Lithium nickel manganese oxide positive active material and preparation method thereof, positive pole piece and battery
Through the mixed single-crystalline nickel-manganese lithium manganese material of spherical particles and octahedral particles, combined with the doping of M and N elements, the problem of the easy breakage of nickel-manganese lithium manganese material and Mn3+ dissolution during the rolling process is solved. It improves the energy density and circulation performance of the battery, and enhances the safety and stability of the battery.
Patent Information
- Application Number
- CN202411046827.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
AI Technical Summary
Spinel-type lithium nickel-manganate material is prone to shatter during rolling, with Jahn-Teller effect, and Mn3+ is easily dissolved, affecting the electrochemical performance of the battery.
Using a mixed single-crystal nickel-manganese lithium material with spherical particles and octahedral particles, the particle morphology and surface energy are regulated by doping M and N elements, reducing the risk of crushing and the probability of Mn3+ dissolution, and improving the battery energy Density and cycling performance.
It improves the energy density and cycling performance of the battery, reduces the risk of crushing and processing costs of lithium nickel manganate during rolling, and enhances the safety and stability of the battery.
Smart Images

Figure CN118983433A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of batteries, and in particular, to a lithium nickel manganese oxide positive electrode active material and a preparation method thereof, a positive electrode sheet, and a battery. Background Art
[0002] The positive electrode active material is a key component of the battery, which determines the energy density and cycle life of the entire battery, and is also the most expensive part of the battery. Spinel-type lithium nickel manganese oxide material is developed on the basis of spinel lithium manganese oxide. It has the advantages of abundant resources, environmental friendliness and low cost. The material has a three-dimensional framework structure, a stable and efficient lithium ion transmission path, and a wide operating voltage window, which makes the battery including the spinel lithium nickel manganese oxide positive electrode active material have a high energy density, and therefore has great development prospects. However, the spinel phase has crystal self-limitation, and the conventional spinel lithium nickel manganese oxide is a regular octahedral structure with clear edges and corners. The sharp corners of the octahedron are easily crushed during the rolling process, and there is a risk of puncturing the aluminum foil during the battery cell manufacturing process. In addition, the material has the Jahn-Teller effect, and Mn 3+ It is easy to dissolve at sharp corners, which is detrimental to the electrochemical performance of the battery. Summary of the invention
[0003] The present application proposes a lithium nickel manganese oxide positive electrode active material, wherein the X-ray diffraction spectrum of the lithium nickel manganese oxide positive electrode active material satisfies: 0.13≤I h / I w ≤0.28, where I w =I (111) +I (311) +I (400) , I h =I (331) +I (511) +I (531) , I (111) is the diffraction peak intensity of the crystal plane (111), I (311) is the diffraction peak intensity of the crystal plane (311), I (400) is the diffraction peak intensity of the crystal plane (400), I (331) is the diffraction peak intensity of the crystal plane (331), I (511) is the diffraction peak intensity of the crystal plane (511), I (531) is the diffraction peak intensity of the crystal plane (531). Therefore, the lithium nickel manganese oxide positive electrode active material proposed in the present application is a single-crystal lithium nickel manganese oxide particle mixed with spherical particles and truncated octahedral particles. Compared with a single spherical single-crystal lithium nickel manganese oxide or a single truncated octahedral single-crystal lithium nickel manganese oxide, the presence of spherical single-crystal particles can reduce the risk of lithium nickel manganese oxide breaking and piercing the aluminum foil during the rolling process, thereby increasing the compaction density of the positive electrode sheet and the energy density of the battery; the presence of truncated octahedral particles can also reduce the Mn in lithium nickel manganese oxide.3+ The probability of dissolution is increased, while exposing the (111) crystal plane, the (100) crystal plane and / or the (110) crystal plane, thereby improving the energy density and cycle performance of the battery.
[0004] According to some embodiments of the present application, the number of spherical particles in the lithium nickel manganese oxide positive electrode active material is n, the roundness of the spherical particles is R, and the following conditions are satisfied: 0.75≤R≤1, 10%≤n≤40%. Thus, the risk of lithium nickel manganese oxide breaking and piercing aluminum foil during rolling is reduced, the compaction density of lithium nickel manganese oxide powder is increased, and the energy density of the battery is increased.
[0005] According to some embodiments of the present application, the lithium nickel manganese oxide positive electrode active material satisfies at least one of the following conditions: 0.9≤R≤1; 15%≤n≤25%. Thus, the roundness of the spherical single crystal particles is improved, and the compaction density of the lithium nickel manganese oxide powder is increased; the number of spherical single crystal particles is reduced, the hardness of the lithium nickel manganese oxide material is reduced, and the crushing processing cost is reduced.
[0006] According to some embodiments of the present application, the lithium nickel manganese oxide positive electrode active material includes: Li (1+a) (Ni 0.5 Mn 1.5 ) (1-a-b-c) M b N c O4, wherein -0.3≤a≤0.3, 0<b≤0.002, 0≤c≤0.003, the M includes at least one of B, W, P, Nb, Mo, Ta, Si, and Ce, and the N includes at least one of Y, Cr, and Co. Thus, the M element and the N element are doped in the lithium nickel manganese oxide material, and the M element and the N element both have an effect on the properties of the lithium nickel manganese oxide positive electrode material particles. The M element can promote the formation of the spherical morphology of the particles in the lithium nickel manganese oxide, and the N element can promote the formation of the truncated corner / edge octahedral morphology of the particles in the lithium nickel manganese oxide material, thereby improving the energy density and cycle performance of the battery.
