Secondary battery and electric device

By using the combination of organic lithium salt and inorganic lithium salt in secondary batteries, as well as the grading of multi-particle-size positive electrode active materials, the problem of insufficient kinetic performance and rate performance is solved, and high energy density and excellent kinetic performance are achieved synchronous improvement.

CN119096387APending Publication Date: 2024-12-06CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202480001335.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-04-18
Filing Date
2024-06-18
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing high-energy density secondary batteries have shortcomings in terms of kinetic performance and rate performance, and it is difficult to take into account both excellent results.

Method used

By using a reasonable ratio of organolithium salt and inorganolithium salt in the electrolyte, and using multi-particle size positive electrode active materials and particle grading with high nickel element content in the positive electrode film layer, the electrode structure and electrolyte interface of the battery are optimized. Improve the transmission rate and interface stability of lithium ions.

Benefits of technology

The energy density and dynamic performance of secondary batteries are synchronized, and the overall performance of the battery is improved, including higher energy density and excellent rate performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119096387A_ABST
    Figure CN119096387A_ABST
Patent Text Reader

Abstract

A secondary battery is provided. The secondary battery comprises an electrolyte and a positive electrode, wherein the electrolyte contains an organic lithium salt; the positive electrode comprises a positive electrode film layer, and the energy density per unit area of the positive electrode film layer on one side is 18-37 mWh / cm < 2 >, and can be 18-35.7 mWh / cm < 2 > optionally. The synchronous improvement of the energy density and the dynamic performance of the battery is realized through the mutual cooperation of the electrolyte and the positive electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Cross-references

[0001] This application refers to the PCT patent application entitled “Secondary Batteries and Electrical Devices” filed on April 18, 2023 with patent application number PCT / CN2023 / 089061, which is incorporated herein by reference in its entirety. Technical Field

[0002] The present application relates to the technical field of secondary batteries, and in particular to a secondary battery with high energy density and an electrical device. Background Art

[0003] Secondary batteries are widely used in electric vehicles, energy storage systems, and mobile electronic devices due to their high energy density, long life, and low self-discharge rate. As secondary batteries have made great progress, higher requirements are placed on the performance of secondary batteries.

[0004] High energy density secondary batteries often have problems such as poor kinetic performance and poor rate performance. How to obtain secondary batteries with excellent comprehensive performance including energy level and kinetic performance is a technical problem that needs to be solved urgently in this field. Summary of the invention

[0005] The present application has been made in view of the above-mentioned problems, and an object of the present application is to provide a secondary battery having both high energy density and dynamic performance.

[0006] In a first aspect of the present application, a secondary battery is provided, wherein the secondary battery comprises an electrolyte and a positive electrode, wherein the electrolyte comprises an organic lithium salt; the positive electrode comprises a positive electrode film layer, and the energy density per unit area of ​​the positive electrode film layer on one side is 18 to 37 mWh / cm 2 , can be selected as 18~35.7mWh / cm 2 .

[0007] Organic lithium salts in the electrolyte can effectively improve the electrolyte's ion conductivity, reduce the impedance of the electrolyte / electrode interface, form a stable passivation film with good ion conductivity on the electrode surface, and improve interface stability. Organic lithium salts in the electrolyte can increase the transmission rate of lithium ions in the positive electrode film layer, optimize the battery's kinetic performance and rate performance, and achieve a simultaneous improvement in the energy density and kinetic performance of secondary batteries.

[0008] In any embodiment, the positive electrode film layer and the organic lithium salt satisfy the following relationship: 0.005≤M-0.0005×w≤0.2, wherein M is the mass content of the organic lithium salt based on the total mass of the electrolyte; w is the surface density of the positive electrode film layer on one side, in mg / cm 2 .

[0009] In order to increase the energy density of the battery, it is usually necessary to increase the surface density of the positive electrode film layer. However, a pole piece with a large surface density is not conducive to the transmission of ions in the positive electrode film layer, resulting in reduced battery kinetic performance and rate performance. The present application achieves simultaneous optimization of battery energy density and rate performance by matching the positive electrode film layer with an organic lithium salt. When the positive electrode film layer and the organic lithium salt satisfy the above relationship, the high energy density positive electrode piece and the organic lithium salt form an effective match to achieve a simultaneous improvement in battery energy density and kinetic performance.

[0010] In any embodiment, the surface density w of the positive electrode film layer on one side is not less than 20 mg / cm 2 , optionally 25 to 45 mg / cm 2 .

[0011] Controlling the surface density of the single-sided positive electrode film layer within an appropriate range can ensure that the battery has both high energy density and rate performance.

[0012] In any embodiment, the organic lithium salt comprises at least one of lithium bis(fluorosulfonyl)imide and lithium bis(trifluoromethylsulfonyl)imide.

[0013] The above-mentioned organic lithium salt has high ionic conductivity and stable electrochemical properties, which can increase the transmission rate of lithium salt in the positive electrode film layer, reduce electrode polarization, and improve the kinetic performance of the battery.

[0014] In any embodiment, the electrolyte further includes an inorganic lithium salt, and the molar ratio of the organic lithium salt to the inorganic lithium salt is 1:5 to 5:1.

[0015] Compared with organic lithium salts, inorganic lithium salts have low cost and high withstand voltage. As an example, inorganic lithium salts include but are not limited to lithium hexafluorophosphate, lithium tetrafluoroborate, lithium hexafluoroarsenate, and lithium perchlorate. When the ratio of inorganic lithium salt to organic lithium salt is within a suitable range, the battery cost can be reduced while effectively improving the battery rate performance.

[0016] In any embodiment, the positive electrode film layer contains positive electrode active materials, and the positive electrode active materials include particles A and particles B. The particles A are polycrystalline particles, and the volume average particle size of the particles A is larger than the volume average particle size of the particles B.

[0017] The positive electrode active material of the present application includes two particles of different particle sizes. Through the grading of large-size particles A and small-size particles B, the pores between the particles can be effectively filled, the compaction density of the pole piece can be increased, and thus the unit volume energy density of the battery can be increased. During the battery cycle, cracks are prone to appear between the grains of polycrystalline particles A, which is conducive to the diffusion of lithium ions and helps to improve the battery rate performance; at the same time, the grading of large-size particles A and small-size particles B can also reduce the electrolyte consumption and increase in pore resistance caused by excessive pores between the particles of the pole piece, thereby improving the battery rate performance.

