Polarizing film
By adjusting the angle between the substrate and the polarizing film and controlling the refractive index difference, combined with the use of a hard coating, the problem of uneven interference caused by interface reflection in the polarizing film is solved, achieving efficient flatness and display effects.
Patent Information
- Application Number
- CN202410361281.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-12-19
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-01
AI Technical Summary
In existing polarizing films, the reflection of the incident light interface between the polarizing film and the alignment film and between the alignment film and the substrate is enhanced, leading to the problem of uneven interference.
By adjusting the slow axis direction of the base material and the absorption axis direction of the polarizing film to 45°±5°, and ensuring that the visible light refractive index difference between the polarizing film and the alignment film and between the alignment film and the base material is within 0.06, the interface is suppressed reflection. At the same time, a hard coating is added to the opposite side of the base material from the alignment film to prevent warping and ensure the flatness of the polarizing film.
It effectively suppresses uneven interface reflection interference caused by incident light, improves the flatness and display effect of the polarizing film, and is suitable for various display devices.
Smart Images

Figure CN118732124A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a polarizing film. Background Art
[0002] In flat panel display devices such as liquid crystal display devices and organic EL display devices, polarizing films are used for the purpose of optical compensation. Polarizing films are generally composed of a substrate, an orientation film, and a polarizing film stacked in this order.
[0003] In recent years, the demand for thinning of flat panel display devices has increased, and accordingly, the demand for thinning of polarizing films has also increased. As a thin polarizing film, there is a polarizing film described in Patent Document 1, for example. This conventional polarizing film is composed of a composition containing a polymerizable liquid crystal compound and a dichroic pigment. As a thin polarizing film, a polarizing film having an absorption axis in a direction inclined relative to the long side direction of the polarizing film is also known.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application No. 2007-510946 Summary of the invention
[0007] Problems to be solved by the invention
[0008] In the polarizing film as described above, if the interface reflection of incident light between the polarizing film and the alignment film and between the alignment film and the substrate increases, there is a problem that interference unevenness becomes noticeable.
[0009] The present invention has been made to solve the above-mentioned problems, and an object of the present invention is to provide a polarizing film capable of suppressing interference unevenness caused by interface reflection of incident light.
[0010] Means for solving problems
[0011] A polarizing film according to one aspect of the present invention is a polarizing film in which a substrate, an oriented film and a polarizing film are stacked in sequence, wherein the angle formed by the slow axis direction of the substrate and the absorption axis direction of the polarizing film is 45°±5°, the refractive index difference between the polarizing film and the oriented film with respect to visible light satisfies the following formula (1), and the refractive index difference between the oriented film and the substrate with respect to visible light satisfies the following formula (2).
[0012] |n(polarizing film)-n(oriented film)|≤0.06 (1)
[0013] |n(oriented film)-n(substrate)|≤0.06 (2)
[0014] (In formula (1), n(polarizing film) represents the refractive index in the transmission axis direction of the polarizing film.)
[0015] In the polarizing film, by suppressing the refractive index difference between the alignment film and the substrate and the refractive index difference between the alignment film and the substrate within the above range, the interface reflection of the incident light between the polarizing film and the alignment film and between the alignment film and the substrate can be suppressed. Therefore, in the polarizing film, the interference unevenness caused by the interface reflection of the incident light can be suppressed.
[0016] The thickness of the alignment film is preferably 10 nm to 400 nm. In this case, in a polarizing film having an alignment film thickness within this range, interference unevenness due to interface reflection of incident light can be preferably suppressed.
[0017] A hard coating layer may be adjacent to the surface of the substrate opposite to the alignment film. When making a polarizing film, it is believed that warping occurs on the substrate due to shrinkage when the polarizing film is cured, and wrinkles are generated in the obtained polarizing film. By having a hard coating layer adjacent to the surface of the substrate opposite to the alignment film, warping of the substrate relative to shrinkage when the polarizing film is cured can be suppressed, and wrinkles can be suppressed in the obtained polarizing film.
[0018] The substrate, the oriented film and the polarizing film may be long. In this case, a long polarizing film capable of suppressing the interference unevenness caused by the interface reflection of the incident light can be obtained. By continuously joining the polarizing film cut out from the long polarizing film to various display devices, a display device using the polarizing film in which the interference unevenness caused by the interface reflection of the incident light is suppressed can be efficiently manufactured.
[0019] The angle between the long side direction and the slow axis direction of the substrate is preferably 0°±5° or 90°±5°. Thus, a polarizing film having high ellipticity can be obtained.
[0020] Effects of the Invention
[0021] According to the present invention, it is possible to suppress interference unevenness caused by interface reflection of incident light. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] [ Figure 1 ] is a schematic diagram showing the layer structure of a polarizing film according to one embodiment of the present invention.
[0023] [ Figure 2 ] is a diagram showing the layer structure of the polarizing film of the embodiment and the comparative example.
[0024] [ Figure 3 ] is a graph showing the evaluation results of polarizing films of Examples and Comparative Examples. DETAILED DESCRIPTION
[0025] Hereinafter, preferred embodiments of a polarizing film according to one aspect of the present invention will be described in detail with reference to the accompanying drawings.
[0026] Figure 1 Schematic diagram showing the layer structure of a polarizing film according to one embodiment of the present invention. Figure 1 As shown, the polarizing film 1 is formed by sequentially laminating a substrate 2, an alignment film 3, and a polarizing film 4. In this embodiment, the substrate 2, the alignment film 3, and the polarizing film 4 are all long, forming the long polarizing film 1.
[0027] The long dimension includes any state of being wound into a roll and any state of being unwound from a roll. The length of the long side direction (extending direction of the polarizing film 1) of the long-sized polarizing film 1 is, for example, 10m to 3000m, preferably 100m to 200m. The length of the short side direction (the direction orthogonal to the extending direction of the polarizing film 1) of the long-sized polarizing film 1 is, for example, 0.1m to 5m, preferably 0.2m to 2m.
[0028] The long polarizing film 1 is cut into required sizes and used in various display devices. Examples of display devices include liquid crystal display devices, organic EL display devices, inorganic EL display devices, electron emission display devices, electronic paper, and piezoelectric ceramic displays. These display devices may be display devices that display 2D images or display devices that display 3D images.
[0029] The substrate 2 is made of resin, for example. The substrate 2 is particularly transparent to visible light, and has a transmittance of 80% or more to light with a wavelength of 380 nm to 780 nm. Considering practical operability and processability, the thickness of the substrate 2 is, for example, 5 μm to 300 μm, preferably 20 μm to 200 μm.
[0030] The substrate 2 is, for example, a phase difference film having a function as a quarter wavelength plate. The substrate 2 as a phase difference film is obtained by stretching a long substrate in a state without phase difference. The slow axis direction of the substrate 2 varies depending on the stretching method. Among the stretching methods, uniaxial stretching, biaxial stretching, oblique stretching, etc. can be cited. The angle between the long side direction of the polarizing film 1 and the slow axis direction of the substrate 2 is preferably 0°±5° or 90°±5°.
[0031] The substrate 2 has the optical properties represented by the following formulas (1) and (2). In addition, the substrate 2 may also have the optical properties represented by the following formulas (3) and (4). In the following formulas (1) to (4), Re(λ) is the front phase difference value for light of wavelength λ nm.
[0032] 100nm <Re(550)<160nm (1)
[0033] 130nm <Re(550)<150nm (2)
[0034] Re(450) / Re(550)≤1.00 (3)
[0035] 1.00≤Re(650) / Re(550) (4)
[0036] The front phase difference value is determined by the following formula (5). In formula (5), d represents the thickness, and Δn(λ) represents the birefringence at a wavelength of λnm. In order to obtain the desired front phase difference value, d and Δn(λ) can be adjusted. By adjusting the front phase difference value, a substrate 2 as a 1 / 4 wavelength plate can be obtained.
[0037] Re(λ)=d×Δn(λ) (5)
[0038] Examples of the resin material constituting the substrate 2 include polyolefins such as polyethylene, polypropylene, and norbornene polymers; cyclic olefin resins; polyvinyl alcohol; polyethylene terephthalate; polymethacrylate; polyacrylate; cellulose esters such as triacetyl cellulose, diacetyl cellulose, and cellulose acetate propionate; polyethylene naphthalate; polycarbonate; polysulfone; polyether sulfone; polyether ketone; polyphenylene sulfide; and polyphenylene ether. The substrate 2 is preferably a cyclic olefin resin, triacetyl cellulose, diacetyl cellulose, cellulose acetate propionate, polyethylene naphthalate, polymethacrylate, polyacrylate, polyethylene, and polypropylene. The substrate 2 is more preferably a cyclic olefin resin, triacetyl cellulose, diacetyl cellulose, cellulose acetate propionate, polymethacrylate, and polyacrylate.