[0007] According to some embodiments of the present application, the lithium nickel manganese oxide positive electrode active material satisfies at least one of the following conditions: the M includes at least one of B and Nb; the N includes Y. Thus, single crystal lithium nickel manganese oxide particles of a mixture of spherical particles and truncated octahedral particles are obtained, the compaction density of the material is increased, and thus the energy density and cycle performance of the battery are improved.
[0008] According to some embodiments of the present application, at least one of the following conditions is satisfied: 0.0003≤b≤0.001; 0.0005≤c≤0.0015, c>b.
[0009] According to some embodiments of the present application, the compaction density of the lithium nickel manganese oxide positive electrode active material is 2.9 g / cm 3-3.4g / cm 3 , optional 3.1g / cm 3 -3.3g / cm 3 . Thus, the compaction density of the positive electrode sheet of the battery is increased, and the energy density of the battery is increased.
[0010] The second aspect of the present application provides a method for preparing a positive electrode active material of lithium nickel manganese oxide, the method comprising: mixing a nickel source, a manganese source, a lithium source, an M source, and an N source according to a stoichiometric ratio to obtain a mixture; heating the mixture to a first temperature for sintering, cooling it to a second temperature for annealing, and cooling it to obtain a block of lithium nickel manganese oxide; and crushing the block of lithium nickel manganese oxide. Thus, by doping M and N elements in the process of preparing lithium nickel manganese oxide, sintering at a constant temperature to obtain uniform and full single crystal large particles, and then repairing the defects in the reaction process of lithium nickel manganese oxide by annealing, a single crystal lithium nickel manganese oxide particle of a mixture of spherical particles and truncated octahedral particles is formed, while improving the compaction density of the material, improving the energy density and cycle performance of the battery, reducing the hardness of the single crystal lithium nickel manganese oxide particles, and reducing the process cost of later crushing.
[0011] According to some embodiments of the present application, the method further comprises: mixing the nickel manganese precursor, the lithium source, the M source, and the N source according to a stoichiometric ratio, thereby improving the uniformity of the distribution of the N element in the single crystal lithium nickel manganese oxide particles and reducing the segregation of the element.
[0012] According to some embodiments of the present application, the first temperature is T1, the second temperature is T2, and 250°C≤T1-T2≤500°C is satisfied.
[0013] According to some embodiments of the present application, the method satisfies at least one of the following conditions: 850°C ≤ T1 ≤ 1100°C; 600°C ≤ T2 ≤ 800°C. Thus, by setting the constant temperature sintering temperature within the above range, more uniform and full single crystal large particles can be obtained; by setting the annealing temperature within the above range, defects generated during the reaction of lithium nickel manganese oxide can be repaired, and the Mn 3+ content, reducing the generation of oxygen vacancies and further improving the battery's cycle performance.
[0014] According to some embodiments of the present application, the cooling rate from the first temperature to the second temperature is 1°C / min-4°C / min. Thus, by making the cooling rate within the above range, while reducing Mn 3+ The content of nickel manganese oxide can be increased, the repair effect on the surface of the lithium nickel manganese oxide positive electrode active material can be improved, and the process cost can be reduced.
[0015] According to some embodiments of the present application, the holding time of the mixture heated to the first temperature is t1, and the holding time of the mixture cooled to the second temperature is t2, and at least one of the following conditions is satisfied: 6h≤t1≤12h, optionally, 8h≤t1≤10h; 2h≤t2≤6h, optionally, 3.5h≤t2≤4h. Thus, by making the holding time of constant temperature sintering within the above range, more uniform and full single crystal large particles can be obtained; by making the holding time of annealing within the above range, the defects generated during the reaction of lithium nickel manganese oxide can be repaired, and the Mn 3+ content, reducing the generation of oxygen vacancies and further improving the battery's cycle performance.
[0016] According to some embodiments of the present application, the sintering and the annealing are performed independently in air or oxygen atmosphere, thereby reducing process costs.
[0017] According to some embodiments of the present application, the sintering is performed in an oxygen atmosphere, thereby allowing the lithium source and other raw materials to fully react with each other, thereby making it easier to obtain single-crystal lithium nickel manganese oxide particles of a mixture of spherical particles and truncated octahedral particles.
[0018] According to some embodiments of the present application, the nickel-manganese precursor satisfies at least one of the following conditions: 3μm≤Dv50≤5μm, wherein Dv50 is the volume distribution average particle size of the nickel-manganese precursor; 0.8≤(Dv90-Dv10) / Dv50≤1.2, wherein Dv10 is the particle size corresponding to when the volume distribution percentage of the nickel-manganese precursor particle size reaches 10%, and Dv90 is the particle size corresponding to when the volume distribution percentage of the nickel-manganese precursor particle size reaches 90%. As a result, the particle size distribution of the nickel-manganese precursor is narrow, which can improve the uniformity of the lithium nickel manganese oxide single crystal particles.
[0019] The third aspect of the present application provides a positive electrode sheet, comprising the lithium nickel manganese oxide positive electrode active material provided in the first aspect of the present application, thereby increasing the compaction density of the positive electrode sheet and the energy density of the battery.
[0020] The fourth aspect of the present application provides a battery, comprising the positive electrode plate provided in the third aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0022] Figure 1 A schematic flow chart of a method for preparing lithium nickel manganese oxide material according to an embodiment of the present application is shown.
[0023] Figure 2The SEM image of the lithium nickel manganese oxide material prepared in Example 11 of the present application is shown.
[0024] Figure 3 The SEM image of the lithium nickel manganese oxide material prepared in Example 3 of the present application is shown.
[0025] Figure 4 The SEM image of the lithium nickel manganese oxide material prepared in Example 9 of the present application is shown.
