Method for measuring packaging performance of optical cement particles of display module
By placing detection particles on the cover of the display module or the main display screen and evaluating the particle wrapping performance of the optical glue, the bubble problem caused by poor optical glue particle wrapping performance is solved, and the appearance quality and customer satisfaction of the display module are improved.
Patent Information
- Application Number
- CN202410717694.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-04
- Publication Date
- 2024-10-01
AI Technical Summary
It is difficult to effectively evaluate and solve the bubble problem caused by poor packaging performance of display module optical glue particles with existing technology, leading to consumer returns and reduced brand recognition.
Divide the detection particles into several detection areas by placing the detection particles on the cover or the visible area of the main display screen, covering the optical glue and performing bubble treatment and UV curing after lamination. Count the number of bubbles and calculate the bubble occurrence rate to evaluate the performance of the optical glue. Particle wrapping performance.
This method can evaluate the particle wrapping performance before the introduction of new optical glue, reduce bubble problems, reduce customer complaints, and ensure the appearance quality of the display module.
Smart Images

Figure HDA0004876046660000011 
Figure HDA0004876046660000012 
Figure HDA0004876046660000021
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of display module bonding, and more specifically, to a method for measuring the packaging performance of optical adhesive particles of a display module. Background Art
[0002] OCA (Optically Clear Adhesive) optical glue is one of the important raw materials for touch screens. OCA optical glue is mainly used for bonding materials on touch screens to achieve the effect of capacitive touch sensing. It has the characteristics of high clarity, strong light transmittance (total light transmittance>99%), high adhesion, water and high temperature resistance, UV resistance, good bonding strength and small curing shrinkage.
[0003] Mobile phone display modules are assembled by bonding the cover plate and the main display screen together with optical glue. Since it is difficult for the bonding clean room to be 100% dust-free, fine particles in the air may fall onto the surface of the optical glue when the cover plate and the main display screen are bonded and wrapped by the optical glue. For particles with larger particle sizes, such as those above 100μm, they are easily identified and picked out by the naked eye during visual inspection, while for particles with smaller particle sizes, especially those below 50μm, they cannot be identified by the naked eye after being wrapped by the optical glue and are easy to flow into the market. As time goes by, the stress concentrated near the particles is released, forming bubbles that gather, resulting in poor appearance bubbles, which are noticed by consumers, resulting in returns and reducing consumers' recognition of the brand. The current specific preventive measures are, on the one hand, to improve the level of clean rooms, and on the other hand, to continuously upgrade the defoaming technology during the bonding process.
[0004] For example, Chinese invention patent CN107340943B discloses a capacitive touch screen and bonding method, which includes: step 1, applying an OCA optical adhesive layer on the surface of a film sensor; step 2, punching a through hole in the thickness direction of the film sensor with the OCA optical adhesive layer in step 1, so that one end of the through hole is in the ink step difference area; step 3, cutting the film sensor in step 2 according to the specification size by a film cutting machine; step 4, bonding the cut film sensor to the protective glass; step 5, defoaming the bonded film sensor and protective glass. However, if the particle wrapping performance of the optical adhesive is poor, even if the bubbles are temporarily eliminated, they will reappear over time.
[0005] Therefore, it is urgent to propose a method for measuring the packaging performance of display module optical adhesive particles, so that display module manufacturers can first evaluate the packaging performance of newly imported optical adhesive particles when introducing new optical adhesives, and solve the fundamental problem from the source. Summary of the invention
[0006] Based on this, it is necessary to provide a method for measuring the packaging performance of optical adhesive particles in display modules in response to the above technical problems, and to evaluate the packaging performance when introducing new optical adhesives.
[0007] In order to solve the above technical problems, the present invention provides a method for measuring the packaging performance of optical adhesive particles of a display module, which adopts the following technical solution: A method for measuring the packaging performance of optical adhesive particles of a display module comprises the following steps: Step 100: Divide the visible area of the cover into several detection areas or / and divide the area corresponding to the main display screen and the visible area of the cover into several detection areas, and place detection particles in each detection area; Step 200: Apply optical adhesive to the visible area of the cover plate or the position corresponding to the main display screen and the visible area of the cover plate; Step 300: completing the bonding of the display main screen and the cover plate, and counting the detection particles in each detection area, the count is A; Step 400: placing the bonded display module into a baking oven for bubble treatment; Step 500: UV curing the display module; Step 600: Selecting display module samples without bubbles to perform reliability testing; Step 700: Count the number of bubbles in each detection area, and the count is B; Step 800: Calculate the bubble occurrence rate C = B / A*100% in each detection area and calculate the average C avg .