[0039] The substrate 2 may be subjected to a surface treatment. Examples of the surface treatment include corona or plasma treatment from vacuum atmosphere to atmospheric pressure atmosphere, laser treatment, ozone treatment, saponification treatment, flame treatment, coating treatment with a coupling agent, primer treatment, and treatment using a graft polymerization method in which a reactive monomer or a reactive polymer is attached to the surface and then irradiated with radiation, plasma or ultraviolet rays to react.
[0040] A hard coating layer 5 may be adjacent to the surface of the substrate 2 opposite to the oriented film 3. The hard coating layer 5 is a cured resin layer having a higher surface smoothness than the adjacent substrate 2 and capable of being peeled off from the substrate 2. The hard coating layer 5 may be formed of a material known in the art as long as the desired peeling force can be ensured at the substrate 2. Examples of the hard coating layer 5 include a layer formed of a resin composition containing a water-soluble polymer, a cured resin layer formed of a resin composition containing an active energy ray-curable or thermosetting resin component, and the like.
[0041] The resin composition constituting the hard coat layer 5 usually contains a resin component (polymer). As the resin component, for example, resin components (polymers) such as (meth) acrylic polymers, urethane polymers, polyester polymers, silicone polymers, polyvinyl ether polymers, and polyvinyl alcohol polymers can be cited. These resin components can be used alone or in combination of two or more.
[0042] The content of the resin component in the resin composition can be appropriately determined according to the type of the resin component used. Relative to 100 parts by mass of the solid content of the resin composition, the content of the resin component is preferably 50 parts by mass or more, more preferably 60 parts by mass or more, and further preferably 70 parts by mass or more. In addition, the content of the resin component is preferably 100 parts by mass or less, more preferably 95 parts by mass or less, and further preferably 90 parts by mass or less.
[0043] The resin composition constituting the hard coat layer 5 may also contain a crosslinking agent. As a crosslinking agent, a crosslinking agent commonly used in the art can be used. The crosslinking agent can be appropriately selected according to the resin component constituting the hard coat layer 5, the composition of the layer adjacent to the hard coat layer 5, etc. As a crosslinking agent, for example, hydroxymethyl compounds, multifunctional thiol compounds, multifunctional (meth) acrylates, etc. can be cited. They can be used alone or in combination of two or more. In addition, the hard coat layer 5 may also contain an additive for improving the strength of the substrate 2. As an additive, for example, inorganic particles, organic particles or mixtures thereof can be cited.
[0044] The orientation film 3 is a film having a control force to orient the dichroic pigment in a desired direction. The orientation film 3 orients the dichroic pigment contained in the composition (polarizing film forming composition) forming the polarizing film 4, thereby adjusting the absorption axis direction of the polarizing film 4 to the desired direction. The absorption axis direction of the polarizing film 4 is, for example, the same direction as the control force direction of the orientation film 3. The angle formed by the long side direction of the polarizing film 1 and the control force direction of the orientation film 3 is, for example, 45°±5°.
[0045] The oriented film 3 has solubility resistance for coating of the polarizing film forming composition, etc., and has heat resistance for heating treatment for removing the solvent and orienting the dichroic pigment. As the oriented film 3, for example, a photo-oriented film, an oriented film containing an oriented polymer, a groove oriented film having a concave-convex pattern or a plurality of grooves on the surface, etc. can be cited. Considering the full presentation of the orientation control force, the thickness of the oriented film 3 is, for example, 10nm to 1200nm, preferably 10 to 400nm, further preferably 10 to 200nm, and particularly preferably 10nm to 100nm. At this time, in the polarizing film 1 in which the thickness of the oriented film 3 is within this range, the interference unevenness caused by the interface reflection of the incident light can be appropriately suppressed.
[0046] As the oriented polymer, polyamides having amide bonds in the molecule, gelatins, polyimides having imide bonds in the molecule and their hydrolyzates, i.e., polyamic acid, polyvinyl alcohol, alkyl-modified polyvinyl alcohol, polyacrylamide, polyoxazole, polyethyleneimine, polystyrene, polyvinyl pyrrolidone, polyacrylic acid and polyacrylate can be cited. Among them, polyvinyl alcohol is preferred. The oriented polymer can be used alone or in combination of two or more.
[0047] The oriented film 3 containing an oriented polymer is usually obtained by coating a composition in which an oriented polymer is dissolved in a solvent (hereinafter also referred to as an "oriented polymer composition") on a substrate 2 and removing the solvent, or by coating the oriented polymer composition on a substrate 2 and removing the solvent and rubbing (rubbing method).
[0048] As the solvent, an organic solvent is preferred. As the organic solvent, alcohol solvents such as methanol, ethanol, ethylene glycol, isopropanol, propylene glycol, methyl cellosolve, butyl cellosolve, and propylene glycol monomethyl ether can be cited; ester solvents such as ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, γ-butyrolactone, propylene glycol methyl ether acetate, and ethyl lactate; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, methyl amyl ketone, and methyl isobutyl ketone, aliphatic hydrocarbon solvents such as pentane, hexane, and heptane; aromatic hydrocarbon solvents such as toluene and xylene, nitrile solvents such as acetonitrile; ether solvents such as tetrahydrofuran and dimethoxyethane; and chlorinated hydrocarbon solvents such as chloroform and chlorobenzene, etc. The solvent can be used alone or in combination of two or more. The content of the solvent is preferably 100 to 1900 parts by mass, more preferably 150 to 900 parts by mass, and further preferably 180 to 600 parts by mass relative to 100 parts by mass of the oriented polymer composition.
[0049] The concentration of the oriented polymer in the oriented polymer composition is preferably 0.1% to 20% in terms of solid content relative to the solution, and more preferably 0.1% to 10%, as long as the oriented polymer material can be completely dissolved in the solvent. The oriented polymer composition can directly use commercially available oriented film materials. As commercially available oriented film materials, for example, SunEver (registered trademark, manufactured by Nissan Chemical Industries, Ltd.), Optomer (registered trademark, manufactured by JSR Corporation), etc. can be cited.
[0050] As a method for coating the oriented polymer composition on the substrate 2, there can be mentioned known methods such as coating methods such as spin coating, extrusion, gravure coating, die coating, rod coating, coater method, printing methods such as flexographic printing, etc. As a method for removing the solvent contained in the oriented polymer composition, there can be mentioned known methods such as natural drying, ventilation drying, heating drying, and reduced pressure drying.
[0051] In order to impart an orientation control force to the oriented film 3, a rubbing treatment (rubbing method) may be performed as required. As a method for imparting an orientation control force by rubbing, for example, the following method can be cited: a film of an oriented polymer formed on the surface of the substrate 2 by coating an oriented polymer composition on the substrate 2 and annealing the oriented polymer composition is brought into contact with a rubbing roller rotating with a rubbing cloth wound around it.
[0052] The photo-alignment film is generally obtained by coating a composition containing a polymer or monomer having a photoreactive group and a solvent (hereinafter also referred to as a "photo-alignment film-forming composition") on a substrate 2 and irradiating the substrate with polarized light (preferably polarized UV). For the photo-alignment film, it is more preferable that the direction of the alignment control force can be arbitrarily controlled by selecting the polarization direction of the polarized light to be irradiated.
[0053] Photoreactive groups refer to groups that generate liquid crystal orientation ability by light irradiation. Specifically, groups that participate in the photoreactions that are the origin of the liquid crystal orientation ability, such as the orientation induction or isomerization reaction, dimerization reaction, photocrosslinking reaction or photodecomposition reaction of molecules generated by light irradiation, can be cited. Among them, from the aspect of excellent orientation, groups that participate in dimerization reaction or photocrosslinking reaction are preferred. As photoreactive groups, groups with unsaturated bonds, especially double bonds, are preferred, and groups with at least one selected from the group consisting of carbon-carbon double bonds (C=C bonds), carbon-nitrogen double bonds (C=N bonds), nitrogen-nitrogen double bonds (N=N bonds) and carbon-oxygen double bonds (C=O bonds) are particularly preferred.
[0054] As photoreactive groups having C=C bonds, vinyl, polyene, stilbene, stilbazolyl, stilbenium, chalcone and cinnamoyl groups can be cited. As photoreactive groups having C=N bonds, groups having structures such as aromatic Schiff bases and aromatic hydrazones can be cited. As photoreactive groups having N=N bonds, groups having structures such as azophenyl, azonaphthyl, aromatic heterocyclic azo, disazo, formazan and oxyazobenzene can be cited. As photoreactive groups having C=O bonds, benzophenone, coumarin, anthraquinone and maleimide groups can be cited. These groups may have substituents such as alkyl, alkoxy, aryl, allyloxy, cyano, alkoxycarbonyl, hydroxyl, sulfonic acid, and halogenated alkyl.