[0018] In any embodiment, the positive electrode film layer also satisfies at least one of the following characteristics: (1) The particle B is a polycrystalline, single crystal or quasi-single crystal particle; (2) The primary particle size of the particle A is 50 nm to 400 nm, and may be 80 to 200 nm; the primary particle size of the particle B is 150 nm to 2 μm, and may be 200 nm to 1.2 μm; (3) The volume average particle size of the particles A is 2 to 25 μm, and may be 2.5 to 23 μm; the volume average particle size of the particles B is 0.65 to 10 μm, and may be 1.2 to 8.5 μm; (4) The mass ratio of the particles A to the particles B is 5:5 to 9:1; (5) The laser particle size distribution curve of the positive electrode active material is bimodal, and the peak position difference between the two peaks is 3 to 7 μm; (6) The positive electrode includes a positive electrode current collector, and the ratio of the thickness of the positive electrode film layer on one side to the thickness of the positive electrode current collector is 5.5 to 15, and optionally 5.6 to 8.8.

[0019] When the positive electrode film layer satisfies at least one of the above conditions, the battery has high energy density and excellent kinetic performance.

[0020] In any embodiment, based on the total molar number of transition metal elements in the positive electrode active material, the molar content of nickel element is not less than 80%; alternatively, not less than 85%; further alternatively, not less than 90%.

[0021] Due to the high relative content of nickel, the gram capacity of the positive electrode active material is correspondingly high, which can effectively improve the energy density of the battery.

[0022] In any embodiment, the compositions of the particles A and B independently satisfy Formula I, Li a1 Ni x1 Co y1 Mn z1 M1 b1 O2M1'c1 , Formula I Among them, a1 is 0.8-1.2, x1 is 0.85-1, y1 is 0-0.15, z1 is 0-0.15, b1 is 0-0.02, c1=1-x1-y1-z1-b1, M1 includes at least one of Zr, Y, Al, Ti, W, Sr, Ta, Sb, Nb, Na, K, B, Mg, Zn, Ca or Ce, and M1' includes at least one of N, F, S or Cl.

[0023] The nickel content in the composition of particles A and B is relatively high, which can improve the energy density of the battery. In addition, the doping of M1 elements in particles A and B can reduce the lithium-nickel mixing of active materials during the cycle process, improve the structural stability of the material, and ensure that after lithium ions are deintercalated from the positive electrode during the charging process, the positive electrode active material can still maintain a relatively complete structure, thereby improving the discharge performance of the battery.

[0024] In any embodiment, the positive electrode film layer contains a positive electrode active material, and the positive electrode active material is a single crystal or a quasi-single crystal particle, and satisfies at least one of the following characteristics: (1) The laser particle size distribution curve of the positive electrode active material is single-peaked; (2) The volume average particle size D of the single crystal or quasi-single crystal particles v 50 is 1 to 3.5 μm, optionally 1.2 to 3.0 μm; (3) The laser particle size distribution of the single crystal or quasi-single crystal particles satisfies: 0.3≤(D v 99-D v 90) / (2×D v 50)≤0.55; (4) The composition of the single crystal or quasi-single crystal particles is as shown in Formula II: Li a2 Ni x2 Co y2 Mn z2 M2 b2 O2M2' c2 , Formula II Wherein, a2 is 0.8-1.2, x2 is 0.85-1, y2 is 0-0.15, z2 is 0-0.15, b2 is 0-0.02, c2=1-x2-y2-z2-b2, M2 includes at least one of Zr, Y, Al, Ti, W, Sr, Ta, Sb, Nb, Na, K, B, Mg, Zn, Ca or Ce, and M2' includes at least one of N, F, S or Cl; optionally, x2 is 0.90-1; (5) The positive electrode includes a positive electrode current collector, and the ratio of the thickness of the positive electrode film layer on one side to the thickness of the positive electrode current collector is 4.5 to 9, and optionally 4.5 to 8.5.

[0025] The positive electrode material formed by single crystal particles has a large surface area and a relatively dense structure, so that the positive electrode active material can maintain good structural stability while having a high compaction density, thereby reducing side reactions during charging and discharging, slowing down the consumption of electrolyte, and improving the battery life. The positive electrode active material that meets the above conditions has good structural stability, so that the battery including the positive electrode active material can have high energy density and excellent rate performance.

[0026] In any embodiment, the pore volume of the positive electrode film layer accounts for 18% to 35% of the total volume of the positive electrode film layer.

[0027] When the pore volume of the positive electrode film layer is within an appropriate range, the organic lithium salt in the electrolyte can easily enter the pores of the positive electrode film layer and fully contact the positive electrode active material, thereby increasing the migration rate of ions at the electrode / electrolyte interface, reducing the internal resistance of the battery, and improving the battery's cycle performance and rate performance.

[0028] In any embodiment, the secondary battery further comprises a negative electrode, the negative electrode comprises a negative electrode membrane, the negative electrode membrane comprises a negative electrode active material, the negative electrode active material comprises a silicon-based material, and the silicon-based material is selected from one or more of elemental silicon, silicon-oxygen material, and silicon-carbon material. The silicon-based material can significantly increase the energy density of the battery.

[0029] In any embodiment, the negative electrode active material further comprises a carbon-based material, and the mass ratio of the carbon-based material to the silicon-based material is no more than 4:6, and can be optionally no more than 2:8.

[0030] When the mass ratio of carbon-based materials to silicon-based materials is within the above range, the battery can have a high energy density while reducing the expansion of the negative electrode and improving the cycle performance and rate performance.

[0031] In any embodiment, the surface density of the negative electrode film is 6 to 13 mg / cm 2 .

[0032] When the surface density of the negative electrode film is within the above range, the negative electrode adopts a thick coating design, which helps to improve the energy density of the battery. The second aspect of the present application provides an electrical device, including the secondary battery of the first aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 is a schematic diagram of a secondary battery cell according to an embodiment of the present application;

[0034] Figure 2 yes Figure 1 An exploded view of a secondary battery cell according to an embodiment of the present application is shown;

[0035] Figure 3 FIG. 1 is a schematic diagram of an electric device using a secondary battery according to an embodiment of the present application as a power source.