[0008] Further, step 100: divide the visible area of the cover plate into several detection areas and divide the area corresponding to the main display screen and the visible area of the cover plate into several detection areas equivalent to the visible area of the cover plate, and place detection particles in each detection area; step 300: after the cover plate and the main display screen are attached to each other, the detection area division of the visible area of the cover plate overlaps with the detection area division of the main display screen, and the number of particles of the detection particles in each overlapping detection area is calculated, and the count is A.
[0009] Furthermore, the particle size of the detection particles is 20-50 μm.
[0010] Furthermore, the detection particles are any one of fluorescent glass beads, glass beads or PET particles.
[0011] Furthermore, the thickness of the optical adhesive is 100-175 μm.
[0012] Furthermore, the detection particles or bubbles on the visible area of the cover are counted by a two-dimensional magnifying device.
[0013] Furthermore, in step 400, the baking temperature is set to 20-30°C, the baking pressure is set to 0.2-0.4 MPa, and the baking time is 5-20 min.
[0014] Furthermore, the energy of the UV furnace is 2000~3000MJ.
[0015] Furthermore, the reliability test of the display module is one or more of a thermal shock test, a high temperature test, a high temperature and high humidity test, and a low temperature test.
[0016] Furthermore, the counted number of bubbles B only includes the bubbles that wrap the detection particles, and does not include bubbles generated by other reasons.
[0017] Compared with the prior art, the present invention has the following beneficial effects: The present invention provides a method for determining the packaging performance of optical adhesive particles of a display module. By using detection particles to simulate environmental particles in an actual production process, the environmental particles are considered to be on one side of a cover plate or on one side of a display main screen, and to appear on one side of a cover plate and on one side of a display main screen at the same time. Before the new optical adhesive is introduced into actual production, the particle packaging performance of the optical adhesive is first evaluated. Finally, the evaluation result is verified using PET environmental particles commonly used in actual production. This proves that the method for determining the packaging performance of optical adhesive particles of a display module provided by the present invention is consistent with the results of actual production conditions. When applied to the manufacturing process, it can avoid the bubble problem caused by poor packaging performance of optical adhesive particles, and greatly reduce customer complaints about display modules caused by bubbles. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the solutions in the present application or the prior art, a brief introduction is given below to the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0019] Figure 1 This is a schematic diagram of the placement of detection particles in Example 1 of the present invention; Figure 2 This is a schematic diagram of the placement of detection particles in Example 2 of the present invention; Figure 3 This is a schematic diagram of the placement of detection particles in Example 3 of the present invention; Figure 4 Schematic diagram of the detection area division of the cover plate and the visible area of the cover plate according to an embodiment of the present invention.
[0020] Reference numerals: Cover plate 1, cover plate visible area 11, optical glue 2, detection particles 3, display main screen 4. DETAILED DESCRIPTION
[0021] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0022] In the description of the present invention, it should be understood that the terms "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside" and "outside" etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.
[0023] In addition, the terms "first", "second", and "third" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first", "second", and "third" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0024] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the accompanying drawings.
[0025] like Figures 1 to 4 As shown, this embodiment proposes a method for measuring the packaging performance of optical adhesive particles of a display module, wherein the display module includes a cover plate 1 and a display main screen 4, wherein the cover plate 1 and the display main screen 4 are adhered by optical adhesive 2, wherein a transparent visual area 11 is provided in the middle of the cover plate 1, so that the bubbles inside the optical adhesive 2 can be observed.
[0026] The method for measuring the packaging performance of optical adhesive particles of a display module comprises the following steps: Step 100: Figure 1 and 4 As shown, the visible area 11 of the cover is divided into a number of detection areas, and the same number of detection particles 3 are placed as evenly as possible in each visible area.