[0026] Figure 5 The SEM image of the lithium nickel manganese oxide material prepared in Comparative Example 1 of the present application is shown.
[0027] Figure 6 The XRD spectrum of the lithium nickel manganese oxide material prepared in Example 11 of the present application is shown. DETAILED DESCRIPTION
[0028] The embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application.
[0029] In a first aspect, the present application provides a lithium nickel manganese oxide positive electrode active material, wherein the X-ray diffraction spectrum of the lithium nickel manganese oxide positive electrode active material satisfies:
[0030] 0.13≤I h / I w ≤0.28,
[0031] Among them, I w =I (111) +I (311) +I (400) , I h =I (331) +I (511) +I (531) , I (111) is the diffraction peak intensity of the crystal plane (111), I (311) is the diffraction peak intensity of the crystal plane (311), I (400) is the diffraction peak intensity of the crystal plane (400), I (331) is the diffraction peak intensity of the crystal plane (331), I (511) is the diffraction peak intensity of the crystal plane (511), I (531)is the diffraction peak intensity of the crystal plane (531). Specifically, the crystal planes (111), (311) and (400) are low-index energy crystal planes, and the crystal planes (331), (511) and (531) are high-index energy crystal planes. Conventional spinel lithium nickel manganese oxide is a regular octahedral structure with clear edges and corners, and the (111) crystal plane is fully exposed.
[0032] This application is made by h and I w The ratio of is within the above range, increasing the proportion of spherical particles in the mixed nickel manganese oxide particles, reducing the risk of nickel manganese oxide breaking and piercing the aluminum foil during rolling, thereby increasing the compaction density of the positive electrode sheet and the energy density of the battery; at the same time, the presence of truncated octahedral particles can also reduce the Mn 3+ The probability of dissolution is increased, and the (111) crystal plane, (100) crystal plane and / or (110) crystal plane are exposed at the same time. The (111) crystal plane has low surface energy, which is beneficial to the battery cycle performance. h and I w The ratio is too small, the number of spherical particles in the mixed nickel manganese oxide is too small, and the risk of the material piercing the aluminum foil during the rolling process increases; if I h and I w If the ratio is too large, the hardness of the mixed nickel manganese oxide lithium particles will be too large, making them difficult to crush and dissociate, which will increase the crushing process cost.
[0033] In the present application, the X-ray diffraction of the positive active material of lithium nickel manganese oxide is obtained by testing with an XRD-6000 X-ray powder diffractometer (Shimadzu, Japan). The test conditions of XRD are: Cu target, Kα ray (wavelength λ = 0.154nm), tube voltage of 40kV, tube current of 200mA, and scanning speed of 10° (2θ) / min.
[0034] As an example, I h / I w It may be 0.13, 0.15, 0.17, 0.19, 0.21, 0.23, 0.25 or 0.28, etc., or may be a range consisting of any of the above values.
[0035] According to some embodiments of the present application, the number of spherical particles in the lithium nickel manganese oxide positive electrode active material accounts for n, the roundness of the spherical particles is R, and satisfies: 0.75≤R≤1, 10%≤n≤40%. In other words, spherical particles refer to particles whose roundness R satisfies 0.75≤R≤1. By making the number of spherical particles within the above range, the risk of particles breaking and piercing aluminum foil during rolling is reduced, and the hardness of the lithium nickel manganese oxide particles is reduced, which is more conducive to breaking and reduces the cost of breaking.
[0036] In the present application, R can be tested by a scanning electron microscope (SEM). Specifically, the length of the longest diagonal of a single crystal particle in SEM is R1, the equivalent area circle diameter of a single crystal particle is R2, R=R1 / R2, and the closer R is to 1, the more rounded and regular the morphology of the spherical particle is.
[0037] As an example, R may be 0.75, 0.8, 0.85, 0.9, 0.95 or 1, or may be a range of any of the above values. Thus, the roundness of the round particles is improved, the risk of particles breaking and piercing the aluminum foil during rolling is reduced, the compaction density of the positive electrode sheet is increased, and the energy density of the battery is increased. According to some specific embodiments of the present application, 0.9≤R≤1.
[0038] As an example, n can be 10%, 15%, 20%, 25%, 30%, 35% or 40%, etc., or can be a range of any of the above values. According to some specific embodiments of the present application, 15%≤n≤25%. Thus, lithium nickel manganese oxide particles with both high powder compaction density and moderate hardness are obtained.
[0039] In the present application, the number ratio n of spherical particles can be tested by SEM. Specifically, n is the ratio of the number of spherical particles identified in the SEM photograph to the number of all particles.
[0040] It should be noted that when counting the number of spherical particles in the present application, what is counted is the sum of the spherical particles that exist alone and are not bonded to other particles, and the spherical particles that are bonded to other particles.
[0041] According to some embodiments of the present application, the lithium nickel manganese oxide positive electrode active material includes: Li (1+a) (Ni 0.5 Mn 1.5 ) (1-a-b-c) M b N c O4, wherein -0.3≤a≤0.3, 0<b≤0.002, 0≤c≤0.003, the M includes at least one of B, W, P, Nb, Mo, Ta, Si, Ce, and the N includes at least one of Y, Cr, and Co. Therefore, the doping element M has a fluxing effect, which can reduce the surface energy of the high-index crystal plane, form multiple high-index crystal planes on the surface of the lithium nickel manganese oxide particles, and make the particles polyhedral. After high temperature and long heat preservation, the crystal planes fuse to obtain spherical lithium nickel manganese oxide particles, thereby reducing the risk of lithium nickel manganese oxide particles breaking and piercing the aluminum foil during rolling. The NO bond energy formed between the N element and the O element is higher, which can reduce the Li +The surface energy of the dominant crystal planes (100) and (110) is used to achieve the effect of particle truncation. The top of the octahedron is truncated to expose the (100) crystal plane (corresponding to the (400) crystal plane in the XRD spectrum). The octahedron is cut from the edge to expose the (110) crystal plane (corresponding to the (310) crystal plane in the XRD spectrum), thus forming truncated octahedral particles. In addition, the doping element N occupies part of the trivalent manganese position, reducing the Mn 3+ The content of Mn 3+ Disproportionation reaction occurs to generate Mn 2+ Probability, Mn 2+ The reduction in content can further improve the cycle stability of lithium nickel manganese oxide.
