R-T-B type permanent magnet
By adopting the main phase and grain boundary phase structures composed of core and shell in the R-T-B type permanent magnet, and optimizing the Tb distribution through a multi-stage diffusion treatment process, the problem of insufficient performance in the existing technology is solved, and high-performance R-T-B is realized. Similar to permanent magnets.
Patent Information
- Application Number
- CN202410375803.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-11-28
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-01
AI Technical Summary
The existing R-T-B permanent magnets have insufficient performance in terms of magnetic flux density Br, coercive force Hcj and squareness ratio Hk/Hcj, making it difficult to improve them simultaneously.
The main phase and grain boundary phase structure composed of core and shell are adopted. The shell contains Tb. The thickness of the shell is more than 70nm. The Tb concentration gradually increases from the vicinity of the core. The grain boundary phase contains Fe and Co. It is optimized through a multi-stage diffusion treatment process. Tb distribution to improve magnetic properties.
It achieves higher residual magnetic flux density Br, coercive force Hcj and squareness ratio Hk/Hcj, improving the overall performance of the magnet, especially the coercive force and squareness ratio reaching more than 97.0%.
Smart Images

Figure CN118737604A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to RTB type permanent magnets. Background Art
[0002] Patent Document 1 discloses an invention regarding a method for producing a rare earth permanent magnet material. It states that by supplying a rare earth element (particularly Dy and / or Tb) compound to the surface of a sintered magnet and performing heat treatment, a rare earth permanent magnet material having a high residual magnetic flux density Br and coercive force Hcj can be provided.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: International Publication No. 2006 / 043348 Summary of the invention
[0006] Problems to be solved by the invention
[0007] An object of the present invention is to obtain an RTB type permanent magnet having high residual magnetic flux density Br, coercive force Hcj and squareness ratio Hk / Hcj.
[0008] Methods for solving problems
[0009] In order to achieve the above object, the present invention provides an RTB permanent magnet having a main phase composed of a core and a shell and a grain boundary phase adjacent to the main phase.
[0010] The shell contains Tb,
[0011] The shell has a thickness of 70 nm or more,
[0012] The maximum value of the Tb concentration in the shell is 1.7 at % or more.
[0013] The Tb concentration in the shell may gradually increase from the vicinity of the core toward the vicinity of the grain boundary phase.
[0014] When measuring points of Tb concentration are set at intervals of 10 nm from the core toward the grain boundary phase inside the shell, the closer the measuring point is to the grain boundary phase, the higher the Tb concentration can be, and the differences in Tb concentration between adjacent measuring points can all be greater than 0.01 at % and less than 0.50 at %.
[0015] The maximum value of the Tb concentration in the shell is defined as [Tb s ], the maximum value of the Tb concentration in the grain boundary phase is set to [Tb b ]hour,
[0016] It can also be 1.0≤[Tb b] / [Tb s ]≤1.5.
[0017] The Tb content may be 0.6 mass % or more and 2.1 mass % or less.
[0018] Fe or Fe and Co may be contained as transition metal elements.
[0019] The grain boundary phase may contain one or more selected from Fe and Co, and the minimum value of the total concentration of Fe and Co in the grain boundary phase may be 65.0 at % or less.
[0020] The squareness ratio Hk / Hcj may be 97.0% or more. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a schematic diagram showing the positional relationship between the main phase, the grain boundary phase, and the line segment AB.
[0022] Figure 2 It is a graph showing the change in Tb concentration in the line segment AB.
[0023] Figure 3 It is a graph showing the change in Cu concentration in the line segment AB.
[0024] Figure 4 It is a graph showing the change in the total concentration of Fe and Co and the change in the concentration of Nd in the line segment AB.
[0025] Figure 5 It is a schematic diagram showing the shape of the magnet according to the embodiment.
[0026] Description of Reference Numerals
[0027] 1…RTB type permanent magnet
[0028] 3… Center of Gravity
[0029] 11…Main phase
[0030] 13…Grain boundary phase DETAILED DESCRIPTION
[0031] Hereinafter, the present invention will be described based on specific embodiments.
[0032] <RTB type permanent magnet>
[0033] The RTB permanent magnet of this embodiment has a 14 The main phase grains of the crystal grains of the B-type crystal structure have grain boundaries formed by two or more adjacent main phase grains.
[0034] In RTB type permanent magnet and R2T 14In the B-type crystal structure, R represents a rare earth element, T represents a transition metal element, and B represents boron.
[0035] RTB type permanent magnet and R2T 14 The rare earth element contained as R in the B-type crystal structure may also be Sc, Y and lanthanum. The transition metal element contained as T does not contain a rare earth element. The transition metal element contained as T may also be an iron group element. The iron group element contained as T may also be one or more selected from Fe and Co. The iron group element contained as T may also be Fe or Fe and Co. A part of the boron contained as B may also be substituted by carbon.
[0036] In this embodiment, rare earth elements are classified into heavy rare earth elements and light rare earth elements. Heavy rare earth elements are Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu. Light rare earth elements are rare earth elements other than heavy rare earth elements. Iron group elements are Fe, Co, and Ni.
[0037] The magnet composition of the RTB-based permanent magnet of this embodiment is shown below. In addition, the measurement method of the RTB-based permanent magnet is not particularly limited. For example, XRF can be used.
[0038] The content of rare earth elements in the RTB permanent magnet is not particularly limited. It can be 25.0 mass% or more and 35.0 mass% or less, 29.0 mass% or more and 33.0 mass% or more, or 30.0 mass% or more and 32.0 mass% or less. When the content of R is 25.0 mass% or more, it is easy to fully carry out the crystals contained in the main phase of the RTB permanent magnet, that is, the crystals having R2T 14 The formation of crystals with a B-type crystal structure. In addition, the precipitation of soft magnetic α-Fe and the like is easily suppressed, and the reduction of magnetic properties is easily suppressed. When the content of R is 35.0 mass % or less, there is a tendency for the Br of the RTB permanent magnet to increase.
