction, f m is the matrix volume fraction:
[0032] or
[0033] f f =1-f i or f =1-f m
[0034] Then we can know that:
[0035] or
[0036] The electrical measuring instrument is a digital multimeter or an electronic source meter or an AC impedance meter. The measured mechanical and electrical response characteristic data of the ceramic-based monofilament composite material include force-resistance, force-volt-ampere characteristics and force-impedance characteristics.
[0037] The conductive glue is quick-drying conductive silver glue, and the quick-drying glue is 401 glue.
[0038] Compared with the prior art, the present invention has the following beneficial effects:
[0039] 1. The present invention provides a ceramic-based single-filament composite material preparation tool combined with a ceramic-based single-filament composite material preparation method, which realizes the preparation of a ceramic-based composite material reinforced with only one fiber single filament, solving the problem that the components and structure of traditional fiber bundle composite materials are complex and it is difficult to extract the electrical and mechanical parameters of the components.
[0040] 2. The present invention provides a ceramic-based monofilament composite material preparation tool combined with a ceramic-based monofilament composite material preparation method. Compared with the traditional fiber bundle composite material preparation, only a few fiber monofilaments are needed, resulting in less material consumption, and the thin thickness of the components reduces the preparation cycle by more than half. At the same time, the preparation tool can be reused, which is more green and environmentally friendly.
[0041] 3. The present invention provides a method for testing the electromechanical parameters of components of a ceramic-based single-filament composite material, which can clearly determine the resistivity, modulus, and electromechanical response characteristics of the component materials based on the single-filament composite material, so that the component parameter measurements have a unified standard, improves the comparability of experimental data, and does not require expensive experimental equipment and complex experimental techniques, with high efficiency and low cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 It is a schematic diagram of an explosion of a tooling for preparing a ceramic-based monofilament composite material according to the present invention.
[0043] Figure 2 It is a schematic diagram of the fiber monofilament after being wound onto the preparation tooling.
[0044] Figure 3 This is a schematic diagram of the mechanical and electrical response test of ceramic-based single-filament composite materials.
[0045] Figure 4 SEM and EDS images of the monofilament composite material prepared by the method of the present invention
[0046] Among them, 1-base plate, 2-positioning bolt, 3-gasket, 4-fiber monofilament, 301-conducting wire, 302-C-shaped paper sheet, 303-conductive glue, 304-quick-drying glue, 305-ceramic-based monofilament composite material, 306-silicon carbide fiber, 307-pyrolytic carbon interface. DETAILED DESCRIPTION
[0047] The technical solution of the present invention is further explained below in conjunction with the accompanying drawings.
[0048] Base plate 1, bolt 2, threaded gasket 3, fiber monofilament 4, conductor 301, C-shaped paper 302, conductive adhesive 303, quick-drying adhesive 304, ceramic-based ceramic-based monofilament composite material 305, silicon carbide fiber 306, pyrolytic carbon interface 307
[0049] like Figure 1As shown, a ceramic-based ceramic-based monofilament composite material 305 preparation tool includes a base plate 1, bolts 2, and gaskets 3, all of which are made of graphite material.
[0050] The bottom plate 1 is provided with four evenly spaced threaded holes, with a spacing of 12 cm between adjacent threaded holes. Bosses are provided at the threaded holes so that the lowest gasket 3 is at a distance from the upper surface of the bottom plate, which is convenient for subsequent winding of the fiber monofilament 4 .
[0051] Bolt 2 is an M10 threaded bolt, and gasket 3 is matched with it. Two adjacent bolts 2 are used to wind fiber monofilament 4. The bolt diameter can be changed according to actual needs. Bolts with smaller diameters can save space on the bottom plate to arrange more bolts, but fiber monofilament 4 is more likely to bend and break when wound.
[0052] Seven washers 3 can be installed on the bolt 2, so that 12 monofilaments can be wound and 24 ceramic-based monofilament composite materials 305 can be prepared.
[0053] like Figure 2 As shown, a method for preparing a ceramic-based ceramic-based monofilament composite material should include the following steps:
[0054] Tighten the seven washers 3 onto each bolt 2, and assemble the four bolts 2 with washers installed onto the base plate 1;
[0055] A 30 cm long silicon carbide fiber bundle is heated at 600°C for one hour to remove the glue, and a degummed fiber monofilament 4 is taken out therefrom;
[0056] Fold the fiber monofilament 4 in half, pass the middle section around the two lowest washers 3 on one bolt 2, and pass the two ends of the fiber monofilament 4 around the two lowest washers 3 on another adjacent bolt 2, and tighten the two washers to clamp the fiber monofilament 4 therebetween;
[0057] In the same way, wind the fiber monofilaments 4 upwards in sequence and tighten the corresponding gaskets until the top group of gaskets is wound, and a total of 12 fiber monofilaments 4 are wound;
[0058] A layer of pyrolytic carbon interface phase is prepared on the surface of the fiber monofilament 4 by using a chemical vapor deposition method;
[0059] After the preparation is completed, the 24 ceramic-based ceramic-based monofilament composite materials 305 are cut from the tooling to complete the preparation.