[0042] As an example, a may be -0.3, -0.25, -0.15, -0.1, -0.05, 0.05, 0.1, 0.15, 0.2, 0.25 or 0.3, etc., or may be a range consisting of any of the above values.
[0043] As an example, b may be 0.0002, 0.0005, 0.001, 0.0015 or 0.002, etc., or may be a range consisting of any of the above values. According to some specific embodiments of the present application, 0.0003≤b≤0.001. Thus, by doping the lithium nickel manganese oxide with the above-mentioned content of the element M, the number of spherical particles in the lithium nickel manganese oxide is increased, and the risk of the lithium nickel manganese oxide particles breaking and piercing the aluminum foil during the rolling process is reduced.
[0044] As an example, c can be 0, 0.0003, 0.0005, 0.001, 0.002 or 0.003, etc., or can be a range composed of any of the above values. According to some specific embodiments of the present application, 0.0005≤c≤0.0015, c>b. Thus, by doping the above-mentioned content of N element in lithium nickel manganese oxide, truncated octahedral lithium nickel manganese oxide particles are formed to improve the cycle performance of the battery. By making c>b, N element doping can play a dominant role, which is beneficial to the specific capacity.
[0045] According to some embodiments of the present application, M includes at least one of B and Nb. Thus, in the process of forming lithium nickel manganese oxide, primary particle fusion is promoted and the surface energy of high-index crystal planes is reduced.
[0046] According to some embodiments of the present application, M includes a Y element.
[0047] According to some embodiments of the present application, the compaction density of the lithium nickel manganese oxide positive electrode active material can be 2.9 g / cm 3 -3.4g / cm 3 , for example, can be 2.9 g / cm 3 , 3g / cm3 、3.1g / cm 3 、3.2g / cm 3 , 3.3g / cm 3 or 3.4g / cm 3 etc., or can be a range composed of any of the above values. Thus, after the nickel manganese oxide positive electrode active material is coated on the positive electrode sheet, the compaction density of the positive electrode sheet can be increased, thereby increasing the energy density of the battery. According to some specific embodiments of the present application, the compaction density of the nickel manganese oxide positive electrode active material can be 3.1 g / cm 3 -3.3g / cm 3 .
[0048] In the present application, the compaction density of the lithium nickel manganese oxide positive electrode active material can be tested by a tap density tester of model BT-30 of Baxter.
[0049] The second aspect of the present application provides a method for preparing the lithium nickel manganese oxide positive electrode active material provided in the first aspect of the present application, the method comprising: mixing a nickel source, a manganese source, a lithium source, an M source, and an N source in a stoichiometric ratio to obtain a mixture; heating the mixture to a first temperature for sintering, then cooling the mixture to a second temperature for annealing, and cooling to obtain block lithium nickel manganese oxide; and crushing the block lithium nickel manganese oxide.
[0050] In the process of preparing lithium nickel manganese oxide, the present application, on the one hand, doped with M element and N element, the doped M element has a fluxing effect, in the process of forming lithium nickel manganese oxide, it can promote the fusion of primary particles, and in addition, it can effectively reduce the surface energy of high-index crystal planes, so as to form multiple high-index crystal planes on the surface of lithium nickel manganese oxide particles, so that the particles are polyhedral, after high temperature and long heat preservation, the crystal planes are fused to achieve a spherical effect; the doped N element is evenly distributed inside the lithium nickel manganese oxide crystal structure, and the NO bond energy formed between the N element and the O element is higher, which can reduce the Li + The surface energy of the dominant crystal planes (100) and (110) is used to achieve the effect of particle truncation. The top of the octahedron is truncated to expose the (100) crystal plane (corresponding to the (400) crystal plane in the XRD spectrum). The octahedron is cut from the edge to expose the (110) crystal plane (corresponding to the (310) crystal plane in the XRD spectrum), thus forming truncated octahedral particles. In addition, the doping element N occupies part of the trivalent manganese position, reducing the Mn 3+ The content of Mn 3+ Disproportionation reaction occurs to generate Mn 2+ Probability, Mn 2+The reduction of Mn content can further improve the cycle stability of lithium nickel manganese oxide. On the other hand, after the lithium nickel manganese oxide doped with M and N elements is formed, annealing is performed. The annealing process can repair the defects generated during the reaction of lithium nickel manganese oxide and regulate the Mn 3+ content, reducing the generation of oxygen vacancies and further improving the cycle performance.
[0051] The method proposed in this application is described in detail below. Figure 1 , the method comprising:
[0052] S10: Mixing a nickel source, a manganese source, a lithium source, an M source, and a N source according to a stoichiometric ratio to obtain a mixture.
[0053] According to some embodiments of the present application, the nickel source, the manganese source, the lithium source, the M source, and the N source are weighed in a stoichiometric ratio and placed in a high-speed mixer for mixing to obtain the mixture.
[0054] According to some embodiments of the present application, the nickel-manganese precursor, the lithium source, the M source, and the N source are mixed according to a stoichiometric ratio.