[0027] In this embodiment, the cover plate visible area 11 is divided into 9 detection areas. The detection particles 3 are glass beads treated with fluorescence, which are convenient for counting under fluorescence irradiation. The particle size of the fluorescent glass beads is 20 μm. Glass beads can also be used directly.
[0028] Step 200: Apply optical glue 2 to the visible area 11 of the cover plate, wherein the thickness of the optical glue 2 is 150 μm. The optical glue 2 used in this step is MPI G6.2 OCA optical glue produced by Mitsubishi Chemical Corporation of Japan.
[0029] Step 300: The display main screen 4 is bonded to the cover plate 1 with the optical glue 2 attached thereto. After the bonding is completed, the detection particles 3 in each detection area are counted. In this embodiment, a two-dimensional magnifying device is used to assist in counting the detection particles 3 on the visible area 11 of the cover plate. A magnifying glass, a microscope and other equipment may also be used for auxiliary counting. The number of detection particles 3 in a single detection area is recorded as A.
[0030] Step 400: placing the bonded display module into a baking oven for a bubbling treatment, wherein the baking temperature is set at 30° C., the baking pressure is set at 0.3 MPa, and the baking time is 10 minutes.
[0031] Step 500: UV curing the display module after the bubble treatment, setting the UV oven energy to 2500MJ.
[0032] Step 600: Select display module samples that do not generate bubbles for reliability testing. In this step, the reliability test of the display module is to conduct a 48-hour hot and cold shock test (-40℃~85℃), a 240-hour high temperature test (85℃), a 240-hour high temperature and high humidity test (65℃*95%RH) and a 240-hour low temperature test (-40℃) on the samples. You can also select one or more of these reliability tests according to actual production needs.
[0033] Step 700: Count the number of bubbles in each detection area, and the obtained number of bubbles is recorded as B. In this step, only the bubbles containing the detection particles are counted.
[0034] In this step, a two-dimensional magnifying device is also used to magnify and count the number of bubbles in each detection area on the cover plate visible area 11. The counted number of bubbles is only the bubbles that wrap the detection particles 3, and does not include bubbles generated by other reasons.
[0035] Step 800: Calculate the bubble generation rate C of each detection area, where C=B / A*100%. The number of bubbles B generated by the detection particles 3 in each detection area divided by the number of detection particles 3 added in each detection area is the bubble generation rate C. The bubble generation rate C of each detection unit is averaged to C. avgThat is, the average bubble occurrence rate of the optical adhesive 2 is obtained, wherein the lower the average bubble occurrence rate, the better the particle foreign matter encapsulation performance of the optical adhesive 2, and conversely, the greater the average bubble occurrence rate, the worse the particle foreign matter encapsulation performance of the optical adhesive 2.
[0036] This embodiment simulates the situation of environmental particles on one side of the cover plate during the actual production and assembly process. The results are shown in Table 1 below. The average bubble generation rate C avg It is 9.31%.
[0037] Table 1: Test results of optical adhesive particle packaging performance of display module in Example 1 This embodiment provides a method for measuring the packaging performance of optical adhesive particles of a display module, which differs from the embodiment 1 in that: Step 100: Figure 2 As shown, the area corresponding to the main display screen 4 and the cover plate visible area 11 is divided into a plurality of detection areas, and the same number of detection particles 3 are evenly placed in each area divided by the main display screen 4 .
[0038] Step 200: Cover the optical adhesive 2 on the display main screen 4, wherein the thickness of the optical adhesive 2 is 150 μm.
[0039] Step 300: The cover plate 1 is bonded with the optical adhesive 2. After the bonding is completed, the number of detection particles 3 in each detection area is counted as A.
[0040] This embodiment simulates the situation of environmental particles on one side of the display main screen 4 during the actual production and assembly process. The detection results are shown in Table 2 below. The average bubble generation rate C avg It is 10.02%.