[0055] Among them, photoreactive groups that participate in the photodimerization reaction are preferred, and cinnamoyl and chalcone groups are preferred from the perspective of easily obtaining a photoalignment film with a small amount of polarized light irradiation required for photoalignment and excellent thermal stability and temporal stability. As a polymer having a photoreactive group, a polymer having a cinnamoyl group that forms a cinnamic acid structure at the terminal of the polymer side chain is particularly preferred.
[0056] By coating the photo-alignment film-forming composition on the substrate 2, a photo-alignment inducing layer can be formed on the substrate 2. Examples of the solvent contained in the composition include the same solvents as those described in the "alignment polymer composition", and the solvent can be appropriately selected according to the solubility of the polymer or monomer having a photoreactive group.
[0057] The content of the polymer or monomer having a photoreactive group in the composition for forming a photo-alignment film can be appropriately adjusted according to the type of the polymer or monomer and the thickness of the target photo-alignment film, and is preferably at least 0.2% by mass, and more preferably in the range of 0.3 to 10% by mass, relative to the mass of the composition for forming a photo-alignment film. The composition for forming a photo-alignment film can contain a polymer material such as polyvinyl alcohol and polyimide, and a photosensitizer within a range that does not significantly impair the properties of the photo-alignment film.
[0058] The method for coating the photo-alignment film-forming composition on the substrate 2 may be the same method as the method for coating the alignment composition on the substrate 2. The method for removing the solvent from the coated photo-alignment film-forming composition may be, for example, natural drying, ventilation drying, heating drying, and reduced pressure drying.
[0059] The polarized light irradiation method may be a method of directly irradiating the polarized UV to the substance after removing the solvent from the photo-alignment film-forming composition coated on the substrate 2, or a method of irradiating the polarized light from the substrate 2 side and transmitting the polarized light. The polarized light is particularly preferably substantially parallel light. The wavelength of the polarized light irradiated is preferably a wavelength region in which the photoreactive group of the polymer or monomer having a photoreactive group can absorb light energy. Specifically, UV (ultraviolet light) in the range of 250 to 400 nm is particularly preferred.
[0060] As the light source for polarized irradiation, for example, xenon lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, ultraviolet lasers such as KrF and ArF can be cited, and high-pressure mercury lamps, ultra-high-pressure mercury lamps and metal halide lamps are more preferred. Among them, since the luminous intensity of ultraviolet rays with a wavelength of 313nm is large, high-pressure mercury lamps, ultra-high-pressure mercury lamps and metal halide lamps are preferred. Polarized UV can be irradiated by passing the light from the above-mentioned light source through an appropriate polarizer. As the polarizer, for example, a polarizing filter, a Glan-Thomson, Glan-Taylor polarizing prism, a wire grid polarizer can be used. It should be noted that when rubbing or polarized irradiation is performed, if masking is performed, multiple regions (patterns) with different directions of liquid crystal orientation can also be formed.
[0061] The groove oriented film is a film having a concave-convex pattern or multiple grooves (grooves, trenches) on the film surface. When a polymerizable liquid crystal compound is coated on a film having multiple linear grooves arranged at equal intervals, the liquid crystal molecules are oriented in the direction along the grooves.
[0062] As methods for obtaining a groove-oriented film, there are exemplified a method of exposing the surface of a photosensitive polyimide film through an exposure mask having a slit in a pattern shape, and then developing and rinsing to form a concave-convex pattern; a method of forming a layer of a pre-cured UV-curable resin on a plate-like original disk having grooves on its surface, and then transferring the formed resin layer to a substrate 2 and curing it; and a method of pressing a roll-shaped original disk having a plurality of grooves against a film of a pre-cured UV-curable resin formed on a substrate 2 to form convex-concave and concave surfaces, and then curing the film.
[0063] The polarizing film 4 contains a dichroic pigment compound. The dichroic pigment compound is a pigment compound having a property that the absorbance in the long axis direction of the molecule is different from the absorbance in the short axis direction of the molecule. The polarizing film 4 composed of the dichroic pigment compound has an absorption axis direction in a specified direction and a transmission axis direction orthogonal to the absorption axis direction. In addition, the polarizing film 4 composed of the dichroic pigment compound has a maximum absorption wavelength within a specified wavelength range.
[0064] In the present embodiment, as described above, the angle formed by the long side direction of the polarizing film 1 and the control force direction of the orientation film 3 is 45°±5°, and the absorption axis direction of the polarizing film 4 is parallel to the control force direction of the orientation film 3. Therefore, the angle formed by the long side direction of the polarizing film 1 and the absorption axis direction of the polarizing film 4 is 45°±5°. It should be noted that the angle here refers to the smaller angle of the angle formed by the two axes, that is, the angle below 90°. The polarizing film 4 has a maximum absorption wavelength in the range of, for example, 380nm to 780nm.
[0065] As dichroic pigments, acridine pigments, oxazine pigments, cyanine pigments, naphthalene pigments, azo pigments and anthraquinone pigments can be mentioned, among which azo pigments are preferred. As azo pigments, monoazo pigments, disazo pigments, triazo pigments, tetrazo pigments and stilbene azo pigments can be mentioned, among which disazo pigments and triazo pigments are preferred.
[0066] Examples of the azo dye include compounds represented by the following formula (I) (hereinafter referred to as "compound (I)" as the case may be).
[0067] K 1 (-N=NK 2 ) p -N=NK 3 (I)
[0068] [In formula (I), K 1 and K 3 Each of them independently represents a phenyl group which may have a substituent, a naphthyl group which may have a substituent, or a monovalent heterocyclic group which may have a substituent. 2represents a p-phenylene group which may have a substituent, a naphthalene-1,4-diyl group which may have a substituent, or a divalent heterocyclic group which may have a substituent. p represents an integer of 1 to 4. When p is an integer of 2 or more, a plurality of K 2 They may be the same or different from each other. In the range showing absorption in the visible region, the -N=N- bond may be replaced by -C=C-, -COO-, -NHCO-, or -N=CH- bonds.]
[0069] Examples of the monovalent heterocyclic group include groups obtained by removing one hydrogen atom from heterocyclic compounds such as quinoline, thiazole, benzothiazole, thienothiazole, imidazole, benzimidazole, oxazole, and benzoxazole. Examples of the divalent heterocyclic group include groups obtained by removing two hydrogen atoms from the above heterocyclic compounds.
[0070] As K 1 and K 3 The phenyl, naphthyl and monovalent heterocyclic groups in K 2 The substituents optionally possessed by the p-phenylene, naphthalene-1,4-diyl and divalent heterocyclic group include alkyl groups having 1 to 4 carbon atoms; alkoxy groups having 1 to 4 carbon atoms such as methoxy, ethoxy and butoxy; fluoroalkyl groups having 1 to 4 carbon atoms such as trifluoromethyl; cyano; nitro; halogen atoms; amino, diethylamino, pyrrolidinyl and other substituted or unsubstituted amino groups (the substituted amino group refers to an amino group having 1 or 2 alkyl groups having 1 to 6 carbon atoms, or an amino group in which two substituted alkyl groups are bonded to each other to form an alkanediyl group having 2 to 8 carbon atoms. The unsubstituted amino group is -NH2.).
[0071] Among the compounds (I), the compounds represented by any one of formula (I-1) to formula (I-8) are preferred, the compounds represented by any one of formula (I-1) to formula (I-3) are more preferred, and the compounds represented by any one of formula (I-1) and formula (I-3) are further preferred.
[0072] [Chemical formula 1]
[0073]
[0074] [In formulas (I-1) to (I-8), B 1 ~B 30 Each of n1 to n4 independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, a nitro group, a substituted or unsubstituted amino group (the definitions of substituted amino group and unsubstituted amino group are as described above), a chlorine atom or a trifluoromethyl group. n1 to n4 independently represent an integer of 0 to 3. When n1 is 2 or more, multiple B 2 They may be the same or different from each other. When n2 is 2 or more, multiple B 6 They may be the same or different from each other. When n3 is 2 or more, multiple B9 They may be the same or different from each other. When n4 is 2 or more, multiple B 14 They may be the same or different from each other.]
[0075] As the anthraquinone dye, a compound represented by formula (I-9) is preferred.
[0076] [Chemical formula 2]
[0077]
[0078] [In formula (I-9), R 1 ~R 8 Independently represent hydrogen atoms, -R x 、-NH2,-NHR x 、-NR x 2. -SR x or a halogen atom. x represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms.]
[0079] As the oxazole dye, a compound represented by formula (I-10) is preferred.
[0080] [Chemical formula 3]
[0081]
[0082] [In formula (I-10), R 9 ~R 15 Independently represent hydrogen atoms, -R x 、-NH2、-NHR x 、-NR x 2. -SR x or a halogen atom. x represents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms.]
[0083] As the acridine dye, a compound represented by formula (I-11) is preferred.
[0084] [Chemical formula 4]
[0085]
[0086] [In formula (I-11), R 16 ~R 23 Independently represent hydrogen atoms, -R x 、-NH2、-NHR x 、-NR x 2. -SR x or a halogen atom. xrepresents an alkyl group having 1 to 4 carbon atoms or an aryl group having 6 to 12 carbon atoms.]