[0055] As an example, the M source includes a compound containing M. For example, when M is an element B, the M source may be boric acid. When M is an element Nb, the M source may be Nb2O5.
[0056] As an example, the N source includes a N-containing compound. For example, when N is an element Y, the N source may be yttrium oxide.
[0057] According to some embodiments of the present application, the volume average particle size Dv50 of the nickel manganese precursor satisfies: 3μm≤Dv50≤5μm, for example, it can be 3μm, 3.5μm, 4μm, 4.5μm or 5μm, or it can be a range composed of any of the above values. As a result, the particle size distribution of the nickel manganese precursor is narrow, which can improve the uniformity of the lithium nickel manganese oxide single crystal particles.
[0058] According to some embodiments of the present application, Dv10, Dv50 and Dv90 of the nickel-manganese precursor satisfy: 0.8≤(Dv90-Dv10) / Dv50≤1.2, wherein Dv10 is the particle size corresponding to when the volume distribution percentage of the nickel-manganese precursor particle size reaches 10%, and Dv90 is the particle size corresponding to when the volume distribution percentage of the nickel-manganese precursor particle size reaches 90%, for example, it can be 0.8, 0.9, 1.0, 1.1 or 1.2, etc., or it can be a range composed of any of the above values. As a result, the particle size distribution of the nickel-manganese precursor is narrow, which can improve the uniformity of the lithium nickel manganese oxide single crystal particles.
[0059] In the present application, Dv10, Dv50 and Dv90 of the nickel-manganese precursor can be obtained by testing with a laser particle size analyzer of the Hydro 3000mu model produced by Marvern.
[0060] S20: heating the mixture to a first temperature for sintering, cooling the mixture to a second temperature for annealing, and cooling the mixture to obtain blocky lithium nickel manganese oxide.
[0061] According to some embodiments of the present application, the mixture is heated so that the temperature of the mixture is raised from room temperature to a first temperature. After the mixture is kept at a constant temperature for a certain period of time, the mixture is naturally cooled to a second temperature for annealing. After the mixture is kept at a constant temperature for a certain period of time, the mixture is cooled to room temperature to obtain blocky lithium nickel manganese oxide.
[0062] According to some embodiments of the present application, the time from room temperature to the first temperature can be 2h-9h, for example, 2h, 4h, 6h, 8h or 9h, or can be a range composed of any of the above numerical values. According to some specific embodiments of the present application, the time from room temperature to the first temperature can be 2h-4h. Thus, the lithium source is fully melted to quickly complete the synthesis reaction of lithium nickel manganese oxide.
[0063] According to some embodiments of the present application, heating from room temperature to the first temperature may be performed in an air atmosphere or an oxygen atmosphere.
[0064] According to some embodiments of the present application, the temperature can be raised from room temperature to the first temperature in an oxygen atmosphere, thereby increasing the melting rate of the lithium source and the reaction rate of the nickel source, manganese source, lithium source, M source, and N source to form lithium nickel manganese oxide crystals.
[0065] According to some embodiments of the present application, the first temperature is T1 and satisfies 850°C≤T1≤1100°C. For example, it may be 850°C, 900°C, 950°C, 1000°C, 1050°C or 1100°C, etc., or may be a range consisting of any of the above numerical values.
[0066] According to some embodiments of the present application, the time for heating to the first temperature for constant temperature sintering may be t1, and satisfies: 6h≤t1≤12h, for example, 6h, 8h, 10h or 12h, etc., or may be a range consisting of any of the above values. According to some specific embodiments of the present application, 8h≤t1≤10h.
[0067] Therefore, by setting the temperature and holding time of constant temperature sintering within the above ranges, uniform and full single crystal large particles can be obtained.
[0068] According to some embodiments of the present application, the constant temperature sintering may be performed in an air atmosphere or an oxygen atmosphere.
[0069] According to some specific embodiments of the present application, the constant temperature sintering can be performed in an air atmosphere, thereby reducing the reaction cost.
[0070] According to some embodiments of the present application, the second temperature is T2 and satisfies: 250°C ≤ T1-T2 ≤ 500°C. For example, it can be 250°C, 300°C, 350°C, 400°C, 450°C or 500°C, or can be a range consisting of any of the above values.
[0071] According to some embodiments of the present application, the cooling rate from the first temperature to the second temperature is 1°C / min-4°C / min. For example, it can be 1°C / min, 1.5°C / min, 2°C / min, 2.5°C / min, 3°C / min, 3.5°C / min or 4°C / min, or can be a range of any of the above values. Thus, by making the cooling rate within the above range, while reducing Mn 3+ The content of nickel manganese oxide can be increased, the repair effect on the surface of the lithium nickel manganese oxide positive electrode active material can be improved, and the process cost can be reduced.
[0072] According to some embodiments of the present application, the time for cooling from the first temperature to the second temperature can be 1h-5h, for example, it can be 1h, 2h, 3h, 4h or 5h, etc., or it can be a range consisting of any of the above numerical values.
[0073] According to some embodiments of the present application, the cooling process can be performed in an air atmosphere or an oxygen atmosphere.
[0074] According to some specific embodiments of the present application, the cooling process can be performed in an air atmosphere, thereby reducing the reaction cost.
[0075] According to some embodiments of the present application, 600°C≤T2≤800°C, for example, it can be 600°C, 650°C, 700°C, 750°C or 800°C, etc., or can be a range consisting of any of the above numerical values.
[0076] According to some embodiments of the present application, the holding time of the mixture for annealing at the second temperature may be t2, and satisfies 2h≤t2≤6h, for example, 2h, 3h, 4h, 5h or 6h, etc., or may be a range consisting of any of the above values. According to some specific embodiments of the present application, 3.5h≤t2≤4h.