[0036] Description of reference numerals: 5 secondary battery; 51 housing; 52 electrode assembly; 53 cover plate. DETAILED DESCRIPTION

[0037] Below, the embodiments of the current collector, secondary battery, battery module, battery pack and power device of the present application are specifically disclosed with appropriate reference to the accompanying drawings. However, there are cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0038] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0039] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0040] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0041] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0042] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0043] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0044] With the widespread application of secondary batteries, the requirements for secondary battery performance, such as energy density, are gradually increasing. In order to improve the energy density of the battery, a thick coating design of active materials is often adopted. However, the thick coating of active materials causes the migration path of lithium ions in the membrane layer to become longer, and the resistance to migration becomes larger, so the polarization resistance of the pole piece increases and the dynamic performance of the battery decreases. Therefore, it is urgent to develop a secondary battery with excellent dynamic performance while improving energy density.

[0045] Based on this, the present application proposes a secondary battery, which achieves a simultaneous improvement in battery energy density and dynamic performance through the cooperation between the electrolyte and the positive electrode.

[0046] In some embodiments, the secondary battery includes an electrolyte and a positive electrode, wherein the electrolyte includes an organic lithium salt; the positive electrode includes a positive electrode film layer, and the energy density per unit area of ​​the single-side positive electrode film layer is 18 to 37 mWh / cm 2 , can be selected as 18~35.7mWh / cm 2 .

[0047] Organic lithium salts can generally be regarded as inorganic lithium salts by introducing one or more electron-withdrawing groups, which are formed by adjusting and controlling the structure of anions. The anions of organic lithium salts generally have a larger radius, a more dispersed charge distribution, and a strong ionization passivation effect, which can reduce the lattice energy of lithium salts, weaken the interaction between positive and negative ions, and increase the solubility of lithium salts. Organic lithium salts include but are not limited to lithium bis(fluorosulfonyl)imide and lithium bis(trifluoromethylsulfonyl)imide.

[0048] In some embodiments, the positive electrode film layer is located on both sides of the current collector. In some embodiments, the positive electrode film layer is located on either side of the current collector. It can be understood that the single-sided positive electrode film layer here refers to the positive electrode film layer on either side of the positive electrode sheet.

[0049] The unit area energy density of the single-sided positive electrode film layer can be measured using methods and equipment commonly used in the art. As an example, the unit area energy density of the positive electrode film layer can be operated according to the following steps: let the battery cell stand at a certain temperature (e.g., 25°C) for a certain time (e.g., 2h), and ensure that the temperature of the battery cell is room temperature (e.g., 25°C). After charging the battery cell to the charging cut-off voltage at a certain rate (e.g., 0.33C) at a certain temperature (e.g., 25°C), continue to charge at a constant voltage at the charging cut-off voltage until the current is 0.05C and the charging is cut off (C represents the rated capacity of the battery cell). After the battery cell is allowed to stand at a certain temperature (e.g., 25°C) for a certain time (e.g., 1h), the battery cell is discharged to the discharge cut-off voltage at a certain rate (0.33C) at a certain temperature (e.g., 25°C), and the total discharge energy is recorded as E0. Disassemble the battery, take out the positive electrode sheet, and use a ruler to measure the length and width of the positive electrode film layer to obtain the area value S0 of the positive electrode film layer. If the positive electrode film layer is coated on both sides, the energy per unit area of ​​the positive electrode film layer = E0 / (2×SS0). If the positive electrode film layer is coated on one side, the energy per unit area of ​​the positive electrode film layer = E0 / S0.

[0050] In the above test method, the charge cut-off voltage of the battery cell is 4.25V, the discharge cut-off voltage is 2.0V, and the charge rate and discharge rate are both 0.33C.

[0051] In some embodiments, the energy density per unit area of ​​the positive electrode film layer on one side is 18 mWh / cm 2 、19.3mWh / cm 2 、20mWh / cm 2 、21mWh / cm 2 、22mWh / cm 2 、23mWh / cm 2 、24mWh / cm 2 、25mWh / cm 2 、26mWh / cm 2、27mWh / cm 2 、28mWh / cm 2 、29mWh / cm 2 、30mWh / cm 2 、31mWh / cm 2 、32mWh / cm 2 、33mWh / cm、34mWh / cm 2 、35mWh / cm 2 、35.7mWh / cm 2 、36mWh / cm 2 、37mWh / cm 2 Or a value in the range formed by any two of the above points.

[0052] Organic lithium salts in the electrolyte can effectively improve the electrolyte's ion conductivity, reduce the impedance of the electrolyte / electrode interface, form a stable passivation film with good ion conductivity on the electrode surface, and improve interface stability. Organic lithium salts in the electrolyte can increase the transmission rate of lithium ions in the positive electrode film layer, optimize the battery's kinetic performance and rate performance, and achieve a simultaneous improvement in the energy density and kinetic performance of secondary batteries.

[0053] In some embodiments, the positive electrode film layer and the organic lithium salt satisfy the following relationship: 0.005≤M-0.0005×w≤0.2, wherein M is the mass content of the organic lithium salt based on the total mass of the electrolyte; w is the surface density of the single-sided positive electrode film layer, in mg / cm 2 .

[0054] In order to increase the energy density of the battery, it is usually necessary to increase the surface density of the positive electrode film layer. However, a pole piece with a large surface density is not conducive to the transmission of ions in the positive electrode film layer, resulting in reduced battery kinetic performance and rate performance. The present application achieves simultaneous optimization of battery energy density and rate performance by matching the positive electrode film layer with an organic lithium salt. When the positive electrode film layer and the organic lithium salt satisfy the above relationship, the high energy density positive electrode piece and the organic lithium salt form an effective match to achieve a simultaneous improvement in battery energy density and kinetic performance.

[0055] In some embodiments, the thickness of the single-sided positive electrode film layer is 70 μm to 160 μm, optionally 80 μm to 140 μm, 90 μm to 130 μm, or 100 μm to 120 μm. Controlling the thickness of the single-sided positive electrode film layer within a suitable range can ensure that the battery has both high energy density and good rate performance.

[0056] In some embodiments, the surface density w of the single-sided positive electrode film layer is not less than 20 mg / cm 2 , optionally 25 to 45 mg / cm 2 .

[0057] In some embodiments, the surface density w of the single-sided positive electrode film layer can be selected to be 20 mg / cm 2 , 25mg / cm 2 、30mg / cm 2 、35mg / cm 2 , 40mg / cm 2 or 45 mg / cm 2 Controlling the surface density of the single-sided positive electrode film layer within an appropriate range can ensure that the battery has both high energy density and rate performance.

[0058] In some embodiments, the organic lithium salt includes at least one of lithium bis(fluorosulfonyl)imide (LiFSI) and lithium bis(trifluoromethylsulfonyl)imide (LiTFSI).