[0087] In the above formula (I-9), formula (I-10) and formula (I-11), R x Examples of the alkyl group having 1 to 6 carbon atoms include methyl, ethyl, propyl, butyl, pentyl and hexyl, and examples of the aryl group having 6 to 12 carbon atoms include phenyl, tolyl, xylyl and naphthyl.
[0088] As the cyanine dye, compounds represented by formula (I-12) and compounds represented by formula (I-13) are preferred.
[0089] [Chemical formula 5]
[0090]
[0091] [In formula (I-12), D 1 and D 2 Each independently represents a group represented by any one of formula (I-12a) to formula (I-12d).
[0092] [Chemical formula 6]
[0093]
[0094] n5 represents an integer from 1 to 3.]
[0095] [Chemical formula 7]
[0096]
[0097] [In formula (I-13), D 3 and D 4 Each independently represents a group represented by any one of formula (I-13a) to formula (I-13h).
[0098] [Chemical formula 8]
[0099]
[0100] n6 represents an integer from 1 to 3.]
[0101] Among these dichroic dyes, azo dyes are preferred from the viewpoint of orientation.
[0102] The polarizing film 4 can be formed by coating a polarizing film-forming composition containing a dichroic pigment compound on the alignment film 3 and drying it. The coating method can use the same method as the coating method of the above-mentioned photo-alignment film-forming composition. From the viewpoint of making the orientation of the dichroic pigment good, the content of the dichroic pigment compound in the polarizing film-forming composition is preferably 0.1 to 30 parts by mass relative to 100 parts by mass of the solid content of the polarizing film-forming composition, more preferably 0.1 to 20 parts by mass, further preferably 0.1 to 10 parts by mass, and particularly preferably 0.1 to 5 parts by mass. The solid content here refers to the total amount of the components after removing the solvent from the polarizing film-forming composition.
[0103] The composition for forming a polarizing film may contain a polymerizable liquid crystal compound, a solvent, a polymerization initiator, a sensitizer, an inhibitor, a leveling agent, and a polymerizable non-liquid crystal compound. In the polarizing film 4 containing a polymerizable liquid crystal compound, while improving the strength, a reduction in color unevenness is also achieved. When the composition for forming a polarizing film contains a polymerizable liquid crystal compound, the dry film obtained by drying the composition for forming a polarizing film can be solidified. Solidification refers to the polymerization of the polymerizable liquid crystal compound contained in the dry film. As a polymerization method, heating, light irradiation, etc. can be cited. By solidification, the orientation state of the dichroic pigment contained in the dry film can be fixed.
[0104] A polymerizable liquid crystal compound refers to a compound having a polymerizable group and showing liquid crystal properties. A polymerizable group refers to a group participating in a polymerization reaction, preferably a photopolymerizable group. A photopolymerizable group refers to a group that can undergo a polymerization reaction through an active free radical, an acid, etc. generated by a photopolymerization initiator. As a polymerizable group, vinyl, vinyloxy, 1-chlorovinyl, isopropenyl, 4-vinylphenyl, acryloyloxy, methacryloyloxy, oxirane, oxetane, etc. can be cited. As a compound showing liquid crystal properties, thermotropic liquid crystals, lyotropic liquid crystals, etc. can be cited. From the perspective of being able to control the thickness of a dense film, thermotropic liquid crystals are preferred. The compound showing liquid crystal properties can be a nematic liquid crystal or a smectic liquid crystal in a thermotropic liquid crystal. In addition, a polymerizable liquid crystal compound can be a monomer, an oligomer formed by polymerization of a polymerizable group, or a polymer.
[0105] From the viewpoint of obtaining higher polarization characteristics, the polymerizable liquid crystal compound is preferably a liquid crystal compound forming a smectic phase. As the smectic phase, smectic B phase, smectic D phase, smectic E phase, smectic F phase, smectic G phase, smectic H phase, smectic I phase, smectic J phase, smectic K phase, smectic L phase can be cited, preferably smectic B phase, smectic F phase or smectic I phase, more preferably smectic B phase. These smectic phases can be the above-mentioned advanced smectic phases.
[0106] When the liquid crystal phase formed by the polymerizable liquid crystal compound is the above-mentioned higher-order smectic phase, a polarizing film 4 with a higher orientation order can be obtained. In the polarizing film 4 with a high orientation order, in the X-ray diffraction measurement, a Bragg peak from a higher-order structure such as a hexagonal phase and a crystal phase can be obtained. The Bragg peak is a peak from a periodic structure of molecular orientation. When the liquid crystal phase formed by the polymerizable liquid crystal compound is these higher-order smectic phases, a periodic interval of molecular orientation can be obtained, for example Polarizing film 4.
[0107] Examples of the polymerizable liquid crystal compound include a compound represented by the following formula (B1) and a polymer of the compound (hereinafter, the compound and the polymer are collectively referred to as a "polymerizable liquid crystal compound (B1)").
[0108] U 1 -V 1 -W 1 -X 1 -Y 1 -X 2 -Y 2 -X 3 -W 2 -V 2 -U 2 (B1)
[0109] [In formula (B1), X 1 , X 2 and X 3 Each of X represents a divalent aromatic group or a divalent alicyclic hydrocarbon group independently of the other. The hydrogen atoms contained in the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted with a halogen atom, an alkyl group having 1 to 4 carbon atoms, a fluoroalkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group or a nitro group, and the carbon atoms constituting the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted with an oxygen atom, a sulfur atom or a nitrogen atom. 1 , X 2 and X 3 At least one of them is 1,4-phenylene which may have a substituent or cyclohexane-1,4-diyl which may have a substituent. 1 and Y 2 are independently a single bond or a divalent linking group. 1 represents a hydrogen atom or a polymerizable group. 2 W represents a polymerizable group. 1 and W 2 are independently a single bond or a divalent linking group. 1 and V 2Each independently represents an alkanediyl group having 1 to 20 carbon atoms which may have a substituent, wherein -CH2- constituting the alkanediyl group may be replaced by -O-, -CO-, -S- or NH-.]
[0110] In the polymerizable liquid crystal compound (B1), X 1 , X 2 and X 3 At least one of X is 1,4-phenylene which may have a substituent or cyclohexane-1,4-diyl which may have a substituent. In particular, X 1 and X 3 Preferably, the cyclohexane-1,4-diyl group may have a substituent, and the cyclohexane-1,4-diyl group is more preferably a trans-cyclohexane-1,4-diyl group. Examples of the substituents that the 1,4-phenylene group or the cyclohexane-1,4-diyl group may have include alkyl groups having 1 to 4 carbon atoms such as methyl, ethyl, and butyl, cyano groups, and halogen atoms such as chlorine atoms and fluorine atoms. Unsubstituted is preferred. In addition, Y 1 and Y 2 When they are of the same structure, X is preferred 1 , X 2 and X 3 At least one of them is a different structure. 1 , X 2 and X 3 When at least one of them has a different structure, there is a tendency that smectic liquid crystal properties are easily exhibited.
[0111] Y 1 and Y 2 Preferred are -CH2CH2-, -CH2O-, -CH2CH2O-, -COO-, -OCOO-, a single bond, -N=N-, -CR a =CR b -、-C≡C-、-CR a =N- or CO-NR a -. R a and R b Y independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 1 More preferably, it is -CH2CH2-, -COO- or a single bond, and Y 2 More preferably, it is -CH2CH2- or CH2O-. 1 , X 2 and X 3 When all are of the same structure, Y is preferably 1 and Y 2 For different structures. 1 and Y 2In the case of mutually different structures, there is a tendency that smectic liquid crystal properties are easily exhibited.
[0112] U 2 U is a polymerizable group. 1 is a hydrogen atom or a polymerizable group, preferably a polymerizable group. 1 and U 2 All of them are polymerizable groups, and preferably all of them are photopolymerizable groups. The photopolymerizable group refers to a group that can participate in a polymerization reaction by an active radical, an acid, or the like generated by a photopolymerization initiator described later.
[0113] U 1 The photopolymerizable groups and U 2 The polymerizable groups shown may be different from each other, but are preferably groups of the same type. Examples of the polymerizable groups include vinyl, vinyloxy, 1-chlorovinyl, isopropenyl, 4-vinylphenyl, acryloyloxy, methacryloyloxy, oxirane, and oxetane. Among them, free radical polymerizable groups are preferred, acryloyloxy, methacryloyloxy, vinyl, and vinyloxy are more preferred, acryloyloxy and methacryloyloxy are further preferred, and acryloyloxy is still further preferred.