[0041] Table 2: Test results of optical adhesive particle packaging performance of display module in Example 2 This embodiment provides a method for measuring the packaging performance of optical adhesive particles of a display module, which differs from the embodiment 1 in that: Step 100: Figure 3 As shown, the cover plate visible area 11 is divided into several detection areas, and an equal number of detection particles 3 are evenly placed in each detection area; the area corresponding to the cover plate visible area 11 of the display main screen 4 is equally divided into several detection areas with the cover plate visible area 11, and an equal number of detection particles 3 are evenly placed in each detection area divided by the display main screen 4.
[0042] Step 200: Cover the visible area 11 of the cover plate with optical adhesive 2, wherein the thickness of the optical adhesive 2 is 150 μm.
[0043] Step 300: The cover plate 1 with the optical adhesive 2 attached is bonded to the main display screen 4. After bonding, the detection area division of the cover plate visible area 11 overlaps with the detection area division of the main display screen 4. The number of particles of the detection particles 3 in each detection area is calculated, and the count is A.
[0044] Step 700: Count the number of bubbles in each overlapping detection area, and the obtained number of bubbles is recorded as B. In this step, only the bubbles containing the detection particles are counted.
[0045] Step 800: Calculate the bubble occurrence rate C in each detection area, where C=B / A*100%, and then calculate the average C avg .
[0046] This embodiment simulates the situation in which environmental particles exist in both the cover plate 1 and the display main screen 4 during the actual production and assembly process. The detection results are shown in Table 3 below. The average bubble occurrence rate Cavg is 11.79%.
[0047] Table 3: Test results of optical adhesive particle packaging performance of display module in Example 3 This embodiment provides a method for measuring the packaging performance of optical adhesive particles of a display module. The difference between this embodiment and embodiment 1 is that: The detection particles 3 used in step 100 are 40 μm fluorescent glass beads; The thickness of the optical adhesive 2 used in step 200 is 100 μm; In step 400, the baking temperature is set to 40°C, the baking pressure is set to 0.2MPa, and the baking time is 5min; In step 500, the UV furnace energy is set to 2000 MJ.
[0048] The test results of this embodiment are shown in Table 4 below, and the average bubble occurrence rate is 13.31%.
[0049] Table 4: Test results of optical adhesive particle packaging performance of display module in Example 4 This embodiment provides a method for measuring the packaging performance of optical adhesive particles of a display module. The difference between this embodiment and embodiment 1 is that: The detection particles 3 used in step 100 are 50 μm fluorescent glass beads; The thickness of the optical adhesive 2 used in step 200 is 175 μm; In step 400, the baking temperature is set to 20°C, the baking pressure is set to 0.4 MPa, and the baking time is 20 minutes.
[0050] In step 500, the UV furnace energy is set to 3000 MJ.
[0051] The test results of this embodiment are shown in Table 5 below: avg It is 10.35%.
[0052] Table 5: Test results of optical adhesive particle packaging performance of display module in Example 5 Comparative Example 1 This comparative example proposes a method for measuring the packaging performance of optical adhesive particles of a display module. The difference between this comparative example and Example 1 is only that: The optical adhesive 2 used in step 200 is optical adhesive A purchased on the market.
[0053] The test results of this comparative example are shown in Table 6 below. The average bubble generation rate C avg It is 29.06%.
[0054] Table 6: Comparative Example 1 shows the test results of the optical adhesive particle packaging performance of the module Comparative Example 2 This comparative example proposes a method for measuring the packaging performance of optical adhesive particles of a display module. The difference between this comparative example and Example 1 is only that: The optical adhesive 2 used in step 200 is optical adhesive B purchased on the market.
[0055] The test results of this comparative example are shown in Table 7 below. The average bubble generation rate C avg It is 43.77%.
[0056] Table 7: Comparative Example 2 shows the test results of the optical adhesive particle packaging performance of the module Verification Example PET debris commonly seen in the actual assembly process is used as the detection particle 3, and the particle size of the PET debris is controlled at 20~50μm. The optical glue 2 used in Example 1, Comparative Example 1 and Comparative Example 2 is taken respectively, and the particle packaging performance of the optical glue is tested according to the method described in Example 1. The test results are shown in Table 8 below. The PET debris commonly seen in the actual production and assembly process is used for verification. Since the PET debris is irregular in shape, the overall bubble rate will increase slightly, but the average bubble incidence rate results of the three optical glues are basically consistent with the trend results of the previous Example 1 and Comparative Example 1 and Comparative Example 2. Therefore, the display module optical glue particle packaging performance detection method proposed in the present invention can be applied to the actual production process to detect the particle packaging performance of the newly introduced optical glue.