[0060] like Figure 3 As shown:
[0061] The ceramic-based ceramic-based monofilament composite material 305 is bonded to the C-shaped paper sheet 302 through the conductive glue 303, and two wires 301 are bonded to the two ends of the paper sheet as electrodes. After the conductive glue 303 is cured, quick-drying glue 304 is applied to the bonding place of the ceramic-based monofilament composite material 305 to supplement the bonding strength. The exposed part in the center of the sample without glue bonding is the test section length;
[0062] The C-shaped paper piece 302 is clamped by an electronic tensile testing machine, and after clamping, the connecting part of the paper piece is cut off to separate the paper piece, and the electrode is connected to a digital multimeter to measure the static resistance of the ceramic-based monofilament composite material 305 to obtain the initial resistance value;
[0063] Start the electronic tensile testing machine and electrical measuring instrument at the same time to make the force and electrical data correspond;
[0064] The broken specimens were observed under a microscope to measure the fracture morphology and the radius of each component.
[0065] According to the obtained force, displacement and resistance data, the resistivity, modulus and electromechanical response characteristic data of each component are calculated and obtained.
[0066] The resistivity of the pyrolytic carbon interface 307 is given by the resistivity of the silicon carbide fiber 306 f , radius r of silicon carbide fiber 306 f , the radius r of the pyrolytic carbon interface 307 is measured i , the length of the test section of the ceramic-based monofilament composite material 305 is L, and the initial resistance of the ceramic-based monofilament composite material 305 is R. All components can be regarded as parallel circuits for calculation. At the same time, because the pyrolytic carbon interface has good contact with the fiber, the contact resistance can be regarded as zero. The specific expression is as follows:
[0067]
[0068]
[0069] In the formula, R i is the pyrolytic carbon interface 307 resistance, ρ i is the resistivity of the pyrolytic carbon interface 307.
[0070] The material modulus can be calculated according to the law of mixtures. The modulus E of silicon carbide fiber 306 is obtained in advance. f After the initial modulus E of the ceramic-based ceramic-based monofilament composite material 305 is measured experimentally, the modulus E of the pyrolytic carbon interface 307 can be calculated. i , the specific expression is as follows:
[0071] E=f f E f +f i E i
[0072] Among them, f f is the fiber volume fraction, f i is the interface volume fraction:
[0073] or
[0074] f f =1-f i
[0075] Then we can know that:
[0076]
[0077] like Figure 4 As shown, the outer layer of the concentric circle structure is the pyrolytic carbon interface layer, and the center is the silicon carbide fiber.
[0078] In this embodiment, according to Figure 4 The radius r of the silicon carbide fiber 306 in the ceramic-based ceramic-based monofilament composite material 305 is measured. f =15.24um, pyrolytic carbon interface 307 radius r i =20.184um.
[0079] In this embodiment, the resistivity of silicon carbide fiber is f =1990Ω·mm, Ceramic-based ceramic-based monofilament composite material 305 test section length L = 19.7mm, R = 1886Ω,
[0080] Therefore, the resistivity ρ of the pyrolytic carbon interface 307 can be obtained i =0.19975Ω·mm.
[0081] The conductive glue 303 in this embodiment is quick-drying conductive silver glue, and the quick-drying glue 304 is 401 glue.
[0082] The above are only preferred embodiments of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should be regarded as the protection scope of the present invention.
Claims
1. A device for preparing a ceramic-based monofilament composite material, characterized in that: The invention comprises a base plate (1), positioning bolts (2) and gaskets (3), wherein the positioning bolts (2) are arranged in groups of two and fixed on the base plate (1), and each positioning bolt (2) is provided with a plurality of gaskets (3). In the same group, the number of gaskets and the installation height of the gaskets on the two positioning bolts (2) are the same. The two ends of a fiber monofilament (4) used for preparing a ceramic-based monofilament composite material are respectively placed between the upper and lower gaskets (3) of the two positioning bolts (2) in the same group, and the gaskets (3) clamp and fix the ends of the fiber monofilament (4).
2. A ceramic-based monofilament composite material preparation device according to claim 1, characterized in that: The positioning bolt (2) is a bolt, an even number of positioning holes matching the positioning bolt (2) are formed on the base plate (1), a gasket through-hole is formed on the gasket (3) for the positioning bolt (2) to pass through, the lower end of the positioning bolt (2) is inserted into the positioning hole on the base plate (1) for fixing, a thread is provided on the gasket through-hole, and the gasket (3) can move up and down on the positioning bolt (2) by rotating.
3. The device for preparing a ceramic-based monofilament composite material according to claim 1, characterized in that: The base plate (1), positioning bolts (2) and gaskets (3) are all made of high-temperature resistant graphite material or ceramic material.