[0039] The content of heavy rare earth elements is not particularly limited. For example, it can be 0.1 mass% to 5.0 mass%, or 0.6 mass% to 2.1 mass%. The type of heavy rare earth elements is not particularly limited, but the RTB permanent magnet of this embodiment contains at least Tb. Heavy rare earth elements other than Tb may or may not be contained. In the case of containing heavy rare earth elements other than Tb, for example, Dy may also be contained.
[0040] The content of Tb is not particularly limited. For example, it can be 0.1 mass % to 5.0 mass %, or 0.6 mass % to 2.1 mass %. When Tb is high, Br is easily reduced. When Tb is low, Hcj is easily reduced.
[0041] The total content of the heavy rare earth elements other than Tb may be 0 mass % or more and 0.1 mass % or less. When the total content of the heavy rare earth elements other than Tb is 0.1 mass % or less, Br tends to increase.
[0042] The content of the light rare earth element is not particularly limited. In addition, the type of the light rare earth element is not particularly limited. For example, it can be one or more selected from Nd and Pr, or it can be Nd.
[0043] The total content of light rare earth elements other than Nd may be 0 mass % to 7.0 mass % or 0 mass % to 0.1 mass %. The total content of light rare earth elements other than Nd and Pr may be 0 mass % to 0.1 mass %.
[0044] The content of boron in the RTB permanent magnet is not particularly limited. It can be 0.50 mass % or more and 1.50 mass % or more, or 0.85 mass % or more and 1.05 mass % or less. When the content of boron is 0.50 mass % or more, Hcj tends to increase. In addition, when the content of boron is 1.50 mass % or less, Br tends to increase.
[0045] The carbon content in the RTB-based permanent magnet is not particularly limited, and may be, for example, 0 mass % or more and 0.10 mass % or less.
[0046] The content of Co in the RTB permanent magnet is not particularly limited. It can be 0% by mass or more and 4.00% by mass or less, or 0% by mass or more and 0.50% by mass or less, or 0% by mass or more and 0.30% by mass or less. The more Co content, the easier it is to increase the raw material cost. The less Co content, the easier it is to reduce the corrosion resistance.
[0047] The RTB-based permanent magnet of the present embodiment may contain Ga, Cu, Al and / or Zr as metal elements other than the above elements. The content of each element is not particularly limited.
[0048] The Ga content in the RTB-based permanent magnet may be 0 mass % to 0.15 mass % or more, or 0 mass % to 0.10 mass %.
[0049] The content of Cu in the RTB-based permanent magnet may be 0 mass % to 0.50 mass %, 0 mass % to 0.20 mass %, or more than 0 mass % to 0.05 mass %.
[0050] The Al content in the RTB-based permanent magnet may be 0 mass % to 0.40 mass % or more, or 0.25 mass % to 0.40 mass % to less.
[0051] The content of Zr in the RTB-based permanent magnet may be 0 mass % to 0.50 mass % or more, or 0 mass % to 0.20 mass % or less.
[0052] The RTB-based permanent magnet may contain oxygen and nitrogen in addition to the above-mentioned elements.
[0053] The content of oxygen in the RTB-based permanent magnet may be 0% by mass or more and 0.10% by mass or less. The content of nitrogen in the RTB-based permanent magnet may be 0% by mass or more and 0.10% by mass or less.
[0054] The content of Fe in the RTB permanent magnet may be the substantial remainder of the RTB permanent magnet. Specifically, the content of other elements, i.e., rare earth elements, Fe, Co, B, C, Ga, Cu, Al, Zr, O and elements other than N may be less than 1.0 mass % in total.
[0055] Examples of other elements include inevitable impurities such as Mn, Ca, Cl, S, and F.
[0056] like Figure 1 As shown, the RTB permanent magnet of this embodiment has a main phase 11 composed of a core and a shell and a grain boundary phase 13 adjacent to the main phase 11. The shell contains Tb. The grain boundary phase 13 contains one or more selected from Fe and Co. The thickness of the shell is 70 nm or more. Moreover, the maximum value of the Tb concentration in the shell is 1.7 at% or more.
[0057] The minimum value of the total concentration of Fe and Co in the grain boundary phase 13 may be 65.0 at % or less. The maximum value of the total concentration of the light rare earth element in the grain boundary phase 13 may be 25.0 at % or more.
[0058] The grain boundary phase 13 may contain transition metal elements other than Fe and Co. For example, it may contain Cu, Zr, Mn, Ni, etc. The ratio of the total concentration of Fe and Co contained in the grain boundary phase 13 to the total concentration of the transition metal elements may be 90% or more on an atomic basis.
[0059] The RTB-based permanent magnet of the present embodiment has the above-mentioned characteristics, and can improve Br, Hcj, and Hk / Hcj with a small amount of heavy rare-earth elements used.
[0060] The Tb concentration in the shell may also gradually increase from the vicinity of the core toward the vicinity of the grain boundary phase 13 .
[0061] The maximum value of Tb concentration in the shell is set to [Tb s] (at%), and the maximum value of the Tb concentration in the grain boundary phase 13 is set to [Tb b ](at%), or 1.0≤[Tb b ] / [Tb s ]≤1.5.