[0114] As V 1 and V 2 Examples of the alkanediyl group represented by V include methylene, ethylene, propane-1,3-diyl, butane-1,3-diyl, butane-1,4-diyl, pentane-1,5-diyl, hexane-1,6-diyl, heptane-1,7-diyl, octane-1,8-diyl, decane-1,10-diyl, tetradecane-1,14-diyl and eicosane-1,20-diyl. 1 and V 2 An alkanediyl group having 2 to 12 carbon atoms is preferred, and an alkanediyl group having 6 to 12 carbon atoms is more preferred. Examples of the substituent group that the alkanediyl group may have include a cyano group and a halogen atom, but the alkanediyl group is preferably unsubstituted, and is more preferably an unsubstituted and linear alkanediyl group. 1 and W 2 , independently of each other, are preferably a single bond, -O-, -S-, -COO- or OCOO-, more preferably a single bond or -O-.
[0115] Examples of the polymerizable liquid crystal compound (B1) include compounds represented by the following formulae (B-1) to (B-25). When the polymerizable liquid crystal compound (B1) has a cyclohexane-1,4-diyl group, the cyclohexane-1,4-diyl group is preferably a trans isomer.
[0116] [Chemical formula 9]
[0117]
[0118] [Chemical formula 10]
[0119]
[0120] [Chemical formula 11]
[0121]
[0122] [Chemical formula 12]
[0123]
[0124] [Chemical formula 13]
[0125]
[0126] Among the above, it is preferred to select at least one from the group consisting of compounds represented by formula (B-2), formula (B-3), formula (B-4), formula (B-5), formula (B-6), formula (B-7), formula (B-8), formula (B-13), formula (B-14), formula (B-15), formula (B-16) and formula (B-17).
[0127] The exemplified polymerizable liquid crystal compounds can be used alone or in combination. When two or more polymerizable liquid crystal compounds are combined, preferably at least one is a polymerizable liquid crystal compound, and more preferably two or more are polymerizable liquid crystal compounds. By combining, liquid crystallinity can sometimes be temporarily maintained even at a temperature below the liquid crystal-crystallization phase transition temperature. The mixing ratio when combining two polymerizable liquid crystal compounds is generally 1:99 to 50:50, preferably 5:95 to 50:50, and more preferably 10:90 to 50:50.
[0128] The polymerizable liquid crystal compound can be produced by a known method described in Lub et al. Recl. Trav. Chim. Pays-Bas, 115, 321-328 (1996), Japanese Patent No. 4719156, and the like.
[0129] The content of the polymerizable liquid crystal compound in the solid content of the light absorbing anisotropic film-forming composition is preferably 50% by mass or more, more preferably 70% by mass or more, preferably 99% by mass or less, more preferably 95% by mass or less, and further preferably 90% by mass or less. In this specification, the solid content in the light absorbing anisotropic film-forming composition refers to the total amount of components after excluding volatile components such as solvents from the light absorbing anisotropic film-forming composition.
[0130] Examples of the solvent include the same solvents as those described in the "oriented polymer composition", and the content of the solvent is preferably 100 to 1900 parts by mass, more preferably 150 to 900 parts by mass, and further preferably 180 to 600 parts by mass, based on 100 parts by mass of the light absorbing anisotropic film-forming composition.
[0131] As the polymerization initiator, a photopolymerization initiator is preferred. As the photopolymerization initiator, a photopolymerization initiator having light absorption at a wavelength of 300 nm to 380 nm is generally used. A photopolymerization initiator is a compound that can initiate a polymerization reaction of a polymerizable liquid crystal compound, and can initiate a polymerization reaction at a lower temperature. Specifically, a photopolymerization initiator that can generate active free radicals or acids by the action of absorbed light can be cited, among which a photopolymerization initiator that generates free radicals by the action of light is preferred.
[0132] Examples of the photopolymerization initiator include benzoin compounds, benzophenone compounds, alkylphenone compounds, acylphosphine oxide compounds, triazine compounds, iodonium salts, and sulfonium salts. These polymerization initiators may be used alone or in combination of two or more.
[0133] Examples of the benzoin compound include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether and benzoin isobutyl ether.
[0134] Examples of the benzophenone compound include benzophenone, methyl o-benzoylbenzoate, 4-phenylbenzophenone, 4-benzoyl-4′-methyldiphenyl sulfide, 3,3′,4,4′-tetrakis(tert-butylperoxycarbonyl)benzophenone, and 2,4,6-trimethylbenzophenone.
[0135] Examples of the alkylphenone compound include diethoxyacetophenone, 2-methyl-2-morpholino-1-(4-methylthiophenyl)propane-1-one, 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butane-1-one, 2-hydroxy-2-methyl-1-phenylpropane-1-one, 1,2-diphenyl-2,2-dimethoxyethane-1-one, 2-hydroxy-2-methyl-1-〔4-(2-hydroxyethoxy)phenyl〕propane-1-one, 1-hydroxycyclohexylphenyl ketone and oligomers of 2-hydroxy-2-methyl-1-〔4-(1-methylvinyl)phenyl〕propane-1-one.
[0136] Examples of the acylphosphine oxide compound include 2,4,6-trimethylbenzoyldiphenylphosphine oxide and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide.
[0137] Examples of the triazine compound include 2,4-bis(trichloromethyl)-6-(4-methoxyphenyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxynaphthyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxyphenyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxyphenyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(5-methylfuran-2-yl)] [vinyl]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(furan-2-yl)vinyl]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(4-diethylamino-2-methylphenyl)vinyl]-1,3,5-triazine and 2,4-bis(trichloromethyl)-6-[2-(3,4-dimethoxyphenyl)vinyl]-1,3,5-triazine.
[0138] A commercially available photopolymerization initiator can be used. Examples of commercially available polymerization initiators include "Irgacure (registered trademark) 907", "Irgacure (registered trademark) 184", "Irgacure (registered trademark) 651", "Irgacure (registered trademark) 819", "Irgacure (registered trademark) 250", and "Irgacure (registered trademark) 369" (Ciba Japan Co., Ltd.); "SEIKUOL (registered trademark) BZ", "SEIKUOL (registered trademark) Z", and "SEIKUOL (registered trademark) BEE" (Seiko Chemical Co., Ltd.); "Kayacure (registered trademark) BP100" (Nippon Kayaku Co., Ltd.); "Kayacure (registered trademark) UVI-6992" (manufactured by Dow); "Adeka optomer SP-152", "Adeka optomer SP-170" (ADEKA Co., Ltd.); "TAZ-A", "TAZ-PP" (Siberhegner Co., Ltd.); and "TAZ-104" (Sanwa Chemical Co., Ltd.).
[0139] The content of the polymerization initiator can be appropriately adjusted according to the type and amount of the polymerizable liquid crystal compound contained in the light absorption anisotropic film-forming composition, relative to 100 parts by mass of the polymerizable liquid crystal compound, preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and more preferably 10 parts by mass or less. When the content of the polymerization initiator is above the above lower limit, polymerization can be performed without disturbing the orientation of the polymerizable liquid crystal compound. In addition, when the content of the polymerization initiator is below the above upper limit, long-term storage stability can be improved, and it is easier to suppress or prevent the generation of orientation defects of the resulting polarizing film.
[0140] As the sensitizer, a photosensitizer is preferred. Examples of the photosensitizer include xanthone compounds such as xanthone and thioxanthone (2,4-diethylthioxanthone, 2-isopropylthioxanthone, etc.); anthracene compounds such as anthracene and anthracene containing an alkoxy group (dibutoxyanthracene, etc.); phenothiazine and rubrene. The sensitizer may be used alone or in combination of two or more.
[0141] When the composition for forming anisotropic light-absorbing films contains a sensitizer, the polymerization reaction of the polymerizable liquid crystal compound contained in the composition can be further promoted. The amount of the sensitizer used can be appropriately adjusted according to the type and amount of the polymerization initiator and the polymerizable liquid crystal compound, and is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 10 parts by mass, and even more preferably 0.5 to 8 parts by mass relative to 100 parts by mass of the polymerizable liquid crystal compound.
[0142] In order to make the polymerization reaction of the light absorption anisotropic film-forming composition proceed more stably, the composition may contain an appropriate amount of a polymerization inhibitor, thereby making it easy to control the degree of progress of the polymerization reaction of the polymerizable liquid crystal compound.
[0143] Examples of the polymerization inhibitor include hydroquinone, alkoxy-containing hydroquinone, alkoxy-containing catechol (eg, butyl catechol), pyrogallol, and radical scavengers such as 2,2,6,6-tetramethyl-1-piperidinyloxy radical; thiophenol; β-naphthylamine and β-naphthol.
[0144] When the light absorption anisotropic film-forming composition contains a polymerization inhibitor, its content can be appropriately adjusted according to the type and amount of the polymerizable liquid crystal compound, the amount of the sensitizer used, etc., and is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 10 parts by mass, and further preferably 0.5 to 8 parts by mass relative to 100 parts by mass of the polymerizable liquid crystal compound. If the content of the polymerization inhibitor is within this range, polymerization can be performed without disturbing the orientation of the polymerizable liquid crystal compound.