[0057] Table 8: Verification example shows the test results of the module optical adhesive particle packaging performance Obviously, the embodiments described above are only some embodiments of the present application, rather than all embodiments. The preferred embodiments of the present application are given in the accompanying drawings, but they do not limit the patent scope of the present application. The present application can be implemented in many different forms. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive. Although the present application is described in detail with reference to the aforementioned embodiments, for those skilled in the art, it is still possible to modify the technical solutions recorded in the aforementioned specific implementation methods, or to perform equivalent replacement of some of the technical features therein. Any equivalent structure made using the contents of the specification and drawings of this application, directly or indirectly used in other related technical fields, is similarly within the scope of patent protection of this application.
Claims
1. A method for measuring the encapsulation performance of optical adhesive particles of a display module, characterized in that: The following steps are involved: Step 100: Divide the cover plate visible area (1) into a plurality of detection areas or / and divide the area corresponding to the display main screen (4) and the cover plate visible area (11) into a plurality of detection areas, and place detection particles (3) in each detection area; Step 200: applying optical adhesive (2) to the visible area (11) of the cover plate or the position of the display main screen (4) corresponding to the visible area (11) of the cover plate; Step 300: completing the bonding of the display main screen (4) and the cover plate (1), and counting the detection particles (3) in each detection area, the count being A; Step 400: placing the bonded display module into a baking oven for bubble treatment; Step 500: UV curing the display module; Step 600: Selecting display module samples without bubbles to perform reliability testing; Step 700: Count the number of bubbles in each detection area, and the count is B; Step 800: Calculate the bubble occurrence rate C = B / A*100% in each detection area and calculate the average C avg .
2. The method for measuring the packaging performance of optical adhesive particles of a display module according to claim 1, characterized in that: Step 100: Divide the visible area of the cover plate (1) into a number of detection areas and divide the area corresponding to the display main screen (4) and the visible area of the cover plate (11) into a number of detection areas that are equal to the visible area of the cover plate (11), and place detection particles (3) in each detection area; Step 300: After the cover plate (1) and the display main screen (4) are attached, the detection area division of the cover plate visible area (11) overlaps with the detection area division of the display main screen (4), and the number of particles of the detection particles (3) in each overlapping detection area is calculated, and the count is A.
3. The method for measuring the packaging performance of optical adhesive particles of a display module according to claim 1, characterized in that: The particle size of the detection particles (3) is 20 to 50 μm.
4. The method for measuring the packaging performance of optical adhesive particles of a display module according to claim 1, characterized in that: The detection particles (3) are any one of fluorescent glass beads, glass beads or PET particles.
5. The method for measuring the packaging performance of optical adhesive particles of a display module according to claim 1, characterized in that: The thickness of the optical adhesive (2) is 100-175 μm.
6. The method for measuring the packaging performance of optical adhesive particles of a display module according to claim 1, characterized in that: The detection particles (3) or bubbles are counted by a two-dimensional amplification device.
7. The method for measuring the packaging performance of optical adhesive particles of a display module according to claim 1, characterized in that: In step 400, the baking temperature is set to 20-30°C, the baking pressure is set to 0.2-0.4 MPa, and the baking time is 5-20 minutes.
8. The method for measuring the packaging performance of optical adhesive particles of a display module according to claim 1, characterized in that: The energy of UV furnace is 2000~3000MJ.
9. The method for measuring the packaging performance of optical adhesive particles of a display module according to claim 1, characterized in that: The reliability test of the display module is one or more of a thermal shock test, a high temperature test, a high temperature and high humidity test, and a low temperature test.
10. The method for measuring the packaging performance of optical adhesive particles of a display module according to claim 1, characterized in that: The counted number of bubbles B only includes the bubbles enveloping the test particles (3), and does not include bubbles generated by other reasons.