[0062] The Tb concentration in the core is not particularly limited. For example, it can be 0 at% to 2.0 at%. It is preferably 0.3 at% to 1.0 at%. When the core contains 0.3 at% to 1.0 at% Tb, the dissolution of the main phase 11 in the high temperature atmospheric pressure diffusion process described later is suppressed. Since the dissolution of the main phase 11 is suppressed, the shell of the main phase 11 does not become too thick, and the maximum value of the Tb concentration in the shell of the main phase 11 [Tb s ] tends to become high. Since the maximum value of the Tb concentration in the shell of the main phase 11 [Tb s ] becomes higher, so the Hcj of the RTB type permanent magnet tends to become higher.
[0063] The following describes a method for distinguishing the core, shell, and grain boundary phase 13 in the RTB permanent magnet of the present embodiment and a method for measuring various parameters. In the following description, the grain boundary phase 13 contains one or more transition metal elements selected from Fe and Co as other than rare earth elements, and contains only Tb and Nd as rare earth elements.
[0064] First, the measurement range of the RTB permanent magnet is set. The method of setting the measurement range will be described later. The RTB permanent magnet is cut at a position including the set measurement range to obtain a cross section.
[0065] The main phase 11 and the grain boundary phase 13 adjacent to the main phase 11 are selected on the obtained cross section using a three-dimensional atom probe microscope (3DAP).
[0066] Then, if Figure 1 As shown, a line segment AB is set which passes through the two main phases 11 and the grain boundary phase 13 existing between the two main phases 11 and is substantially perpendicular to the boundary line between the main phase 11 and the grain boundary phase 13. Figure 1 This is a diagram for explaining how to set the line segment AB. The actual length of the line segment AB is Figure 1 The lengths of the line segments AB shown are not necessarily the same.
[0067] Next, line analysis of the Tb concentration was performed along line segment AB. Figure 2 An example of the result is shown below. Figure 2 In FIG. 1 , the horizontal axis represents the distance from point A. Furthermore, the vertical axis represents the Tb concentration.
[0068] At the same time, elements that are difficult to be contained in the main phase 11, especially the shell, and are easy to be contained in the grain boundary phase 13 are selected ( Figure 3 The concentration of Cu in the figure is analyzed along line segment AB. Figure 3 An example of the result is shown. Figure 2 Same, in Figure 3 In FIG. 1 , the horizontal axis also represents the distance from point A. Moreover, the vertical axis represents the concentration of the element. Furthermore, the Fe concentration, the Co concentration, and the concentration of the light rare earth element (Nd concentration) are analyzed along the line segment AB. Figure 4 This shows an example of the result. Figure 4 : represents the concentration of each element in the grain boundary phase 13 and its vicinity.
[0069] according to Figure 3 , the boundary between the shell and the grain boundary phase 13 can also be determined visually. Figure 3 The Cu concentration decreases sharply from the grain boundary phase 13 toward the shell. The position where the Cu concentration is substantially constant is defined as the boundary between the shell and the grain boundary phase 13. Figure 3 The dashed line indicates the Figure 3 The location of the boundary is determined by Figure 2 The position of the boundary is Figure 3 same.
[0070] exist Figure 3 In the embodiment, the boundary between the shell and the grain boundary phase 13 is determined by the change in Cu concentration, but the boundary between the shell and the grain boundary phase 13 may be determined by using elements other than Cu, or by observing matters other than the change in the concentration of each element.
[0071] according to Figure 2 , the Tb concentration decreases from the boundary between the shell and the grain boundary phase 13 toward the interior of the main phase, and the Tb concentration is approximately constant at a location far enough from the boundary. The location where the Tb concentration is approximately constant is the core. The location where the concentration decreases from the boundary toward the main phase Tb is the shell. Based on the Tb concentration measurement results, visually determine whether the Tb concentration in the shell gradually increases from the vicinity of the core toward the vicinity of the grain boundary phase 13. Figure 2 In the embodiment, the Tb concentration in the shell gradually increases from the vicinity of the core toward the vicinity of the grain boundary phase 13. Figure 2 The core and shell boundaries were determined visually.
[0072] The boundary between the shell and the grain boundary phase 13 may be determined so that the Cu concentration in the grain boundary phase 13 is always 0.15 at % or more and the Cu concentration in the portion of the shell that contacts the grain boundary phase 13 is lower than 0.15 at %.
[0073] The portion contained in the core and at a distance of more than 100 nm from the boundary between the core and the shell may also be set as the interior of the core. The Tb concentration inside the core before the diffusion treatment described later is approximately equal to the Tb concentration of the substrate before the diffusion treatment. Since it is difficult to diffuse Tb into the interior of the core through the diffusion treatment process, the Tb concentration inside the core after the diffusion treatment is also approximately equal to the Tb concentration of the substrate before the diffusion treatment. Inside the core, the Tb concentration is approximately constant. The Tb concentration inside the core can be measured by methods such as 3DAP and EPMA. Moreover, the boundary between the core and the shell may also be determined so that the portion where the Tb concentration increases by more than 0.10 at% from the Tb concentration inside the core becomes the shell.
[0074] The portion included in the shell and at a distance of 1.0 nm or more from the grain boundary phase 13 in contact with the shell may be regarded as the inside of the shell. The Cu concentration is substantially constant inside the shell.
[0075] Alternatively, when measuring points of Tb concentration are set at intervals of 10 nm from the core toward the grain boundary phase 13 inside the shell, the closer the measuring point is to the grain boundary phase 13, the higher the Tb concentration is. Furthermore, the difference in Tb concentration between adjacent measuring points may all be 0.01 at% or more and 0.50 at% or less. Alternatively, when measuring points closer to the grain boundary phase 13, the higher the Tb concentration is, and when the difference in Tb concentration between adjacent measuring points is all 0.01 at% or more and 0.50 at% or less, the Tb concentration in the shell gradually increases from the vicinity of the core toward the vicinity of the grain boundary phase 13.