[0145] The composition for forming anisotropic light-absorbing film may contain one or more leveling agents. The leveling agent has the function of adjusting the fluidity of the composition for forming anisotropic light-absorbing film and making the coating film obtained by coating the composition flatter. Specifically, a surfactant may be mentioned. As the leveling agent, at least one selected from the group consisting of a leveling agent containing a polyacrylate compound as a main component and a leveling agent containing a fluorine atom-containing compound as a main component is preferred.
[0146] Examples of leveling agents containing a polyacrylate compound as a main component include "BYK-350", "BYK-352", "BYK-353", "BYK-354", "BYK-355", "BYK-358N", "BYK-361N", "BYK-380", "BYK-381" and "BYK-392" [BYK Chemie].
[0147] Examples of leveling agents containing a fluorine atom-containing compound as a main component include "Megafac (registered trademark) R-08", Megafac "R-30", Megafac "R-90", Megafac "F-410", Megafac "F-411", Megafac "F-443", Megafac "F-445", Megafac "F-470", Megafac "F-471", Megafac "F-477", Megafac "F-479", Megafac "F-482" and Megafac "F-483" [DIC Corporation]; "Surflon (registered trademark) S-381", Surflon "S-382", Surflon "S-383", Surflon "S-393", Surflon "SC-101", Surflon "SC-105", "KH-40" and "SA-100" [AGC Seimi Chemical Co., Ltd.]; "E1830", "E979" [Daikin Fine Chemical Laboratories Co., Ltd.]; "F-top EF301", "F-top EF303", "F-top EF351" and "F-top EF352" [Mitsubishi Materials Electronic Chemicals Co., Ltd.].
[0148] When the light absorption anisotropic film-forming composition contains a leveling agent, the content thereof is preferably 0.05 to 5 parts by mass, more preferably 0.05 to 3 parts by mass, relative to 100 parts by mass of the polymerizable liquid crystal compound. When the content of the leveling agent is within the above range, the resulting polarizing film tends to be smoother and less prone to unevenness.
[0149] <Polarizing film>
[0150] The present invention includes a polarizing film which is a cured product of the above-mentioned polarizing film forming composition. The polarizing film of the present invention is a film (film) having a polarizing function, and contains a dichroic pigment in an oriented polymerizable liquid crystal. Since the polarizing film of the present invention is formed by the above-mentioned polarizing film forming composition, it has almost or completely no orientation defects and has excellent polarizing performance.
[0151] The polarizing film of the present invention can be produced, for example, by a method comprising the steps of forming a coating film of the polarizing film-forming composition, drying and removing the organic solvent from the coating film (ii), and orienting and curing the polymerizable liquid crystal compound in a smectic liquid crystal phase (iii).
[0152] Step (ii) is a step of coating the polarizing film-forming composition on a substrate, an oriented film or other layer (e.g., a functional layer) described later to form a coating film, and drying and removing the organic solvent under the condition that the polymerizable liquid crystal compound contained in the obtained coating film does not polymerize to obtain a dried film. The polarizing film can be directly coated on a substrate or other layer (e.g., a functional layer), but is preferably coated on an oriented film having an orientation control force.
[0153] In step (ii), as a drying method, for example, natural drying, ventilation drying, heating drying and reduced pressure drying can be cited. When the polymerizable liquid crystal compound is a polymerizable smectic liquid crystal compound, it is preferred to make the liquid crystal state of the polymerizable smectic liquid crystal compound contained in the dry film become a nematic phase (nematic liquid crystal state) and then transform it to a smectic phase. In order to form a smectic phase via a nematic phase, for example, the following method is used: the dry film is heated to a temperature above the temperature at which the polymerizable smectic liquid crystal compound contained in the dry film transforms into a liquid crystal state of a nematic phase, and then cooled to a temperature at which the polymerizable smectic liquid crystal compound exhibits a liquid crystal state of a smectic phase.
[0154] Step (iii) is a step of orienting and solidifying the polymerizable liquid crystal compound in the dry film in the state of smectic liquid crystal phase. The following is a method of photopolymerizing the polymerizable liquid crystal compound while maintaining the liquid crystal state of the smectic phase after the liquid crystal state of the polymerizable liquid crystal compound in the dry film is changed to a smectic phase in step (ii). In the photopolymerization, the light irradiated to the dry film can be appropriately selected according to the type of photopolymerization initiator contained in the dry film, the type of polymerizable liquid crystal compound (especially the type of photopolymerization group possessed by the polymerizable liquid crystal compound) and the amount thereof.
[0155] As a specific example, one or more light selected from the group consisting of visible light, ultraviolet light, infrared light, X-rays, α-rays, β-rays and γ-rays, and active electron beams can be cited. Among them, from the aspect of easily controlling the progress of the polymerization reaction and the aspect of being able to use the photopolymerization device widely used in the art, ultraviolet light is preferred, and the types of polymerizable liquid crystal compounds and photopolymerization initiators contained in the polymerizable liquid crystal composition are preferably pre-selected so that photopolymerization can be performed by ultraviolet light. In addition, during polymerization, the polymerization temperature can also be controlled by irradiating light while cooling and drying the film with a suitable cooling device. By adopting such a cooling means, if the polymerization of the polymerizable liquid crystal compound is implemented at a lower temperature, a polarizing film can be appropriately formed even if the substrate uses a material with lower heat resistance. During photopolymerization, a patterned polarizing film can also be obtained by masking, developing, etc.
[0156] As the light source of the above-mentioned active energy rays, for example, there can be mentioned a low-pressure mercury lamp, a medium-pressure mercury lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a xenon lamp, a halogen lamp, a carbon arc lamp, a tungsten lamp, a gallium lamp, an excimer laser, an LED light source emitting light in the wavelength range of 380 to 440 nm, a chemical lamp, a black light lamp, a microwave-excited mercury lamp, a metal halide lamp, and the like.
[0157] UV radiation intensity is usually 10 to 3,000 mW / cm 2 The ultraviolet irradiation intensity is preferably an intensity in the wavelength region effective for activating the photopolymerization initiator. The irradiation time is usually 0.1 seconds to 10 minutes, preferably 1 second to 5 minutes, more preferably 5 seconds to 3 minutes, and further preferably 10 seconds to 1 minute. When irradiating once or more times with such ultraviolet irradiation intensity, the cumulative light amount is 10 to 3,000 mJ / cm 2 , preferably 50 to 2,000 mJ / cm 2 , more preferably 100 to 1,000 mJ / cm 2 .
[0158] By photopolymerization, the polymerizable liquid crystal compound is polymerized in a liquid crystal state maintaining a smectic phase, preferably a higher smectic phase, to form a polarizing film. For the polarizing film obtained by polymerizing the polymerizable liquid crystal compound in a liquid crystal state maintaining a smectic phase, accompanied by the effect of the above-mentioned dichroic pigment, it has the advantage of high polarization performance compared with the conventional host-guest polarizing film, that is, the polarizing film formed by the liquid crystal state of the nematic phase. Furthermore, compared with the case where only the dichroic pigment or the lyotropic liquid crystal is applied, it has the advantage of excellent strength.
[0159] The thickness of the polarizing film can be appropriately selected according to the display device to which it is applied, and is preferably 0.1 to 5 μm, more preferably 0.3 to 4 μm, and further preferably 0.5 to 3 μm.
[0160] In the polarizing film 1 described above, the refractive index difference between the polarizing film 4 and the oriented film 3 with respect to visible light satisfies the following formula (6), and the refractive index difference between the oriented film 3 and the substrate 2 with respect to visible light satisfies the following formula (7). In formula (6), n(polarizing film) represents the refractive index of the polarizing film in the transmission axis direction.
[0161] |n(polarizing film)-n(oriented film)|≤0.06 (6)
[0162] |n(oriented film)-n(substrate)|≤0.06 (7)
[0163] The refractive index difference between the polarizing film 4 and the alignment film 3 with respect to visible light is preferably 0.04 or less, more preferably 0.02 or less. The refractive index difference between the alignment film 3 and the substrate 2 with respect to visible light is preferably 0.04 or less, more preferably 0.02 or less.
[0164] In such a polarizing film 1, by suppressing the refractive index difference between the orientation film 3 and the substrate 2 and the refractive index difference between the orientation film 3 and the substrate 2 within the above range, it is possible to suppress the interface reflection of the incident light between the polarizing film 4 and the orientation film 3 and between the orientation film 3 and the substrate 2. Therefore, it is possible to suppress the interference unevenness caused by the interface reflection of the incident light.
[0165] In the present embodiment, the thickness of the alignment film 3 is 10 nm to 400 nm. In this case, in the polarizing film 1 in which the thickness of the alignment film 3 is within this range, interference unevenness due to interface reflection of incident light can be preferably suppressed.