[0077] Therefore, by making the annealing temperature and the annealing holding time within the above range, the defects generated during the reaction of lithium nickel manganese oxide can be repaired and the Mn 3+ content, thereby reducing the generation of oxygen vacancies and further improving the battery's cycle performance.
[0078] According to some embodiments of the present application, the annealing process may be performed in an air atmosphere or an oxygen atmosphere.
[0079] According to some specific embodiments of the present application, the annealing process can be performed in an air atmosphere, thereby reducing the reaction cost.
[0080] S30: crushing the blocky lithium nickel manganese oxide.
[0081] According to some embodiments of the present application, the obtained bulk lithium nickel manganese oxide product is crushed and dissociated to obtain powdered spinel lithium manganese oxide.
[0082] In general, the lithium nickel manganese oxide positive electrode active material and the preparation method thereof proposed in this application have the following advantages:
[0083] (1) The lithium nickel manganese oxide positive electrode active material proposed in the present application is a mixed type of spherical particles and truncated octahedral particles. Compared with single-type particles, the mixed type particles as the positive electrode active material of the battery can reduce the risk of piercing the aluminum foil during the preparation process, increase the compaction density of the positive electrode sheet, and thus improve the energy density and safety of the battery.
[0084] (2) The present application can obtain single crystal particles with two mixed morphologies through one sintering. Compared with the method of separately preparing spherical particles and truncated octahedral particles and then mixing the two, the process is simpler and can significantly reduce production costs.
[0085] (3) The synthesis process of the present application utilizes an oxygen atmosphere during the heating stage, which can accelerate the melting rate of the lithium salt and quickly complete the synthesis reaction of lithium nickel manganese oxide. At the same time, the oxygen atmosphere can also make the reaction effect between Li and other raw materials more sufficient, thereby making it easier to obtain the spherical and octahedral truncation morphology effects.
[0086] (4) In the cooling stage and annealing stage of the synthesis process of the present application, the defects generated during the reaction of lithium nickel manganese oxide can be repaired by slow cooling and medium-temperature annealing, and the Mn 3+ content, reducing the generation of oxygen vacancies and further improving the cycle performance.
[0087] (5) The constant temperature sintering stage, the cooling stage and the constant temperature annealing stage of the synthesis process of the present application are all carried out in an air atmosphere, which can significantly reduce the production cost.
[0088] The third aspect of the present application provides a positive electrode sheet, wherein the positive electrode sheet comprises the lithium nickel manganese oxide positive electrode active material provided in the first aspect of the present application or the lithium nickel manganese oxide positive electrode active material prepared by the method provided in the second aspect of the present application. Thus, the compaction density of the positive electrode sheet can be increased while reducing the risk of the positive electrode active material puncturing the aluminum foil, thereby improving the energy density and safety of the battery.
[0089] The fourth aspect of the present application provides a battery, comprising the positive electrode sheet provided in the third aspect of the present application. Thus, the battery has a higher energy density and excellent cycle performance.
[0090] It should be noted that the shape of the battery in the present application is not particularly limited and can include at least one of a soft-pack battery, a cylindrical battery, a button battery and an aluminum shell square battery.
[0091] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.
[0092] Example 1
[0093] 1. According to the molar ratio of the elements, a nickel-manganese precursor (the mass ratio of Ni and Mn is 25:75), lithium carbonate, yttrium oxide and boric acid are weighed and added into a high-speed mixer for mixing to obtain a mixture, wherein the nickel-manganese precursor has a Dv10 of 3.17 μm, a Dv50 of 4.61 μm, and a Dv90 of 6.94 μm;
[0094] 2. Add the mixture into the Al2O3 sagger for heating, heat the mixture to a first temperature T1 of 970°C in an oxygen atmosphere for constant temperature sintering, the sintering atmosphere is oxygen, the sintering time t1 is 10h, then cool down in an air atmosphere at a cooling rate of 2°C / min, cool down to T2 of 500°C for annealing, the annealing time t2 is 4h, and then cool down to room temperature in an air atmosphere;
[0095] 3. Crushing the mixture to obtain Li(Ni 0.5 Mn 1.5 ) 0.998 B 0.0008 Y 0.0012 O4.
[0096] 4. Preparation of positive electrode
[0097] Will Li(Ni 0.5 Mn 1.5 ) 0.998 B 0.0008 Y 0.0012O4, conductive carbon black and polyvinylidene fluoride (PVDF) are mixed with an appropriate amount of N-methylpyrrolidone (NMP) in a mass ratio of 95%:2.5%:2.5% to form a slurry, which is coated on aluminum foil and placed in a vacuum drying oven at 120°C for 12 hours. After drying, it is stamped at a pressure of 100 MPa to form a positive electrode sheet with a diameter of 15.8 mm and a thickness of 3.2 mm. The surface density of the positive electrode sheet is 147.4 g / m 2 .
[0098] 5. Preparation of negative electrode sheet
[0099] A metal lithium sheet with a diameter of 15.8 mm and a thickness of 1 mm was used.
[0100] 6. Isolation film
[0101] A polypropylene microporous membrane (Celgard 2325) having a thickness of 25 μm was used.
[0102] 7. Preparation of Electrolyte
[0103] The electrolyte used was a mixture of 1 mol / L LiPF6, ethylene carbonate (EC), and diethyl carbonate (DEC) in equal amounts.