[0076] When 3DAP is used to measure the Tb concentration, provisional measurement points can be set at 1 nm intervals to measure the Tb concentration. Furthermore, the average position of 10 consecutive provisional measurement points can be used as the position of the above-mentioned measurement point, and the average Tb concentration of the 10 consecutive provisional measurement points can be used as the Tb concentration of the measurement point. When the position of the measurement point is set by the above method and the Tb concentration of the measurement point is measured, the influence of measurement noise is easily reduced, and the difference in Tb concentration between adjacent measurement points is less likely to cause errors.
[0077] When an element other than Cu (an element more likely to be contained in the grain boundary phase 13 ) is used to determine the boundary between the shell and the grain boundary phase 13 , Cu may be replaced with an element other than Cu (an element more likely to be contained in the grain boundary phase 13 ) in the above-mentioned boundary determination methods.
[0078] Furthermore, the thickness of the shell in the main phase 11, the Tb concentration in the core, the minimum value of the total concentration of Fe and Co in the grain boundary phase 13, the maximum value of the Nd concentration in the grain boundary phase 13, [Tb] and [Tb] can be determined based on the determined boundaries between the grain boundary phase 13 and the shell and between the shell and the core. s ] and [Tb bMoreover, it is possible to calculate [Tb b ] / [Tb s ].
[0079] The following is an explanation of the method for setting the measurement range. The measurement range may be any part of the RTB permanent magnet. In addition, the measurement range may be located in a part away from the surface of the RTB permanent magnet. For example, the measurement range may be a part that is more than 500 μm away from the surface of the RTB permanent magnet.
[0080] The content ratio of the main phase 11 having the above-mentioned structure in the RTB-based permanent magnet is not particularly limited.
[0081] For example, the content ratio of the main phase 11 having the above structure may be 80% or more based on the number of the main phases 11 contained in the RTB-based permanent magnet.
[0082] For example, the content ratio of the main phase 11 having the above structure to the main phase 11 contained in a portion 500 μm or more away from the surface of the RTB-based permanent magnet may be 65% or more on a number basis.
[0083] For example, a line segment may be drawn from the center of gravity of the surface of the RTB permanent magnet to the center of gravity of the RTB permanent magnet, and several measuring positions may be set at equal intervals on the line segment to confirm whether the main phase 11 at each measuring position has the above structure. At each measuring position, the content ratio of the main phase 11 having the above structure may be 80% or more on a number basis.
[0084] For example, with respect to the main phase 11 contained in the center of gravity of the RTB-type permanent magnet, that is, a part that has a similar shape and the same center of gravity as the RTB-type permanent magnet and accounts for about 10% of the volume, for example, more than 5% and less than 15%, the content ratio of the main phase 11 having the above-mentioned structure can also be more than 55% based on the number of pieces.
[0085] <Method for manufacturing RTB type permanent magnet>
[0086] Hereinafter, a method for producing the RTB-based permanent magnet will be described in detail, but matters not particularly described may be carried out using a known method.
[0087] [Raw material powder preparation process]
[0088] The raw material powder can be prepared by a known method. In this embodiment, the raw material powder is mainly prepared by using R2T 14 The RTB type permanent magnet can be manufactured by a single alloy method using one raw material alloy consisting of the B phase, but can also be manufactured by a two-alloy method using two raw material alloys.
[0089] First, a raw material metal corresponding to the composition of the raw material alloy of the present embodiment is prepared, and a raw material alloy corresponding to the present embodiment is produced from the raw material metal. There is no particular limitation on the method for producing the raw material alloy. For example, the raw material alloy can be produced by strip casting.
[0090] The greater the amount of Tb in the raw material alloy (mainly the raw material alloy that becomes the main phase when the two-alloy method is used), the more difficult it is for the Tb concentration in the grain boundary phase to be higher than the Tb concentration in the main phase in the grain boundary diffusion described below.
[0091] When the amount of Tb in the raw material alloy is large, dissolution of the main phase by the diffusion material is suppressed, and diffusion of Tb from the grain boundary phase to the main phase is suppressed.
[0092] By suppressing the dissolution of the main phase caused by the diffusion material, the extreme dissolution of the main phase near the diffusion surface is suppressed. By suppressing the extreme dissolution of the main phase near the diffusion surface, Tb can be diffused to the center of the magnet.
[0093] By inhibiting the diffusion of Tb from the grain boundary phase to the main phase, [Tb b ] / [Tb s ]Easy to become smaller.
[0094] After the raw material alloy is produced, the produced raw material alloy is crushed (crushing step). The crushing step can be carried out in two stages or in one stage. The crushing method is not particularly limited. For example, it can be carried out by using various crushers. For example, the crushing step can be carried out in two stages, namely, a coarse crushing step and a fine crushing step. The coarse crushing step can be subjected to a hydrogen crushing treatment, for example. Specifically, after hydrogen is absorbed in the raw material alloy at room temperature, dehydrogenation is carried out in an Ar gas atmosphere at a temperature between 400°C and 650°C for a period of 0.5 hours and less than 2 hours. In addition, the fine crushing step can be carried out by adding a lubricant such as oleamide or zinc stearate as a crushing aid to the coarsely crushed powder, using, for example, a jet mill or a wet mill. The particle size of the obtained finely crushed powder (raw material powder) is not particularly limited. For example, the particle size (D 50 ) is finely pulverized in the form of a finely pulverized powder (raw material powder) of 1 μm or more and 10 μm or less. In addition, from the hydrogen absorption pulverization to the sintering step described later, a low oxygen atmosphere with an oxygen concentration of less than 200 ppm can also be used throughout.
[0095] [Forming process]
[0096] In the molding step, the finely pulverized powder (raw material powder) obtained in the pulverization step is molded into a predetermined shape. The molding method is not particularly limited, but in this embodiment, the finely pulverized powder (raw material powder) is filled into a mold and pressurized in a magnetic field.