[0059] The above-mentioned organic lithium salt has high ionic conductivity and stable electrochemical properties, which can increase the transmission rate of lithium salt in the positive electrode film layer, reduce electrode polarization, and improve the kinetic performance of the battery.

[0060] In some embodiments, the electrolyte further includes an inorganic lithium salt, and the molar ratio of the organic lithium salt to the inorganic lithium salt is 1:5 to 5:1.

[0061] Compared with organic lithium salts, inorganic lithium salts have low cost and high withstand voltage. As an example, inorganic lithium salts include but are not limited to lithium hexafluorophosphate, lithium tetrafluoroborate, lithium hexafluoroarsenate, and lithium perchlorate. When the ratio of inorganic lithium salt to organic lithium salt is within a suitable range, the battery cost can be reduced while effectively improving the battery rate performance.

[0062] In some embodiments, the positive electrode film layer contains a positive electrode active material, the positive electrode active material includes particles A and particles B, particles A are polycrystalline particles, and the volume average particle size of particles A is greater than the volume average particle size of particles B.

[0063] Herein, the "volume average particle size" is also referred to as Dv50, and refers to the particle size corresponding to when the cumulative volume of particles reaches 50% in particle size distribution measurement performed by a laser scattering method.

[0064] The volume average particle size can be tested using equipment and methods known in the art. For example, the particle size distribution test is performed using a Microtrac MRB S3500 series laser particle size analyzer. The specific test process is as follows: 0.05-2 g of positive electrode active material is added with 10-20 ml of deionized water, and ultrasonicated at 53 KHz frequency and 120 W power for 5 minutes to ensure that the sample is completely dispersed, and then the sample is measured according to GB / T19077-2016 or ISO 13320:2009 standards. The Dv50 of the particles is measured by the particle size volume distribution curve.

[0065] In this article, "polycrystalline" refers to a crystal composed of many single crystal particles with different orientations. The entire structure is not penetrated by the same lattice. The structure of each small crystal is the same and anisotropic.

[0066] The positive electrode active material of the present application includes two particles of different particle sizes. Through the grading of large-size particles A and small-size particles B, the pores between the particles can be effectively filled, the compaction density of the pole piece can be increased, and thus the unit volume energy density of the battery can be increased. During the battery cycle, cracks are prone to appear between the grains of polycrystalline particles A, which is conducive to the diffusion of lithium ions and helps to improve the battery rate performance; at the same time, the grading of large-size particles A and small-size particles B can also reduce the electrolyte consumption and increase in pore resistance caused by excessive pores between the particles of the pole piece, thereby improving the battery rate performance.

[0067] In some embodiments, the particles B are polycrystalline, single crystal, or quasi-single crystal particles.

[0068] In this article, "single crystal" refers to a crystal that has grown perfectly and has an internal structure that conforms to a lattice structure. A single crystal has no grain boundaries on a macroscopic scale and the crystal orientation is consistent throughout the crystal.

[0069] In this article, "quasi-single crystal" refers to a crystal with a small number of grains and a large grain size.

[0070] Particle B is polycrystalline, which can further improve the rate performance of the battery. Particle B is single crystal or quasi-single crystal, which helps to improve the structural stability of the positive electrode active material during the cycle process.

[0071] In some embodiments, the primary particle size of particle A is 50 nm to 400 nm, and may be 80 to 200 nm; the primary particle size of particle B is 150 nm to 2 μm, and may be 200 nm to 1.2 μm.

[0072] In some embodiments, the primary particle size of particle A is any one of 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 110nm, 120nm, 130nm, 140nm, 150nm, 160nm, 170nm, 180nm, 190nm, 200nm, 250nm, 300nm, 350nm, 400nm or any value therebetween.

[0073] In some embodiments, the primary particle size of particle B is 150nm, 200nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm, 1μm, 1.1μm, 1.2μm, 1.3μm, 1.4μm, 1.5μm, 1.6μm, 1.7μm, 1.8μm, 1.9μm, 2μm, or any value in between. In this article, "primary particle size" refers to the particle size of a primary particle.

[0074] In this article, "primary particles" refer to solid basic particles obtained by dispersion or refinement without changing the essential structure of the substance. Primary particles are particles that have not formed an agglomerate state.

[0075] In some embodiments, the volume average particle size of particles A is 2 to 25 μm, and may be 2.5 to 23 μm; the volume average particle size of particles B is 0.65 to 10 μm, and may be 1.2 to 8.5 μm.

[0076] In some embodiments, the volume average particle size of particles A is 2μm, 2.5μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm, 19μm, 20μm, 21μm, 22μm, 23μm, 24μm, 25μm, or any value therebetween.

[0077] In some embodiments, the volume average particle size of particle B is any one of 0.65 μm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 8.5 μm, 9 μm, 10 μm or any value therebetween. It is understood that the volume average particle size can be either a primary particle size or a secondary particle size. In some embodiments, for single crystal materials, the volume average particle size is a primary particle size. In some embodiments, for polycrystalline materials, the volume average particle size is the particle size of the secondary particles after the primary particles are agglomerated.

[0078] The volume average particle size of polycrystalline particles A is larger than that of polycrystalline particles B. The migration path of lithium ions in particles A is long, while its primary particle size is small, which can promote the rapid migration of lithium ions and balance the kinetic performance.

[0079] In some embodiments, the mass ratio of particle A to particle B is 5:5 to 9:1. In some embodiments, the laser particle size distribution curve of the positive electrode active material is bimodal, and the peak position difference between the two peaks is 3 to 7 μm.

[0080] In some embodiments, the mass ratio of particles A to particles B is any one of 1, 2, 3, 4, 5, 6, 7, 8, 9 or any value therebetween.

[0081] In some embodiments, the laser particle size distribution curve of the positive electrode active material is bimodal, and the peak position difference between the two peaks is any one of 3μm, 4μm, 5μm, 6μm, 7μm or any value therebetween. By matching the mass and / or particle size of large and small particles, the compaction density of the pole piece can be further increased, and the volume energy density of the battery can be improved.

[0082] In some embodiments, the positive electrode includes a positive electrode collector, the positive electrode film layer contains positive electrode active materials, the positive electrode active materials include particles A and particles B, and the ratio of the thickness of the single-sided positive electrode film layer to the thickness of the positive electrode collector is 5.5 to 15, and optionally 5.6 to 8.8.

[0083] When the ratio of the thickness of the single-sided positive electrode film layer to the thickness of the positive electrode current collector is within this range, the energy density per unit area of ​​the positive electrode film layer can be improved.