[0104] 8. Preparation of button cells
[0105] The assembly was carried out in a glove box with an argon atmosphere, where the water and oxygen content in the glove box was less than 5 ppm. The positive electrode sheet, the isolation membrane, the negative electrode sheet and the electrolyte were assembled into a CR2032 button cell and then left to stand for 6 hours.
[0106] The preparation methods of lithium nickel manganese oxide in Examples 2 to 17 and Comparative Example 1 are the same as those in Example 1, and the differences are detailed in Table 1.
[0107]
[0108]
[0109] Performance Testing
[0110] 1. Morphology test
[0111] The result was obtained by using a scanning electron microscope S4800 of Hitachi, Japan, wherein the roundness R was obtained by using a SEM image test.
[0112] 2. Compacted density of powder
[0113] The results were obtained by testing the tap density tester of Baxter Company, model BT-30.
[0114] 3. Discharge specific capacity
[0115] Shenzhen Xinwei Battery Testing System is used to test the electrochemical performance of CR2032 button batteries.
[0116] 3.5-4.95V, nominal specific capacity 120mAh / g, fully charge at 0.1C constant current and constant voltage, then fully discharge, and record the 0.1C first week discharge specific capacity C0.
[0117] 4. Capacity retention rate
[0118] Shenzhen Xinweier battery testing system was used to test the electrochemical performance of CR2032 button batteries. The button voltage window was 3.5-4.95V, the nominal specific capacity was 120mAh / g, and two cycles of full charge and full discharge were performed at 0.1C constant current and constant voltage. After two cycles of 0.1C, full charge and full discharge were performed at 1C constant current and constant voltage. The first cycle discharge specific capacity C1 was recorded, and the discharge specific capacity C was recorded after 100 cycles. 100 , the capacity retention rate is determined by C 100 / C1×100%, and the cycle performance was evaluated by the capacity retention rate.
[0119] 5.Mn 3+ Proportion
[0120] Shenzhen Xinweier Battery Testing System was used to test the electrochemical performance of CR2032 button batteries. The button voltage window was 3.5V-4.95V, the nominal specific capacity was 120mAh / g, and the battery was fully charged and fully discharged at 0.1C constant current and constant voltage. The first charge and discharge curve was drawn. According to the first charge and discharge curve, the discharge specific capacity Cm in the range of 3.5V-4.3V, the total discharge specific capacity Cn and Mn in the range of 3.5V-4.95V were recorded. 3+ Content = Cm / Cn×100%.
[0121] The performance test results of the lithium nickel manganese oxide materials and batteries in Examples 1 to 17 and Comparative Examples 1 to 3 are shown in Table 2.
[0122] Table 2
[0123]
[0124]
[0125] Conclusion: Compared with Example 1 to Example 17 and Comparative Example 1, it can be seen that the present invention h / I w The ratio of I to M in the above range can increase the number of spherical particles in the nickel manganese oxide positive electrode active material, improve the compaction density of the nickel manganese oxide positive electrode active material, and improve the discharge capacity and cycle capacity retention rate of the battery. h / I wThe ratio is within the above range, which can improve the energy density and cycle performance of the battery.
[0126] It can be seen from Examples 1 to 5 that by adjusting the temperature during the annealing process, the Mn 3+ Proportion, T2 = 700℃, Mn 3+ The proportion is the lowest, and the battery's discharge specific capacity and capacity retention rate are improved.
[0127] It can be seen from the comparison between Example 3 and Example 6 that the faster the cooling rate in the cooling stage, the higher the Mn 3+ As the proportion increases, the battery's discharge specific capacity and capacity retention rate decrease.
[0128] It can be seen from the comparison between Examples 7 and 9 that by adjusting the doping amount of the M element in the lithium nickel manganese oxide positive electrode active material, the I h / I w The ratio of , thereby increasing the compaction density of the nickel manganese oxide lithium positive electrode active material, and the discharge specific capacity and capacity retention rate of the battery are improved. However, when the doping amount of the M element is too high (Example 10), the condition b<c is not satisfied. Although the compaction density of the material is increased, the number of truncated octahedrons is reduced, and the discharge specific capacity and capacity retention rate of the battery are reduced.
[0129] It can be seen from the comparison between Example 3 and Example 11 that the type of doped M element can also satisfy I h / I w The ratio requirements and the proportion range of spherical particles make the battery's discharge specific capacity and capacity retention rate better.
[0130] It can be seen from the comparison between Example 12 and Example 3 that there is no N element doping, although I h / I w The ratio requirements and the proportion range of spherical particles are met, but the discharge specific capacity and capacity retention rate of the battery are reduced.
[0131] It can be seen from Examples 13-14 that increasing the N element doping amount increases the discharge capacity and capacity retention rate of the battery. However, because the b<c condition is not met, compared with Example 3, the discharge capacity and capacity retention rate of the battery are poor.
[0132] It can be seen from Example 15 compared with Example 3 that when the c content is too large, I h / I w The ratio of is reduced, the compaction density is reduced, the discharge specific capacity of the battery is poor, and the proportion of spherical particles is too small, which will reduce the capacity retention rate of the battery, but the capacity retention rate is still higher than that of the control example.
[0133] It can be seen from the comparison between Example 16 and Example 3 that the type of doped N element can also satisfy Ih / I w The ratio requirements and the proportion range of spherical particles make the battery's discharge specific capacity and capacity retention rate better.
[0134] It can be seen from the comparison between Example 17 and Example 3 that the spherical particles have a higher roundness and a higher proportion when sintered at a constant temperature in an oxygen atmosphere than when sintered at a constant temperature in an air atmosphere. h / I w The ratio is slightly better, and the battery's discharge specific capacity and capacity retention rate are better.