[0097] The pressure during molding is preferably between 30 MPa and 300 MPa. The applied magnetic field is preferably between 950 kA / m and 1600 kA / m. The applied magnetic field is not limited to a static magnetic field, but can also be a pulsed magnetic field. In addition, a static magnetic field and a pulsed magnetic field can also be used in combination. The shape of the molded body obtained by molding the finely pulverized powder (raw material powder) is not particularly limited, and can be, for example, a rectangular parallelepiped, a flat plate, a columnar shape, or any other shape according to the desired shape of the RTB permanent magnet.
[0098] [Sintering process]
[0099] The sintering process is a process of sintering the molded body in a vacuum or inert gas atmosphere to obtain a sintered body. The sintering temperature needs to be adjusted according to various conditions such as the composition, pulverization method, particle size and particle size distribution, but the molded body is sintered by heating it at 1000°C to 1200°C for 1 to 10 hours in a vacuum or in the presence of an inert gas. Thus, a high-density sintered body (permanent magnet) is obtained.
[0100] [Aging process]
[0101] The aging treatment step is performed by heating the sintered body (permanent magnet) after the sintering step at a temperature lower than the sintering temperature and in a vacuum or inert gas atmosphere. The temperature and time of the aging treatment are not particularly limited, but for example, it can be performed at 450°C to 900°C for 0.2 hours to 3 hours. In addition, the aging treatment step can also be omitted.
[0102] In addition, the aging treatment process can be carried out in one stage or in two stages. In the case of two stages, for example, the first stage can be set to be 700°C to 900°C and 0.2 hours to 3 hours, and the second stage can be set to be 450°C to 700°C and 0.2 hours to 3 hours. In addition, the first and second stages can be carried out continuously, or the second stage can be carried out after cooling to near room temperature after the first stage and then heating.
[0103] [Processing steps (before grain boundary diffusion)]
[0104] If necessary, the sintered body of the present embodiment may be processed into a desired shape. Examples of the processing method include cutting, shaping such as grinding, and chamfering such as barreling.
[0105] [Diffusion treatment process]
[0106] In this embodiment, there is also a diffusion treatment step for diffusing Tb. The diffusion treatment can be implemented by attaching a compound containing Tb to the surface of the sintered body and then performing a heat treatment. The type of compound containing Tb is arbitrary. For example, a hydride of Tb can be cited. The method of attaching the compound containing Tb is arbitrary. For example, it can be attached by applying a slurry containing Tb. By controlling the amount of slurry applied and the concentration of Tb contained in the slurry, the thickness of the shell and the concentration of Tb in the shell can be controlled. In addition, the Tb concentration of the core does not substantially change before and after the diffusion treatment step.
[0107] The method of attaching Tb is not particularly limited, and examples thereof include methods using vapor deposition, sputtering, electrodeposition, spraying, brush coating, jet dispenser, nozzle, screen printing, squeegee printing, sheet process, and the like.
[0108] When the slurry is applied, the compound containing Tb is preferably in a particle form and has an average particle size of preferably 100 nm to 50 μm, more preferably 1 μm to 30 μm.
[0109] As the solvent used in the slurry, a solvent that does not dissolve the compound containing Tb but can be uniformly dispersed is preferred, and examples thereof include alcohols, aldehydes, and ketones, and among them, ethanol is preferred.
[0110] The content of the compound containing Tb in the slurry is not particularly limited. For example, it can be 50% by mass or more and 90% by mass or less. The slurry may contain components other than Tb as needed. For example, a dispersant for preventing the aggregation of Tb particles may be mentioned.
[0111] By subjecting the sintered body to the above diffusion treatment step, Tb diffuses into the grain boundaries of the entire sintered body, and a shell having a high Tb concentration is formed in the main phase, thereby obtaining a main phase composed of a core and a shell.
[0112] In this embodiment, the diffusion process is divided into multiple stages. Specifically, the diffusion process is performed by repeatedly performing the diffusion process in a low-temperature reduced pressure atmosphere and the diffusion process in a high-temperature atmospheric pressure atmosphere. First, the temperature in the atmosphere is raised from room temperature to the diffusion process temperature in the low-temperature reduced pressure atmosphere. At the same time, the pressure in the atmosphere is reduced from atmospheric pressure to the diffusion process pressure in the low-temperature reduced pressure atmosphere. Then, the predetermined holding time is maintained in the low-temperature reduced pressure atmosphere.
[0113] The diffusion treatment temperature in the low temperature and reduced pressure atmosphere may be, for example, 500° C. to 700° C. The diffusion treatment pressure in the low temperature and reduced pressure atmosphere may be, for example, 0.1 kPa to 20 kPa. The holding time in the low temperature and reduced pressure atmosphere is not particularly limited. For example, it may be 3 hours to 9 hours.
[0114] Next, the temperature in the atmosphere is raised from the diffusion processing temperature in the low-temperature reduced-pressure atmosphere to the diffusion processing temperature in the high-temperature atmospheric pressure atmosphere. At the same time, the pressure in the atmosphere is raised from the diffusion processing pressure in the low-temperature reduced-pressure atmosphere to the diffusion processing pressure in the high-temperature atmospheric pressure atmosphere. Next, the high-temperature atmospheric pressure atmosphere is maintained for a predetermined holding time.
[0115] The diffusion treatment temperature in the high temperature atmospheric pressure atmosphere may be, for example, 750° C. to 1000° C. The diffusion treatment pressure in the high temperature atmospheric pressure atmosphere may be, for example, 80 kPa to 120 kPa. The holding time in the high temperature atmospheric pressure atmosphere is not particularly limited. For example, it may be 3 hours to 9 hours.