[0084] When the positive electrode film layer meets the above conditions, the positive electrode plate can achieve an increase in the compaction density of the plate through mutual matching between the positive electrode active materials, so that the battery including the positive electrode active material can have both high energy density and excellent rate performance.

[0085] In some embodiments, based on the total molar number of transition metal elements in the positive electrode active material, the molar content of nickel element is not less than 80%; alternatively, not less than 85%; further alternatively, not less than 90%.

[0086] In some embodiments, the molar content of nickel element can be selected to be 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99% or 100% based on the total molar number of transition metal elements in the positive electrode active material.

[0087] Due to the high relative content of nickel, the gram capacity of the positive electrode active material is correspondingly high, which can effectively improve the energy density of the battery.

[0088] In some embodiments, the compositions of particle A and particle B independently satisfy Formula I, Li a1 Ni x1 Co y1 Mn z1 M1 b1 O2M1' c1 , Formula I Among them, a1 is 0.8-1.2, x1 is 0.85-1, y1 is 0-0.15, z1 is 0-0.15, b1 is 0-0.02, c1=1-x1-y1-z1-b1, M1 includes at least one of Zr, Y, Al, Ti, W, Sr, Ta, Sb, Nb, Na, K, B, Mg, Zn, Ca or Ce, and M1' includes at least one of N, F, S or Cl.

[0089] In some embodiments, a1 can be selected as 0.8, 0.9, 1.0, 1.1, 1.2 or any value therein.

[0090] In some embodiments, b1 can be selected as 0, 0.01, 0.02 or any value therein.

[0091] In some embodiments, x1 can be selected as 0.85, 0.9, 0.95, 1 or any value therein. In some embodiments, y1 can be selected as 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.11, 0.12, 0.13, 0.14, 0.15 or any value therein.

[0092] In some embodiments, z1 can be selected as 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.11, 0.12, 0.13, 0.14, 0.15 or any value therein.

[0093] In some embodiments, Particle A and Particle B have the same composition.

[0094] In some embodiments, Particle A and Particle B have different compositions.

[0095] The nickel content in the composition of particles A and B is relatively high, which can improve the energy density of the battery. In addition, the doping of M1 elements in particles A and B can reduce the lithium-nickel mixing of active materials during the cycle process, improve the structural stability of the material, and ensure that after lithium ions are deintercalated from the positive electrode during the charging process, the positive electrode active material can still maintain a relatively complete structure, thereby improving the discharge performance of the battery.

[0096] In some embodiments, the positive electrode film layer contains a positive electrode active material, the positive electrode active material is a single crystal or quasi-single crystal particle, and the laser particle size distribution curve of the positive electrode active material is a single peak.

[0097] In some embodiments, the positive electrode film layer contains a positive electrode active material, the positive electrode active material is a single crystal or a quasi-single crystal particle, and the volume average particle size D of the single crystal or the quasi-single crystal particle is v50 is 1 to 3.5 μm, optionally 1.2 to 3.0 μm.

[0098] In some embodiments, the positive electrode film layer contains a positive electrode active material, the positive electrode active material is a single crystal or a quasi-single crystal particle, and the volume average particle size D of the single crystal or the quasi-single crystal particle is v 50 is 1 μm, 1.2 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm or any value therein.

[0099] In some embodiments, the positive electrode film layer contains a positive electrode active material, the positive electrode active material is a single crystal or a quasi-single crystal particle, and the laser particle size distribution of the single crystal or the quasi-single crystal particle satisfies: 0.3≤(D v 99-D v 90) / (2×D v 50)≤0.55.

[0100] In some embodiments, the positive electrode film layer contains a positive electrode active material, the positive electrode active material is a single crystal or a quasi-single crystal particle, and the laser particle size distribution (D v 99-D v 90) / (2×D v 50) is 0.3, 0.35, 0.4, 0.45, 0.5, 0.55 or any value therein.

[0101] In some embodiments, the positive electrode film layer contains a positive electrode active material, and the positive electrode active material is a single crystal or a quasi-single crystal particle, and the composition of the single crystal or the quasi-single crystal particle is as shown in Formula II: Li a2 Ni x2 Co y2 Mn z2 M2 b2 O2M2' c2 , Formula II Among them, a2 is 0.8~1.2, x2 is 0.85~1, y2 is 0~0.15, z2 is 0~0.15, b2 is 0~0.02, c2=1-x2-y2-z2-b2, M2 includes at least one of Zr, Y, Al, Ti, W, Sr, Ta, Sb, Nb, Na, K, B, Mg, Zn, Ca or Ce, and M2' includes at least one of N, F, S or Cl; optionally, x2 is 0.90~1.

[0102] In some embodiments, a2 can be selected as 0.8, 0.9, 1.0, 1.1, 1.2 or any value therein.

[0103] In some embodiments, b2 can be selected as 0, 0.01, 0.02 or any value therein.

[0104] In some embodiments, x2 can be selected as 0.85, 0.9, 0.95, 1 or any value therein. In some embodiments, y2 can be selected as 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.11, 0.12, 0.13, 0.14, 0.15 or any value therein.

[0105] In some embodiments, z2 can be selected as 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.11, 0.12, 0.13, 0.14, 0.15 or any value thereof. In some embodiments, the positive electrode includes a positive electrode current collector, the positive electrode film layer includes a positive electrode active material, the positive electrode active material is a single crystal or a quasi-single crystal particle, and the ratio of the thickness of the single-sided positive electrode film layer to the thickness of the positive electrode current collector is 4.5 to 9, and optionally 4.5 to 8.5.

[0106] The positive electrode material formed by single crystal particles has a large surface area and a relatively dense structure, so that the positive electrode active material can maintain good structural stability while having a high compaction density, thereby reducing side reactions during charging and discharging, slowing down the consumption of electrolyte, and improving the battery life. The positive electrode active material that meets the above conditions has good structural stability, so that the battery including the positive electrode active material can have high energy density, excellent rate performance and long cycle life.

[0107] In some embodiments, the pore volume of the positive electrode film layer accounts for 18% to 35% of the total volume of the positive electrode film layer.

[0108] When the pore volume of the positive electrode film layer is within an appropriate range, the organic lithium salt in the electrolyte can easily enter the pores of the positive electrode film layer and fully contact the positive electrode active material, thereby increasing the migration rate of ions at the electrode / electrolyte interface, reducing the internal resistance of the battery, and improving the battery's rate performance.