[0166] In the present embodiment, a hard coating layer 5 is adjacent to the surface of the substrate 2 opposite to the oriented film 3. When the polarizing film 1 is produced, it is considered that the substrate 2 is warped due to the shrinkage when the polarizing film 4 is cured, and wrinkles are generated on the obtained polarizing film 1. In contrast, by providing the substrate 2 with the hard coating layer 5, the warping of the substrate 2 with respect to the shrinkage when the polarizing film 1 is cured can be suppressed, and the generation of wrinkles on the obtained polarizing film 1 can be suppressed.
[0167] In this embodiment, the substrate 2, the orientation film 3, and the polarizing film 4 are long. That is, in this embodiment, the polarizing film 1 is a long polarizing film 1 capable of suppressing interference unevenness caused by interface reflection of incident light. By continuously joining the polarizing film 1 cut out from the long polarizing film 1 to various display devices, a display device using the polarizing film 1 in which interference unevenness caused by interface reflection of incident light is suppressed can be efficiently manufactured.
[0168] In this embodiment, the angle between the long side and the slow axis of the substrate 2 is 0°±5° or 90°±5°, and the angle between the slow axis of the substrate 2 and the absorption axis of the polarizing film 4 is 45°±5°. Thus, a polarizing film 1 having high ellipticity is obtained.
[0169] Example
[0170] The present invention is described in more detail below by way of examples. Unless otherwise specified, "%" and "parts" in the following examples refer to "mass %" and "mass parts". The composition and evaluation results of the polarizing films in the examples and comparative examples are summarized in Figure 2 and Figure 3 middle.
[0171] [Preparation of Photo-Alignment Film-Forming Composition]
[0172] The following components were mixed, and the obtained mixture was stirred at 80° C. for 1 hour to obtain a composition (1) for forming a photo-alignment film.
[0173] Photo-aligned polymer: 2 parts
[0174] [Chemical formula 14]
[0175]
[0176] (Polymer described in Japanese Patent Application Laid-Open No. 2013-033249, number average molecular weight: about 28,200, Mw / Mn: 1.82)
[0177] Solvent: 98 parts of o-xylene
[0178] [Preparation of Polarizing Film-Forming Composition]
[0179] The following components were mixed and stirred at 80° C. for 1 hour to obtain a polarizing film-forming composition (1). The dichroic dye used was an azo dye described in Examples of JP-A-2013-101328.
[0180] Polymerizable liquid crystal compound: A1 90 parts
[0181] [Chemical formula 15]
[0182]
[0183] Polymerizable liquid crystal compound: A2 10 parts
[0184] [Chemical formula 16]
[0185]
[0186] ·Dichroic pigment: 2.5 parts of azo pigment A
[0187] [Chemical formula 17]
[0188]
[0189] ·Dichroic pigment: 2.5 parts of azo pigment B
[0190] [Chemical formula 18]
[0191]
[0192] ·Dichroic pigment: 2.5 parts of azo pigment C
[0193] [Chemical formula 19]
[0194]
[0195] Photopolymerization initiator: 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (Irgacure 369; manufactured by Ciba Specialty Chemicals Co., Ltd.) 6 parts
[0196] Leveling agent: 1.2 parts of polyacrylate compound (BYK-361N; manufactured by BYK-Chemie)
[0197] Solvent: 400 parts of methyl ethyl ketone
[0198] [Production of base material]
[0199] A protective film of a cyclic olefin resin (ZeonorFilm ZM series (registered trademark) manufactured by ZEON Corporation of Japan) was used as the substrate of the polarizing film of Examples 1, 3 to 5, and 7. A protective film of a cyclic olefin resin (ZeonorFilm ZT series (registered trademark) manufactured by ZEON Corporation of Japan) was used as the substrate of the polarizing film of Example 2.
[0200] A protective film of a cyclic olefin resin (ZeonorFilm ZD series (registered trademark) manufactured by ZEON Co., Ltd., Japan) was used as the substrate of the polarizing film of Example 6. In the polarizing film of Comparative Example 1, a uniaxially stretched film WRF-S (modified polycarbonate resin) was used as the substrate. The thickness of the obtained substrate was 50 μm, and the in-plane phase difference value at a wavelength of 550 nm was 144.6 nm.
[0201] [Preparation of hard coat layer forming composition]
[0202] The following components were mixed and stirred at 50° C. for 4 hours to obtain a hard coat layer-forming resin composition (1).
[0203] · 50 parts of a multifunctional acrylate compound having the following structure (dipentaerythritol hexaacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd., “NK ester A-DPH”), the number of atoms in the chain connecting the branch point closest to the acryloyl group in the branch structure to the acryloyl group is 2.)
[0204] [Chemical formula 20]
[0205]
[0206] Urethane acrylate polymer: 50 parts of urethane acrylate ("Ebecryl 4858" manufactured by Daicel-Allnex Co., Ltd., having a functional group number of 2, a weight average molecular weight Mw of 450, and a functional group number per unit molecular weight of 44.4×10-4)
[0207] Radical polymerization initiator: 3 parts of 2-[4-(methylthio)benzoyl]-2-(4-morpholinyl)propane (manufactured by BASF, "Irgacure 907")
[0208] Solvent: 10 parts of methyl ethyl ketone
[0209] [Formation of hard coat layer]
[0210] The hard coat layer-forming composition (1) was applied to the substrate by a bar coating method (#2 30 mm / s). The coating film of the hard coat layer-forming composition (1) was irradiated with a UV irradiation device (SPOT CURE SP-7; manufactured by Ushio Electric Co., Ltd.) at an exposure dose of 500 mJ / cm 2 The substrate with a hard coat layer was obtained by applying ultraviolet rays (365 nm standard). The thickness of the hard coat layer was measured by a laser microscope (OLS3000 manufactured by Olympus Corporation) and found to be 1.5 μm.
[0211] [Production of polarizing film]
[0212] After the substrate surface of the substrate with a hard coating layer is subjected to corona treatment, a composition for forming a photo-alignment film (1) is applied by a rod coating method, and the composition is dried at 120°C to obtain a dry coating film. Subsequently, polarized UV is irradiated on the dry coating film to form a photo-alignment film, and a laminate having a hard coating layer / substrate / photo-alignment film in this order is obtained. The results of measurement using a laser microscope (OLS3000 manufactured by Olympus Corporation) show that in Examples 1 to 3, 6, and 7, the thickness of the photo-alignment film is 100 nm, and in Example 4, the thickness of the photo-alignment film is 200 nm. In addition, in Example 5, the thickness of the photo-alignment film is 400 nm. The polarized UV treatment is carried out by a UV irradiation device (SPOT CURE SP-7; manufactured by Ushio Electric Co., Ltd.) under the condition that the measured intensity at a wavelength of 365 nm is 100 mJ.
[0213] The polarizing film forming composition (1) was applied to the surface of the photo-alignment film in the obtained laminate by a bar coating method, and the polymerizable liquid crystal compound was heated and dried in a drying oven at 120°C for 1 minute to change the phase of the polymerizable liquid crystal compound into a liquid phase, and then cooled to room temperature to change the phase of the polymerizable liquid crystal compound into a smectic liquid crystal state. Next, a UV irradiation device (SPOT CURESP-7; manufactured by Ushio Electric Co., Ltd.) was used to irradiate the coating film formed by the polarizing film forming composition (1) at an exposure dose of 1000 mJ / cm 2 (365nm reference) ultraviolet rays. Thus, the polymerizable liquid crystal compound contained in the dry coating film is polymerized while maintaining the smectic liquid crystal of the polymerizable liquid crystal compound, to obtain a polarizing film having a hard coating layer / substrate / photo-alignment film / polarizing film in sequence. The thickness of the polarizing film was measured using a laser microscope (OLS3000 manufactured by Olympus Corporation) and the result was that the thickness of the polarizing film was 2.3 μm.
[0214] [Production of long polarizing films]
[0215] The long polarizing films of each embodiment and comparative example are continuously produced by the Roll-to-Roll method. The long substrates of each embodiment and comparative example are continuously unwound, and the surface of the substrate is subjected to plasma treatment. Then, a slit coater is used to spray the composition (1) for forming a photo-alignment film onto the central part of the substrate to form a first coating film. Furthermore, the substrate formed with the first coating film is conveyed in a ventilated drying furnace set at 100°C for 2 minutes to remove the solvent and form a first dry film. The substrate formed with the first dry film is subjected to a plasma treatment at 20 mJ / cm in the long side direction. 2 The first dried film is irradiated with polarized UV light in a predetermined direction at an intensity (based on 313 nm) to provide an alignment control force to form a long photo-alignment film.
[0216] Next, the composition for forming a polarizing film was sprayed onto the center of the substrate using a slit coater to form a second coating film. The substrate with the second coating film was then conveyed in a ventilated drying oven set at 110°C for 2 minutes to remove the solvent and form a second dry film. The substrate with the second dry film was treated with 1000 mJ / cm 2 The polymerizable liquid crystal compound contained in the second dry film is cured by irradiating with UV light (365 nm standard), thereby forming a long polarizing film.