[0135] By the attached Figure 2 -Attached Figure 4 It can be seen that the lithium nickel manganese oxide positive electrode active material particles prepared in the embodiment of the present application are uniform, and include spherical particles and truncated octahedral particles.
[0136] By the attached Figure 5 It can be seen that the lithium nickel manganese oxide positive electrode active material prepared in Comparative Example 1 of the present application has no spherical particle morphology.
[0137] Attached Figure 6 In the XRD data of I h / I w The ratio is within the protection scope of this application.
[0138] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.
Claims
1. A lithium nickel manganese oxide positive electrode active material, characterized in that: The X-ray diffraction spectrum of the lithium nickel manganese oxide positive electrode active material satisfies: 0.13≤I h / I w ≤0.28, Among them, I w =I (111) +I (311) +I (400) , I h =I (331) +I (511) +I (531) , I (111) is the diffraction peak intensity of the crystal plane (111), I (311) is the diffraction peak intensity of the crystal plane (311), I (400) is the diffraction peak intensity of the crystal plane (400), I (331) is the diffraction peak intensity of the crystal plane (331), I (511) is the diffraction peak intensity of the crystal plane (511), I (531) is the diffraction peak intensity of the crystal plane (531).
2. The lithium nickel manganese oxide positive electrode active material according to claim 1, characterized in that: The number of spherical particles in the lithium nickel manganese oxide positive electrode active material accounts for n, the roundness of the spherical particles is R, and the following conditions are satisfied: 0.75≤R≤1, 10%≤n≤40%.
3. The lithium nickel manganese oxide positive electrode active material according to claim 2, characterized in that: Satisfy at least one of the following conditions: 0.9≤R≤1; 15%≤n≤25%。 4. The lithium nickel manganese oxide positive electrode active material according to any one of claims 1 to 3, characterized in that: include: Li (1+a) (Ni 0.5 Mn 1.5 ) (1-a-b-c) M b N c O4, wherein -0.3≤a≤0.3, 0<b≤0.002, 0≤c≤0.003, the M includes at least one of B, W, P, Nb, Mo, Ta, Si, and Ce, and the N includes at least one of Y, Cr, and Co.
5. The lithium nickel manganese oxide positive electrode active material according to claim 4, characterized in that: Satisfy at least one of the following conditions: The M includes at least one of B and Nb; The N includes Y.
6. The lithium nickel manganese oxide positive electrode active material according to claim 4, characterized in that: Satisfy at least one of the following conditions: 0.0003≤b≤0.001; 0.0005≤c≤0.0015, c>b.
7. The lithium nickel manganese oxide positive electrode active material according to any one of claims 1 to 3, characterized in that: The compaction density of the lithium nickel manganese oxide positive electrode active material is 2.9 g / cm 3 -3.4g / cm 3 , optional 3.1g / cm 3 -3.3g / cm 3 .
8. A method for preparing the lithium nickel manganese oxide positive electrode active material according to any one of claims 1 to 7, characterized in that: include: Mixing a nickel source, a manganese source, a lithium source, an M source, and a N source in a stoichiometric ratio to obtain a mixture; The mixture is heated to a first temperature for sintering, then cooled to a second temperature for annealing, and cooled to obtain bulk lithium nickel manganese oxide; The blocky lithium nickel manganese oxide is crushed.
9. The method according to claim 8, characterized in that The method further includes: mixing the nickel-manganese precursor, the lithium source, the M source, and the N source according to a stoichiometric ratio.
10. The method according to claim 9, characterized in that The first temperature is T1, the second temperature is T2, and 250°C≤T1-T2≤500°C is satisfied.
11. The method according to claim 10, characterized in that Satisfy at least one of the following conditions: 850℃≤T1≤1100℃; 600℃≤T2≤800℃。 12. The method according to claim 8, characterized in that The cooling rate from the first temperature to the second temperature is 1°C / min-4°C / min.
13. The method according to claim 12, characterized in that The mixture is heated to the first temperature for a holding time of t1, the mixture is cooled to the second temperature for a holding time of t2, and at least one of the following conditions is met: 6h≤t1≤12h, optionally, 8h≤t1≤10h; 2h≤t2≤6h, optionally, 3.5h≤t2≤4h.
14. The method according to claim 8, characterized in that The sintering and the annealing are independently performed in air or oxygen atmosphere.
15. The method according to claim 14, characterized in that The sintering is performed in an oxygen atmosphere.
16. The method according to claim 9, characterized in that The nickel-manganese precursor satisfies at least one of the following conditions: 3μm≤Dv50≤5μm, wherein Dv50 is the volume average particle size of the nickel-manganese precursor particles; 0.8≤(Dv90-Dv10) / Dv50≤1.2, wherein Dv10 is the particle size corresponding to when the volume distribution percentage of the nickel manganese precursor particle size reaches 10%, and Dv90 is the particle size corresponding to when the volume distribution percentage of the nickel manganese precursor particle size reaches 90%.
17. A positive electrode plate, characterized in that: The invention comprises the lithium nickel manganese oxide positive electrode active material as described in any one of claims 1 to 7.
18. A battery, characterized in that: Including the positive electrode sheet as described in claim 17.
Citation Information
Cited By
Method for synthesizing lithium nickel manganese oxide positive electrode material through rapid Joule thermal shock
CN119349660A
Positive electrode active material and preparation method thereof, positive electrode plate, lithium secondary battery and electric equipment
CN120878836A
Positive electrode active material, method for manufacturing same, positive electrode sheet, lithium secondary battery, and electric device
CN120878836B
Lithium ion secondary battery, battery device, and power device
CN121964766A
Lithium-ion secondary batteries, battery devices and electrical appliances
CN121964766B