[0109] In some embodiments, the secondary battery further comprises a negative electrode, the negative electrode comprises a negative electrode membrane, the negative electrode membrane comprises a negative electrode active material, the negative electrode active material comprises a silicon-based material, and the silicon-based material is selected from one or more of elemental silicon, silicon-oxygen material, and silicon-carbon material. The negative electrode active material preferably contains at least a silicon-carbon material.

[0110] Silicon-based materials can significantly increase the energy density of batteries.

[0111] In some embodiments, the negative electrode active material further comprises a carbon-based material, and the mass ratio of the carbon-based material to the silicon-based material is no more than 4:6, and can be optionally no more than 2:8.

[0112] In some embodiments, the mass ratio of the carbon-based material to the silicon-based material does not exceed 4:6, 4:7, 4:8, 4:9, 4:10, 4:11, 4:12, 4:13, 4:14, 4:15, 2:8 or any value thereof. When the mass ratio of the carbon-based material to the silicon-based material is within the above range, the battery can have a high energy density while reducing the expansion of the negative electrode, and improving the cycle performance and rate performance.

[0113] In some embodiments, the surface density of the negative electrode film is 6 to 13 mg / cm 2 .

[0114] In some embodiments, the surface density of the negative electrode film is 6 mg / cm 2 , 7mg / cm 2 , 8mg / cm 2 , 9mg / cm 2 、10mg / cm 2 、11mg / cm 2 , 12mg / cm 2 、13mg / cm 2 or any value therein.

[0115] When the surface density of the negative electrode film is within the above range, the negative electrode adopts a thick coating design, which helps to improve the energy density of the battery.

[0116] In some embodiments, the negative electrode sheet includes a negative electrode current collector, and the negative electrode film layer of any embodiment is disposed on at least one side of the negative electrode current collector.

[0117] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.

[0118] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, copper foil may be used. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0119] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS).

[0120] In some embodiments, the negative electrode film layer may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.

[0121] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).

[0122] In some embodiments, the negative electrode sheet can be prepared in the following manner: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.

[0123] In some embodiments, the positive electrode sheet includes a positive electrode current collector, and the positive electrode film layer of any embodiment is disposed on at least one side of the positive electrode current collector.

[0124] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.

[0125] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0126] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.

[0127] In some embodiments, the positive electrode film layer may further include a conductive agent, which may include, for example, at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0128] In some embodiments, the positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0129] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical stability and mechanical stability can be selected.

[0130] In some embodiments, the material of the isolation membrane can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane can be a single-layer film or a multi-layer composite film, without particular limitation. When the isolation membrane is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0131] In one embodiment of the present application, there is provided an electric device, comprising the secondary battery of any embodiment.

[0132] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square or any other shape. Figure 1 The secondary battery 5 is a square structure as an example.

[0133] In some embodiments, reference Figure 2 , the outer packaging may include a shell 51 and a cover plate 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0134] The electrical device includes the secondary battery provided in the present application. The secondary battery can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device can include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.

[0135] Figure 3 The power consumption device is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the high power and high energy density requirements of the power consumption device for the secondary battery, a battery pack or a battery module can be used.

[0136] Another example of a device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be thin and light, and a secondary battery may be used as a power source. Example

[0137] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0138] 1. Preparation method

[0139] 1. Preparation of positive electrode sheet Preparation of positive electrode active materials: lithium hydroxide and dried high nickel ternary precursor are weighed according to the stoichiometric ratio of the chemical formula, the mixture is mixed evenly in a high-speed mixer and then sintered in a kiln. The sintering temperature is S760°C, the sintering time is S20Sh, and the sintering atmosphere is oxygen. After cooling, the matrix material can be obtained. The material is washed with water at a mass ratio of S1:1S for 30 minutes, centrifuged, filtered, and then vibrated and dried at a vibration frequency of S30SHz and a drying time of S5Sh to obtain the positive electrode active material. In this sintering process, the primary particle size is adjusted by adjusting the sintering temperature, and the secondary particle size is adjusted by adjusting the precursor particle size.

[0140] The composition of the positive electrode active material is LiNi 0.93 Co 0.05 Mn 0.01 Al 0.005 N 0.005O2, wherein the primary particle size of particle A is 200 nm and the volume average particle size is 10 μm; the primary particle size of particle B is 1 μm and the volume average particle size is 5 μm; the mass ratio of particle A to particle B is 4:1.

[0141] The positive electrode active material, conductive agent carbon black, and binder polyvinylidene fluoride (PVDF) were mixed uniformly in N-methylpyrrolidone (NMP) solution at a mass ratio of 97%:1%:2% to prepare the positive electrode slurry, which was then evenly coated on the positive electrode current collector, coated on the surface of aluminum foil by an extrusion coater and dried, and then the coated electrode was cold pressed by a cold press. The compacted density of the positive electrode film was 3.3 mg / cm 3 The final positive electrode sheet is prepared, wherein the thickness of the positive electrode current collector is 13 μm.

[0142] 2. Preparation of negative electrode sheet The negative electrode active materials artificial graphite and carbon silicon material, conductive agent carbon black, carbon nanotubes, binder styrene butadiene rubber (SBR), thickener sodium hydroxymethyl cellulose (CMC-Na) are mixed in a proper amount of deionized water at a weight ratio of 60.48%: 34.02%: 1%: 0.375%: 2.8%: 1.325% to form a uniform negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and the negative electrode film layer is obtained after drying and other processes. The surface density of the negative electrode film is 9.4Smg / cm 2 .

[0143] 3. Isolation film A polyethylene film (PE membrane) is used as the isolation membrane.

[0144] 4. Electrolyte Ethylene carbonate, ethyl methyl carbonate and diethyl carbonate are mixed in a volume ratio of 1:1:1 to obtain an organic solvent, and fully dried lithium salt LiPF6 is dissolved in the mixed organic solvent to prepare an electrolyte with a LiPF6 concentration of 1 mol / L; then 10 wt% of LiFSI is added and mixed evenly.

[0145] 5. Preparation of batteries The positive electrode sheet, the separator, and the negative electrode sheet are stacked in order, so that the separator is between the positive and negative electrode sheets to play an isolating role, and the electrolyte is injected to assemble into a secondary battery.

[0146] See Table 1 for specific parameters

[0147] Example 2 The preparation method of Example 2 is basically the same as that of Example 1, except that the type of organic lithium salt is adjusted. The specific parameters are shown in Table 1.