[0116] In the diffusion treatment under the low temperature and reduced pressure atmosphere initially performed in the diffusion treatment process, the dissolution of the grain boundary and the diffusion material (compounds containing Tb, etc.) can be promoted while suppressing the dissolution of the main phase. Therefore, in the diffusion treatment under the low temperature and reduced pressure atmosphere initially performed, it is difficult for Tb to diffuse into the main phase near the diffusion surface (the surface to which the compound containing Tb is attached) of the RTB-type permanent magnet. Moreover, the difference in Tb concentration between the grain boundary phase near the diffusion surface of the RTB-type permanent magnet and the grain boundary phase inside the RTB-type permanent magnet becomes the driving force for Tb diffusion. Therefore, Tb easily diffuses from the grain boundary phase near the diffusion surface of the RTB-type permanent magnet to the grain boundary phase inside the RTB-type permanent magnet.
[0117] In the diffusion treatment under high temperature atmospheric pressure atmosphere which is then carried out in the diffusion treatment process, the dissolution of the main phase, especially the part adjacent to the grain boundary phase, is carried out. In the diffusion treatment under low temperature and reduced pressure atmosphere, Tb diffused into the grain boundary phase of the whole RTB permanent magnet diffuses into the main phase adjacent to the grain boundary. During the subsequent cooling, the dissolved main phase reprecipitates on the surface of the undissolved main phase. At this time, the amount of Tb contained in the reprecipitated part increases.
[0118] As a result, compared with the diffusion method of the existing diffusion treatment process, it is easy to diffuse Tb into the RTB permanent magnet, especially into the magnet. Moreover, inside the RTB permanent magnet, the shell contained in the main phase can be thickened, and the Tb concentration of the shell can be increased. Furthermore, it is easy to reduce the difference in Tb concentration between the surface of the RTB permanent magnet and the main phase inside. Therefore, an RTB permanent magnet with high Br, Hcj and Hk / Hcj is obtained.
[0119] In particular, Hcj can be improved because the high Tb concentration in the shell increases the magnetic anisotropy of the outer edge of the main phase, which is the starting point of magnetization reversal, and the thick shell promotes magnetic disconnection between adjacent main phases.
[0120] In particular, Hk / Hcj can be increased, and in particular, can be made 97.0% or more. This is considered to reduce the difference in Tb concentration between the main phase inside the magnet and the magnet surface, thereby reducing the variation in magnetic properties of the entire magnet.
[0121] Below, it is also possible to repeatedly perform diffusion treatment under low temperature reduced pressure atmosphere and diffusion treatment under high temperature atmospheric pressure atmosphere. In the case of repeatedly performing diffusion treatment under low temperature reduced pressure atmosphere and diffusion treatment under high temperature atmospheric pressure atmosphere, it is also possible to appropriately change diffusion treatment temperature, diffusion treatment pressure and / or holding time according to the number of repetitions. In addition, by repeatedly performing diffusion treatment under low temperature reduced pressure atmosphere and diffusion treatment under high temperature atmospheric pressure atmosphere, the Tb concentration in the shell of the main phase is easily increased gradually from the vicinity of the core of the main phase toward the vicinity of the grain boundary phase adjacent to the main phase.
[0122] In addition, in the diffusion method of the existing diffusion process, the main phase near the magnet surface near the diffusion material is dissolved by the diffusion material. Therefore, Tb will excessively stay near the magnet surface near the diffusion material. Moreover, the diffusion of Tb from the magnet surface near the diffusion material to the center of the magnet will stagnate. Since it is difficult for Tb to diffuse into the grain boundary phase in the center of the magnet, the diffusibility of Tb from the grain boundary phase in the center of the magnet to the main phase is further reduced. As a result, in the comparison between the grain boundary phase in the center of the magnet and the main phase in the center of the magnet, the grain boundary phase in the center of the magnet is likely to contain more Tb, [Tb b ] / [Tb s ] is likely to be higher than 1.5. Therefore, the coercive force and the squareness ratio are likely to be lower than those of the RTB permanent magnet of this embodiment.
[0123] Furthermore, an aging treatment step may be performed after the heat treatment in the diffusion treatment step.
[0124] The surface to which Tb is attached (diffusion surface) may be polished after the diffusion process to remove the residue. The above method can reduce the Tb content in the residue removed by diffusing Tb, and can effectively use expensive Tb to improve the magnetic properties of the RTB permanent magnet.
[0125] Although preferred embodiments of the RTB permanent magnet of the present invention have been described above, the RTB permanent magnet of the present invention is not limited to the above embodiments. The RTB permanent magnet of the present invention can be variously modified and combined without departing from the gist of the present invention.
[0126] Furthermore, it is possible to use a magnet obtained by cutting and dividing the RTB-based permanent magnet of the present embodiment.
[0127] Specifically, the RTB-based permanent magnet of the present embodiment is suitable for use in motors, compressors, magnetic sensors, speakers, and the like.
[0128] In addition, the RTB permanent magnet of this embodiment can be used alone, or two or more RTB permanent magnets can be combined and used as needed. There is no particular limitation on the combination method. For example, there are mechanical combination methods or resin molding combination methods.
[0129] By combining two or more RTB permanent magnets, a large RTB permanent magnet can be easily manufactured. The magnet combining two or more RTB permanent magnets is particularly preferably used for applications requiring large RTB permanent magnets, such as IPM motors, wind turbines, large motors, etc.
[0130] [Example]
[0131] Hereinafter, the present invention will be described based on more detailed examples, but the present invention is not limited to these examples.
[0132] (Magnet manufacturing process before Tb diffusion)
[0133] As raw material metals, Nd, Tb, electrolytic iron, and low-carbon iron-boron alloys are prepared. Furthermore, Al, Cu, Co, and Zr are prepared in the form of alloys with pure metals or Fe.