[0217] Then, it was continuously rolled into a roll to obtain a 200m long polarizing film in each embodiment and comparative example. The angle between the long side direction of the long polarizing film and the slow axis direction of the substrate was 0° in Examples 1, 3 to 5, 7 and Comparative Example 1, 90° in Example 2, and 45° in Example 6. The angle between the long side direction of the long polarizing film and the absorption axis direction of the polarizing film was 45° in Examples 1, 3 to 5 and Comparative Example 1, 45° in Example 2, 0° in Example 6, and 46° in Example 7.
[0218] [Measurement of refractive index]
[0219] The refractive index (average refractive index at a wavelength of 589 nm) of the substrate, photo-alignment film, and hard-coat layer was measured using a refractometer ("Multi-wavelength Abbe Refractometer DR-M4" manufactured by ATAGO Co., Ltd.). The refractive index of the substrate in Examples 1 to 7 was 1.53. The refractive index of the substrate in Comparative Example 1 was 1.62. The refractive index of the photo-alignment film in Examples 1 to 7 and Comparative Example 1 was 1.55. The refractive index of the hard-coat layer in Example 3 was 1.53.
[0220] Regarding the refractive index of the transmission axis direction of the polarizing film, the samples of the polarizing films for refractive index evaluation in each embodiment and comparative example are prepared as follows. First, a composition for forming a polarizing film for refractive index evaluation is prepared with a composition excluding the pigment. The substrate uses a protective film of an unstretched cyclic olefin resin with a thickness of 23 μm and an in-plane phase difference value of 0 (ZeonorFilm (registered trademark) made by ZEON Co., Ltd. of Japan). In addition, the samples of the polarizing films for refractive index evaluation of each embodiment and comparative example are formed by the same steps as in the above-mentioned embodiment.
[0221] For the sample of polarizing film used for refractive index evaluation, the automatic birefringence meter KOBRA-WPR manufactured by Oji Instruments Co., Ltd. was used to change the incident angle of light on the sample, and the phase difference value at the time of tilting 40° relative to the fast axis center was measured. The average refractive index at each wavelength was measured using an ellipsometer M-220 manufactured by JASCO Corporation. The film thickness of the polarizing film was measured using an optical nanometer film thickness meter C12562-01 manufactured by Hamamatsu Photonics Co., Ltd. Based on the obtained front phase difference value, the phase difference value at a tilt of 40° relative to the fast axis center, the average refractive index and the film thickness value, the three-dimensional refractive index was calculated with reference to the Oji Instruments technical data (http: / / www.oji-keisoku.co.jp / products / kobra / reference.html).
[0222] The refractive index of the polarizing film in the transmission axis direction in Examples 1 to 7 and Comparative Example 1 was 1.53. As a result, |n(polarizing film)-n(oriented film)| was 0.02 in all Examples 1 to 7 and Comparative Example 1. In addition, |n(oriented film)-n(substrate)| was 0.02 in all Examples 1 to 7, while |n(oriented film)-n(substrate)| was 0.07 in Comparative Example 1.
[0223] [Appearance inspection]
[0224] The long polarizing films prepared in each example and comparative example were cut into 70 mm × 150 mm squares, and a λ / 4 wavelength plate was attached to the polarizing film side by means of a pressure-sensitive adhesive, and an aluminum plate was attached to the λ / 4 wavelength plate side by means of a pressure-sensitive adhesive, thereby obtaining the appearance inspection samples of each example and comparative example. The obtained appearance inspection samples were visually inspected for interference unevenness from a position inclined 20° relative to the vertical direction of the front surface.
[0225] In the appearance inspection, the area where the visual interference unevenness is less than 2% of the sample area is evaluated as "A", the area where the visual interference unevenness is more than 2% and less than 5% of the sample area is evaluated as "B", the area where the visual interference unevenness is more than 5% and less than 15% of the sample area is evaluated as "C", and the area where the visual interference unevenness is more than 15% of the sample area is evaluated as "D".
[0226] It is "A" in Examples 1 to 3, 6, and 7, "B" in Example 4, "C" in Example 5, and "D" in Comparative Example 1. From these results, it can be confirmed that by suppressing the refractive index difference between the alignment film and the substrate and the refractive index difference between the alignment film and the substrate to 0.06 or less, the interface reflection of the incident light between the polarizing film and the alignment film and between the alignment film and the substrate can be suppressed, and the interference unevenness caused by the interface reflection of the incident light can be suppressed in the polarizing film.
[0227] [Curl Evaluation]
[0228] The long polarizing film prepared in each example and comparative example was cut into 70 mm × 150 mm squares, and a λ / 4 wavelength plate was attached to the polarizing film side using a laminator via a pressure-sensitive adhesive to obtain curl evaluation samples of each example and comparative example. The shape of the obtained curl evaluation samples was visually observed.
[0229] In the curl evaluation, the evaluation of forming a gentle convex shape on the substrate side was "A", and the evaluation of forming a flat shape was "B" in view of the good workability of bonding to the panel. Example 3 in which a hard coating layer was adjacent to the surface opposite to the orientation surface of the substrate was "A", and Examples 1, 2, 4 to 7 and Comparative Example 1 without a hard coating layer were "B".
[0230] [Curling habit test]
[0231] The long polarizing films prepared in each embodiment and comparative example were cut into 50 mm wide and 300 mm long (in the long dimension direction), and the films were wound around an iron rod with a diameter of 6 mm along the long dimension direction, and then put into an oven at 140°C and left to stand for 3 minutes. After each film was taken out to room temperature, the iron rod was removed and the curling behavior of each film was confirmed.
[0232] The curling habit test is a test that assumes that a roll of a long polarizing film is stored for a long time in a high temperature environment. From the perspective of long-term storage stability, in the curling habit test, the case where the central axis in the width direction of the film is parallel to the long side of the film is evaluated as "A", and the case where the central axis in the width direction of the film is not parallel to the long side of the film is evaluated as "B". The results are "A" in Examples 1 to 5, 7 and Comparative Example 1, and "B" in Example 6.
[0233] The gist of the present invention is as shown in the following [1] to [5].
[0234] [1] A polarizing film, which is a polarizing film having a substrate, an orientation film and a polarizing film laminated in this order, wherein the angle formed by the slow axis direction of the substrate and the absorption axis direction of the polarizing film is 45°±5°, the refractive index difference between the polarizing film and the orientation film with respect to visible light satisfies the following formula (1), and the refractive index difference between the orientation film and the substrate with respect to visible light satisfies the following formula (2),
[0235] |n(polarizing film)-n(oriented film)|≤0.06 (1)
[0236] |n(oriented film)-n(substrate)|≤0.06 (2)
[0237] (In formula (1), n(polarizing film) represents the refractive index of the polarizing film in the transmission axis direction).
[0238] [2] The polarizing film according to [1], wherein the thickness of the alignment film is 10 nm to 400 nm.
[0239] [3] The polarizing film according to [1] or [2], wherein a hard coat layer is adjacent to the surface of the substrate opposite to the alignment film.
[0240] [4] The polarizing film according to any one of [1] to [3], wherein the substrate, the oriented film, and the polarizing film are elongated.
[0241] [5] The polarizing film according to [4], wherein the angle between the long side direction and the slow axis direction of the substrate is 0°±5° or 90°±5°.
[0242] Description of Reference Numerals
[0243] 1: Polarizing film, 2: Substrate, 3: Oriented film, 4: Polarizing film, 5: Hard coating.
Claims
1. A polarizing film, which is a polarizing film having a substrate, an orientation film and a polarizing film laminated in sequence, wherein: The angle between the slow axis direction of the substrate and the absorption axis direction of the polarizing film is 45°±5°, The refractive index difference between the polarizing film and the alignment film with respect to visible light satisfies the following formula (1), and the refractive index difference between the alignment film and the substrate with respect to visible light satisfies the following formula (2), |n(polarizing film)-n(oriented film)|≤0.06(1) |n(oriented film)-n(substrate)|≤0.06(2) In the formula (1), n(polarizing film) represents the refractive index in the transmission axis direction of the polarizing film.
2. The polarizing film according to claim 1, wherein The thickness of the alignment film is 10 nm to 400 nm.
3. The polarizing film according to claim 1, wherein: A hard coating layer is adjacent to a surface of the substrate opposite to the alignment film.
4. The polarizing film according to any one of claims 1 to 3, wherein The substrate, the alignment film, and the polarizing film are long. 5 . The polarizing film according to claim 4 , wherein the angle formed between the long side direction of the polarizing film and the slow axis direction of the substrate is 0°±5° or 90°±5°.
Citation Information
Patent Citations
Dichroic Guest-Host Polarizers Containing Oriented Polymer Films
JP2007510946A
Polarization element, circularly polarizing plate and method of manufacturing those
JP2013033249A