[0148] Embodiments 3 to 6 The preparation methods of Examples 3 to 6 are basically the same as those of Example 1, except that the mass content of the organic lithium salt is adjusted. The specific parameters are shown in Table 1.

[0149] Example 7 The preparation method of Example 7 is basically the same as that of Example 1, except that the B particles of the positive electrode active material are single crystals. The specific parameters are shown in Table 1.

[0150] Embodiments 8 to 12 The preparation methods of Examples 8 to 12 are basically the same as those of Example 1, except that the mass content of the organic lithium salt and the surface density of the positive electrode film layer are adjusted. The specific parameters are shown in Table 1. Among them, the compacted density of the positive electrode film layer of Example 8 is 3.3 mg / cm 3 The compacted density of the positive electrode film of Example 12 is 3.2 mg / cm 3 , and the rest is the same as the compaction density of the positive electrode film layer in Example 1.

[0151] Embodiments 13 to 16 The preparation methods of Examples 13 to 16 are basically the same as those of Example 1, except that the composition of the positive electrode active material particles is adjusted, and the specific parameters are shown in Table 1. In Examples 13 to 15, the primary particle size and secondary particle size of particles A and B are adjusted by adjusting the sintering temperature, and the particles are obtained by preparing precursors with different particle sizes; in Example 16, the positive electrode active material includes only one single crystal particle.

[0152] Comparative Example 1 The preparation methods of Comparative Example 1 and Example 1 are basically the same, except that the electrolyte in Comparative Example 1 only includes inorganic lithium salt but not organic lithium salt. Specific parameters are shown in Table 1.

[0153] Comparative Example 2 The preparation method of Comparative Example 2 is basically the same as that of Example 1, except that the surface density of the positive electrode film layer is adjusted. The specific parameters are shown in Table 1. Among them, the compacted density of the positive electrode film layer is 3.6 mg / cm 3 .

[0154] 2. Performance Test

[0155] 1. Mass energy density and unit area energy density test 1) The discharge energy measurement method of a battery cell is as follows: Leave the battery cell at 25°C for 2 hours to ensure that the temperature of the battery cell is 25°C; After charging the battery cell to the charging cut-off voltage at 0.1C at 25°C, continue to charge at a constant voltage at the charging cut-off voltage until the current reaches 0.05C and the charging is cut off (where C represents the rated capacity of the battery cell); Let the battery cells stand at 25°C for 1 hour; At 25°C, the battery cells were discharged at 0.1C to the discharge cut-off voltage, and the total discharge capacity C0 released by the battery cells was recorded, and the total discharge energy was E0. Among them, the charge cut-off voltage was 4.25V and the discharge cut-off voltage was 2.0V. 2) The calculation formula of energy density per unit area of ​​positive electrode film is as follows: If the battery is coated on both sides with positive electrode active materials, the energy density per unit area of ​​the positive electrode film layer = battery cell discharge energy E0 / (2×area of ​​the positive electrode film layer); If the battery is coated with positive electrode active material on one side, the energy density per unit area of ​​the positive electrode film layer = battery cell discharge energy E0 / area of ​​the positive electrode film layer.

[0156] 2. Dynamic performance

[0157] Charging rate test

[0158] At 25°C, fully charge the battery at xSC and fully discharge at 1C for 10 times, then fully charge the battery at xSC again, disassemble the negative electrode, and observe the lithium deposition on the surface of the negative electrode. If there is no lithium deposition on the negative electrode surface, increase the charging rate xSC by 0.1C and test again until lithium deposition on the negative electrode surface. Stop the test. The charging rate minus 0.1C is the maximum charging rate of the battery. The charging cut-off voltage is 4.25V and the discharging cut-off voltage is 2.0V.

[0159] Discharge rate performance

[0160] At 25°C, the battery is fully charged at 0.33C and the constant voltage charging cut-off current is 0.05C, then fully discharged at 0.33C, and C0 is recorded as the initial capacity; then fully charged at 0.33SC and the constant voltage charging cut-off current is 0.05C, then fully discharged at 2C, and the capacity C1S is recorded at this time, and the 2C discharge retention rate is C1 / C0. Among them, the charging cut-off voltage is 4.25V, and the discharging cut-off voltage is 2.0V.

[0161] 3. Measurement method of unit surface density of positive electrode film layer and negative electrode film layer

[0162] The unit surface density of the positive and negative electrode film layers = m / S, where m represents the weight of the film layer and S represents the area of ​​the film layer. m can be obtained by subtracting the weight of the current collector from the weight of the pole piece, and the length and width of the film layer can be measured with a ruler. If the pole piece is a double-sided coated film layer, the surface density of the film layer = (pole piece weight - current collector weight) / (2×film area).

[0163] 4. Particle size test The particle size distribution test was conducted using a Microtrac MRB S3500 laser particle size analyzer. The specific test process is as follows: 0.05-2g of positive electrode active material was taken, 10-20ml of deionized water was added, and ultrasonication was performed at a frequency of 53KHz and a power of 120W for 5 minutes to ensure that the sample was completely dispersed. The sample was then measured in accordance with the GB / T19077-2016 or ISO 13320:2009 standard. The volume average particle size and peak position difference of the particles were measured through the particle size volume distribution curve. The cross section of the particles was observed using a scanning electron microscope to test the primary particle size.

[0164] The test results of the embodiments and comparative examples are shown in Table 1.

[0165] According to the above results, the secondary battery of Examples 1-16 includes an electrolyte and a positive electrode, the positive electrode includes a positive electrode film layer, and the energy density per unit area of ​​the single-side positive electrode film layer meets 18-37 mWh / cm 2 .

[0166] The electrolyte of the secondary battery of Comparative Example 1 includes only inorganic lithium salts but no organic lithium salts. Compared with Comparative Example 1, the batteries of Examples 1-16 have high energy density and exhibit excellent kinetic performance, and the maximum charge rate and the discharge capacity retention rate at high rate are improved.

[0167] It can be seen from Examples 1-12 that when the relationship between the positive electrode film layer and the organic lithium salt satisfies 0.005≤M-0.0005×w≤0.2, the organic lithium salt can form an effective combination with the positive electrode film layer, so that the battery has a high charging rate or a capacity retention rate at a high charging rate, that is, the battery's kinetic performance is improved.

[0168] From the comparison between Examples 1-16 and Comparative Example 2, it can be seen that the surface density w of the single-sided positive electrode film layer is not less than 20 mg / cm 2 , can be selected as 25~45mg / cm 2 The battery has a high energy density.