[0134] The raw metals were strip cast to produce raw alloys in such a manner that the composition of the magnet before Tb diffusion described later became the composition shown in Table 1. In addition, the Fe content is recorded as bal., which means that the Fe content is substantially the remainder. In all the examples and comparative examples, the content of elements other than the elements shown in Table 1 was 1% by mass or less. In addition, the alloy thickness of the raw alloy was 0.2 mm to 0.6 mm.
[0135] As elements other than those shown in Table 1, H, Si, Ca, La, Ce, Cr, etc. are sometimes detected as inevitable impurities. Si is mainly mixed from the iron boron raw material and the crucible when the alloy is dissolved. Ca, La, and Ce are mixed from rare earth raw materials. In addition, Cr may be mixed from electrolytic iron.
[0136] Next, hydrogen gas was flowed over the raw alloy at room temperature for 1 hour to absorb hydrogen. Next, the atmosphere was switched to Ar gas, and a dehydrogenation treatment was performed at 450° C. for 1 hour to hydrogen-crush the raw alloy. After cooling, a powder with a particle size of 400 μm or less was obtained using a sieve.
[0137] Next, a lubricant (oleic acid amide) was added as a pulverization aid in an amount of 0.1% by mass to the powder of the raw alloy after hydrogen pulverization, and the mixture was mixed.
[0138] Next, the particles were finely pulverized in a nitrogen stream using a collision plate type jet mill to obtain fine powders (raw material powders) with an average particle size of about 4 μm. The average particle size is the average particle size D measured by a laser diffraction particle size distribution meter. 50 .
[0139] The obtained fine powder was formed in a magnetic field to produce a molded body. The applied magnetic field at this time was a static magnetic field of 1200 kA / m. In addition, the pressure during molding was 120 MPa. In addition, the direction of magnetic field application and the direction of pressure application were orthogonal. When the density of the molded body at this time was measured, the density of all the molded bodies was 4.10 Mg / m 3 Above 4.25Mg / m 3 Within the following range.
[0140] Next, the molded body is sintered to obtain a pre-Tb diffusion magnet. The sintering conditions are 1060°C for 4 hours. The sintering atmosphere is vacuum. At this time, the sintered density is 7.50Mg / m 3 Above 7.55Mg / m 3 Then, in an Ar atmosphere and atmospheric pressure, a first aging treatment was performed at a first aging temperature T1 = 900° C. for 1 hour, and a second aging treatment was performed at a second aging temperature T2 = 500° C. for 1 hour.
[0141] The composition of the obtained permanent magnet before diffusion was evaluated by fluorescent X-ray analysis. The content of B was evaluated by ICP. As a result, it was confirmed that the composition was substantially the same as that of the raw material alloy. Then, the obtained permanent magnet before diffusion was subjected to the following treatment.
[0142] (Comparative Example 1)
[0143] The Tb pre-diffusion magnet obtained through the above process is processed into Figure 5 The rectangular parallelepiped shown. W = 20 mm, H = 10 mm. For D, the length of D in the final permanent magnet is 4 mm. The orientation direction is parallel to D. Then, TbH2 particles (D) dispersed in ethanol are applied to both surfaces of the 20 mm × 10 mm magnet before Tb diffusion. 50 =5 μm) slurry was used to adhere Tb. The total amount of Tb adhered to the mass of the magnet before Tb diffusion was the ratio shown in Table 1.
[0144] After the slurry is applied, the diffusion treatment pressure is set to atmospheric pressure (100 kPa), and a heat treatment is performed at a diffusion treatment temperature of 850°C for 24 hours while Ar is flowing to diffuse Tb grain boundaries. Furthermore, an aging treatment is performed at 500°C for 1 hour in an Ar atmosphere and atmospheric pressure.
[0145] Next, two surfaces of 20 mm×10 mm as diffusion surfaces were cut by 500 μm in the D direction to obtain permanent magnets (Tb diffused magnets) of various samples with dimensions of W=20 mm, H=10 mm, and D=4 mm.
[0146] The Tb content in the obtained permanent magnet was measured using a fluorescent X-ray analyzer (XRF).
[0147] The magnetic properties (Br, Hcj and Hk / Hcj) of the obtained permanent magnets were evaluated at RT (23°C) using a BH tracer. In this experimental example, Hcj of 2000 kA / m or more was considered good, and 2300 kA / m or more was considered even better. Hk / Hcj of 97.0% or more was considered good.
[0148] Furthermore, for the obtained RTB permanent magnet 1, the main phase 11 located at the measurement position (center of gravity 3) 2.0 mm inside in the D direction from the center of gravity of the 20 mm × 10 mm surface was used to obtain a three-dimensional distribution image of atoms using 3DAP. Furthermore, it was confirmed that the main phase 11 had a core and a shell. Figure 1 As shown, 3DAP is used to set a line segment AB passing through the main phase 11 and the grain boundary phase 13 adjacent to the main phase 11, and line analysis is performed on the Tb concentration, Cu concentration, Fe concentration, Co concentration, and Nd concentration in the line segment AB to generate Figure 2 to Figure 4 Based on the shape of the graph, the Tb concentration in the core, the shell thickness, the minimum value of the total concentration of Fe and Co in the grain boundary phase, the maximum value of the Nd concentration in the grain boundary phase, [Tb s ] and [Tb b ], calculate [Tb b ] / [Tb s ]. The results are shown in Table 1.
[0149] Figure 2 The dotted line is a dotted line corresponding to the grain boundary of Example 1, not a dotted line corresponding to the grain boundary of Comparative Example 1. However, the grain boundary phase of Comparative Example 1 is located close to the position indicated by the dotted line. In addition, Comparative Example 1 does not contain Co. Therefore, Figure 4 The change in the concentration of Fe+Co in Comparative Example 1 shown is the same as the change in the concentration of Fe.