4. A method for preparing a ceramic-based monofilament composite material, characterized in that: The use of a ceramic-based monofilament composite material preparation device as claimed in claim 1 comprises the following steps: Step 1: Install the gasket (3) on the positioning bolt (2), determine the number of gaskets (3) to be installed according to the length of the positioning bolt (2) and the number of ceramic-based monofilament composite materials to be prepared, and install the positioning bolt (2) with the gasket (3) installed on the bottom plate (1); Step 2: Take a fiber bundle slightly longer than twice the distance between the positioning pins (2) in the same group, remove the sizing agent on the surface of the fiber bundle according to the required degumming process, and take out the degummed fiber monofilament (4) therefrom; Step 3, fold the fiber monofilament (4) in half, pass the middle section around the two lowest gaskets (3) on a positioning bolt (2), and pass the two ends of the fiber monofilament (4) around the two lowest gaskets (3) of another positioning bolt (2) in the same group, and tighten the two gaskets (3) to clamp the fiber monofilament (4) therebetween; Step 4: Using the method of step 3, wind the fiber monofilament (4) between each gasket (3) in turn and tighten the corresponding gasket (3) until the top group of gaskets is reached; Step 5: prepare the required interface or matrix component material on the surface of the fiber monofilament (4) between the two positioning bolts (2) in the same group; after the preparation is completed, cut the fiber monofilament (4) from the gasket (3) to obtain a ceramic-based monofilament composite material.
5. The method for preparing a ceramic-based monofilament composite material according to claim 4, characterized in that: In step five, the required interface or matrix component material is prepared on the surface of the fiber monofilament (4) by using chemical vapor deposition or precursor impregnation and pyrolysis method.
6. The method for preparing a ceramic-based monofilament composite material according to claim 4, characterized in that: The fiber monofilament (4) is carbon fiber, silicon carbide fiber, oxide fiber or glass fiber.
7. The method for preparing a ceramic-based monofilament composite material according to claim 4, characterized in that: The interface is a pyrolytic carbon, boron nitride, silicon carbide interface or a multi-layer composite interface, and the matrix is a silicon carbide or carbon matrix.
8. A method for testing the electromechanical parameters of ceramic-based monofilament composite materials, characterized by: The component electromechanical response test is performed on the ceramic-based monofilament composite material prepared as claimed in claim 4, specifically comprising the following steps: Step S1, bonding two ends of the ceramic-based monofilament composite material (305) to a C-shaped paper sheet (302) through a conductive adhesive (303), bonding two wires (301) to the two ends of the C-shaped paper sheet (302) as electrodes, waiting for the conductive adhesive (303) to solidify, and then coating the bonding position of the ceramic-based monofilament composite material (305) with quick-drying adhesive (304) to increase the bonding strength, and the exposed portion of the center of the ceramic-based monofilament composite material (305) without adhesive bonding is the test section; Step S2, using an electronic tensile testing machine to clamp the C-shaped paper piece (302), and after clamping, cutting off the connecting part of the C-shaped paper piece (302) to separate them, connecting the electrodes to an electrical measuring instrument, and starting the electronic tensile testing machine to gradually break the ceramic-based monofilament composite material (305). During this process, the electrical measuring instrument correspondingly measures the electromechanical response characteristic data of the ceramic-based monofilament composite material (305); Step S3, observing the broken ceramic-based monofilament composite material (305) using a scanning electron microscope to measure the fracture morphology and the radius of each component; Step S4: Calculate and obtain the resistivity, modulus and electromechanical response characteristic data of each component, specifically: Calculate the interface resistivity and matrix resistivity. Given the resistivity of the fiber (4) ρ f , fiber monofilament (4) radius r f , the interface radius r is measured i , base radius r m , the length of the test section of the ceramic-based monofilament composite material (305) L, the initial resistance R of the ceramic-based monofilament composite material (305), all components can be regarded as parallel circuits to prepare the fiber monofilament + interface ceramic-based monofilament composite material (305) and the fiber monofilament + matrix ceramic-based monofilament composite material (305) respectively, and the specific expression is as follows: or or In the formula, R i is the interface component resistance, R m is the matrix component resistance, R r is the contact resistance between different components due to contact, ρ i is the interface resistivity, ρ m is the substrate resistivity, R f is the resistance of the fiber single filament (4), Calculate the interface modulus and matrix modulus, and obtain the fiber single fiber modulus E in advance f After the initial modulus E of the ceramic-based monofilament composite material (305) is measured experimentally, the interface modulus E can be calculated. i and matrix modulus E m , the specific expression is as follows: E = f f E f +f i E i Some E=f f E f +f m E m Among them, f f is the volume fraction of the fiber, f i is the interface volume fraction, f m is the matrix volume fraction: or f f =1-f i or f =1-f m Then we can know that: or 9. A method for testing mechanical and electrical parameters of ceramic-based monofilament composite material components according to claim 8, characterized in that: The electrical measuring instrument is a digital multimeter or an electronic source meter or an AC impedance meter, and the measured force-electric response characteristic data of the ceramic-based monofilament composite material (305) include force-resistance, force-volt-ampere characteristics and force-impedance characteristics.
10. The method for testing mechanical and electrical parameters of ceramic-based monofilament composite material components according to claim 8, characterized in that: The conductive glue (303) is quick-drying conductive silver glue, and the quick-drying glue (304) is 401 glue.