[0169] It can be seen from Examples 1 and 13-15 that the battery kinetic performance can be improved by grading the two sizes of particles, AB.

[0170] From the comparison among Example 1, Example 7 and Example 16, it can be seen that compared with the positive electrode active material including single crystal, the small particles of the positive electrode active material are all polycrystalline, which is beneficial to improving the dynamic performance of the battery.

[0171] From the comparison between Example 1 and Examples 13-16, it can be seen that when the positive electrode active material includes particles A and particles B and particles A and particles B have two different particle sizes, it is beneficial to further improve the energy density and kinetic performance of the battery.

[0172] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A secondary battery, wherein: The secondary battery comprises: an electrolyte, wherein the electrolyte comprises an organic lithium salt; and The positive electrode comprises a positive electrode film layer, and the energy density per unit area of ​​the positive electrode film layer on one side is 18 to 37 mWh / cm 2 , can be selected as 18~35.7mWh / cm 2 .

2. The secondary battery according to claim 1, wherein the positive electrode film layer and the organic lithium salt satisfy the following relationship: 0.005≤M-0.0005×w≤0.2 in, M is the mass content of the organic lithium salt based on the total mass of the electrolyte; w is the surface density of the positive electrode film layer on one side, in mg / cm 2 .

3. The secondary battery according to claim 1 or 2, wherein: The surface density w of the positive electrode film layer on one side is not less than 20 mg / cm 2 , optionally 25 to 45 mg / cm 2 .

4. The secondary battery according to any one of claims 1 to 3, wherein The organic lithium salt includes at least one of lithium bis(fluorosulfonyl)imide and lithium bis(trifluoromethylsulfonyl)imide.

5. The secondary battery according to any one of claims 1 to 4, wherein The electrolyte also includes an inorganic lithium salt, and the molar ratio of the organic lithium salt to the inorganic lithium salt is 1:5 to 5:

1.

6. The secondary battery according to any one of claims 1 to 5, wherein The positive electrode film layer contains positive electrode active materials, and the positive electrode active materials include particles A and particles B. The particles A are polycrystalline particles, and the volume average particle size of the particles A is larger than the volume average particle size of the particles B.

7. The secondary battery according to claim 6, wherein The positive electrode film layer also satisfies at least one of the following characteristics: (1) The particle B is a polycrystalline, single crystal or quasi-single crystal particle; (2) The primary particle size of the particle A is 50 nm to 400 nm, and may be 80 to 200 nm; the primary particle size of the particle B is 150 nm to 2 μm, and may be 200 nm to 1.2 μm; (3) The volume average particle size of the particles A is 2 to 25 μm, and may be 2.5 to 23 μm; the volume average particle size of the particles B is 0.65 to 10 μm, and may be 1.2 to 8.5 μm; (4) The mass ratio of the particles A to the particles B is 5:5 to 9:1; (5) The laser particle size distribution curve of the positive electrode active material is bimodal, and the peak position difference between the two peaks is 3 to 7 μm; (6) The positive electrode includes a positive electrode current collector, and the ratio of the thickness of the positive electrode film layer on one side to the thickness of the positive electrode current collector is 5.5 to 15, and optionally 5.6 to 8.

8.

8. The secondary battery according to claim 6 or 7, wherein: Based on the total molar number of transition metal elements in the positive electrode active material, the molar content of nickel element is not less than 80%; optionally, not less than 85%; further optionally, not less than 90%.

9. The secondary battery according to any one of claims 6 to 8, wherein The compositions of the particles A and B independently satisfy Formula I, Li a1 Ni x1 Co y1 Mn z1 M1 b1 O2M1' c1 , formula I Among them, a1 is 0.8-1.2, x1 is 0.85-1, y1 is 0-0.15, z1 is 0-0.15, b1 is 0-0.02, c1=1-x1-y1-z1-b1, M1 includes at least one of Zr, Y, Al, Ti, W, Sr, Ta, Sb, Nb, Na, K, B, Mg, Zn, Ca or Ce, and M1' includes at least one of N, F, S or Cl.

10. The secondary battery according to any one of claims 1 to 5, wherein The positive electrode film layer contains a positive electrode active material, and the positive electrode active material is a single crystal or a quasi-single crystal particle, and meets at least one of the following characteristics: (1) The laser particle size distribution curve of the positive electrode active material is single-peaked; (2) The volume average particle size D of the single crystal or quasi-single crystal particles v 50 is 1 to 3.5 μm, optionally 1.2 to 3.0 μm; (3) The laser particle size distribution of the single crystal or quasi-single crystal particles satisfies: 0.3≤(D v 99-D v 90) / (2×D v 50)≤0.55; (4) The composition of the single crystal or quasi-single crystal particles is as shown in Formula II: Li a2 Ni x2 Co y2 Mn z2 M2 b2 O2M2' c2 , Formula II Wherein, a2 is 0.8-1.2, x2 is 0.85-1, y2 is 0-0.15, z2 is 0-0.15, b2 is 0-0.02, c2=1-x2-y2-z2-b2, M2 includes at least one of Zr, Y, Al, Ti, W, Sr, Ta, Sb, Nb, Na, K, B, Mg, Zn, Ca or Ce, and M2' includes at least one of N, F, S or Cl; optionally, x2 is 0.90-1; (5) The positive electrode includes a positive electrode current collector, and the ratio of the thickness of the positive electrode film layer on one side to the thickness of the positive electrode current collector is 4.5 to 9, and optionally 4.5 to 8.

5.

11. The secondary battery according to any one of claims 1 to 10, wherein The secondary battery further comprises a negative electrode, which comprises a negative electrode membrane, which comprises a negative electrode active material, which comprises a silicon-based material, and which comprises one or more of elemental silicon, silicon-oxygen material, and silicon-carbon material.

12. The secondary battery according to claim 11, wherein The negative electrode active material further comprises a carbon-based material, and a mass ratio of the carbon-based material to the silicon-based material is no more than 4:6, and can be optionally no more than 2:

8.

13. The secondary battery according to claim 11 or 12, wherein: The surface density of the negative electrode membrane is 6 to 13 mg / cm 2 .

14. An electrical device comprising the secondary battery according to any one of claims 1 to 13.

Citation Information

Cited By

  • Battery cell, battery device, electric device, and energy storage device

    CN120300266A

  • Battery cell, battery device, power consuming device, and energy storage device

    CN120300266B

  • Battery cell, battery device, and electrical device

    WO2026214020A1

  • Battery cell and electric device

    WO2026214207A1