[0150] (Examples 1 to 6)
[0151] Examples 1 to 6 were carried out under the same conditions as Comparative Example 1, except that the diffusion process was performed as a multi-stage diffusion. The diffusion process of Examples 1 to 6 is shown below.
[0152] After applying the above slurry, a diffusion treatment is performed under a low-temperature reduced-pressure atmosphere. Specifically, the diffusion treatment pressure is set to 1 kPa, and a heat treatment is performed at a diffusion treatment temperature of 600°C while Ar is flowing, and a heat treatment is performed for 6 hours. Next, a diffusion treatment is performed under a high-temperature atmospheric pressure atmosphere. Specifically, the diffusion treatment pressure is increased to atmospheric pressure (100 kPa), the diffusion treatment temperature is increased to 850°C (870°C for Example 5 only), and a heat treatment is performed for 6 hours at a temperature of 600°C. Next, a diffusion treatment is performed under a low-temperature reduced-pressure atmosphere. Specifically, the diffusion treatment pressure is set to 1 kPa, and a heat treatment is performed at a diffusion treatment temperature of 600°C while Ar is flowing, and a heat treatment is performed for 6 hours at a temperature of 600°C. Next, a diffusion treatment is performed under a high-temperature atmospheric pressure atmosphere. Specifically, the diffusion treatment pressure is increased to atmospheric pressure (100 kPa), the diffusion treatment temperature is increased to 850°C (870°C for Example 5 only), and a heat treatment is performed for 6 hours at a temperature of 600°C. Furthermore, an aging treatment is performed at 500°C in an Ar atmosphere and atmospheric pressure for 1 hour. The results are shown in Table 1.
[0153] [Table 1]
[0154]
[0155] According to Table 1, in each embodiment in which the diffusion process is set as a multi-stage diffusion, the shell thickness is 70nm or more, [Tb s ] is 1.7 at% or more, and the minimum value of the total concentration of Fe and Co in the grain boundary phase is 65.0 at% or less. As a result, each embodiment has good Hcj and Hk / Hcj. On the other hand, in Comparative Example 1, in which the magnet does not contain Tb before Tb diffusion and the diffusion process is not a multi-stage diffusion, the shell thickness and [Tb s ] is too small, Hcj and Hk / Hcj are reduced.
[0156] It was confirmed that even when the boundary between the shell and the grain boundary phase was determined so that the Cu concentration in the grain boundary phase was always 0.15 at% or more, the Cu concentration in the portion in contact with the grain boundary phase in the shell was lower than 0.15 at%, and the boundary between the core and the shell was determined so that the portion where the Tb concentration increased by 0.10 at% or more from the Tb concentration inside the shell was the shell, there was no change in the test results shown in Table 1. In this case, the calculation was performed assuming that the Tb concentration inside the core was equal to the Tb concentration of the magnet before Tb diffusion.
[0157] In all the examples, it was confirmed that when the measurement points of the Tb concentration were set at intervals of 10 nm from the core toward the grain boundary phase 13 inside the shell, the closer the measurement point was to the grain boundary phase 13, the higher the Tb concentration was, and the difference in Tb concentration between adjacent measurement points was 0.01 at% or more and 0.50 at% or less. In other words, in all the examples, it was confirmed that the Tb concentration in the shell gradually increased from the vicinity of the core toward the vicinity of the grain boundary phase.
[0158] On the other hand, in Comparative Example 1, it was confirmed that when the measurement points of the Tb concentration were set at intervals of 10 nm from the core toward the grain boundary phase 13 inside the shell, the difference in Tb concentration between adjacent measurement points was sometimes about 1 at%. That is, in Comparative Example 1, it was confirmed that the Tb concentration in the shell did not gradually increase from the vicinity of the core toward the vicinity of the grain boundary phase.
Claims
1. An RTB type permanent magnet, characterized in that: having a main phase consisting of a core and a shell and a grain boundary phase adjacent to the main phase, The shell contains Tb, The shell has a thickness of 70 nm or more, The maximum value of the Tb concentration in the shell is 1.7 at % or more.
2. The RTB type permanent magnet according to claim 1, characterized in that: The Tb concentration in the shell gradually increases from the vicinity of the core toward the vicinity of the grain boundary phase.
3. The RTB type permanent magnet according to claim 1 or 2, characterized in that: When measuring points of Tb concentration are set at intervals of 10 nm from the core to the grain boundary phase inside the shell, the closer the measuring point is to the grain boundary phase, the higher the Tb concentration is, and the differences in Tb concentration between adjacent measuring points are all 0.01 at % to 0.50 at %.
4. The RTB type permanent magnet according to claim 1 or 2, characterized in that: The maximum value of the Tb concentration in the shell is defined as [Tb s ], the maximum value of the Tb concentration in the grain boundary phase is set to [Tb b ], satisfied 1.0≤[Tb b ] / [Tb s ]≤1.5。 5. The RTB type permanent magnet according to claim 1 or 2, characterized in that: The content of Tb is 0.6 mass % or more and 2.1 mass % or less.
6. The RTB type permanent magnet according to claim 1 or 2, characterized in that: Contains Fe or Fe and Co as transition metal elements.
7. The RTB type permanent magnet according to claim 1 or 2, characterized in that: The grain boundary phase contains one or more elements selected from Fe and Co, and the minimum value of the total concentration of Fe and Co in the grain boundary phase is 65.0 at % or less.
8. The RTB type permanent magnet according to claim 1 or 2, characterized in that: The squareness ratio Hk / Hcj is 97.0% or more.
Citation Information