Laminated ceramic electronic device
By using a second metal layer with a Young's modulus smaller than the first metal layer to cover the first metal layer in the laminated ceramic electronic device, the problem of cracks and peeling caused by the accumulation of contact stress between the external electrode and the component body is solved, and the stability of the device is improved. Sexual and contact performance.
Patent Information
- Application Number
- CN202410374447.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-29
- Publication Date
- 2024-10-01
AI Technical Summary
In laminated ceramic electronic devices, stress accumulation in the contact between the external electrodes and the component body may cause cracks in the component body or peeling off of the external electrodes.
Adopt a structural design in which the second metal layer of the external electrode covers the first metal layer and is in contact with it, and the Young's modulus of the second metal layer is smaller than the first metal layer, ensuring that cracks in the component body are reduced when stress is concentrated. and risk of external electrode stripping.
Effectively suppresses cracks on the component body and external electrode peeling, reduces contact resistance, and achieves more stable electrode connection.
Smart Images

Figure CN118737701A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a stacked ceramic electronic device. Background Art
[0002] In a laminated ceramic electronic device (e.g., a laminated ceramic capacitor), it is known to provide an uncovered area where the internal nickel electrode layer is not covered by the external nickel electrode layer, and to arrange an external copper electrode layer in the uncovered area (e.g., Japanese Patent Application Publication No. 2022-14532). A known structure is that the external electrode does not cover the side surface of the side edge portion (e.g., Japanese Patent Application Publication No. 2017-195359). Summary of the invention
[0003] According to one aspect of an embodiment of the present invention, there is provided a laminated ceramic electronic device, comprising: an element body, comprising: a laminated body in which a plurality of internal electrodes and a plurality of dielectric layers are alternately laminated in a first direction, a pair of covering dielectric layers sandwiching the laminated body in the first direction, and a pair of end faces opposite to each other in a second direction, the plurality of internal electrodes being alternately exposed at the pair of end faces, the plurality of dielectric layers comprising a pair of side edge portions, the pair of side edge portions sandwiching the plurality of internal electrodes in a third direction perpendicular to the first direction and the second direction; and a pair of external electrodes covering each of the pair of end faces, respectively, wherein at least one of the pair of external electrodes comprises a first metal layer and a second metal layer, wherein, at the corresponding end faces of the element body, the first metal layer covers a portion of the plurality of internal electrodes and a first portion of the pair of covering dielectric layers and the pair of side edge portions located on one side of the plurality of internal electrodes, does not cover a second portion of the pair of covering dielectric layers and the pair of side edge portions other than the first portion, and contacts a portion of the plurality of internal electrodes, and is mainly composed of nickel or copper, and wherein the second metal layer covers the first metal layer and contacts at least a portion of the second portion located on one side of the first metal layer, and is mainly composed of tin.
[0004] According to another aspect of an embodiment of the present invention, there is provided a laminated ceramic electronic device, comprising: an element body, comprising: a laminated body in which a plurality of internal electrodes and a plurality of dielectric layers are alternately laminated in a first direction, a pair of covering dielectric layers sandwiching the laminated body in the first direction, and a pair of end faces opposite to each other in a second direction, the plurality of internal electrodes being alternately exposed at the pair of end faces, the plurality of dielectric layers comprising a pair of side edge portions sandwiching the plurality of internal electrodes in a third direction perpendicular to the first direction and the second direction; and a pair of external electrodes covering each end face of the pair of end faces, wherein at least one of the pair of external electrodes comprises a first metal layer and a second metal layer, wherein, at the corresponding end face of the element body, the first metal layer covers a portion of the plurality of internal electrodes and a first portion of the pair of covering dielectric layers and the pair of side edge portions located on one side of the plurality of internal electrodes, does not cover a second portion of the pair of covering dielectric layers and the pair of side edge portions other than the first portion, and contacts a portion of the plurality of internal electrodes, and wherein the second metal layer covers the first metal layer and contacts at least a portion of the second portion located on one side of the first metal layer, and the Young's modulus of the second metal layer is smaller than that of the first metal layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0005] Figure 1 is a partial cross-sectional perspective view of a laminated ceramic capacitor according to an embodiment;
[0006] Figure 2 is along Figure 1 The cross-sectional view taken along line AA in FIG.
[0007] Figure 3 is along Figure 1 The cross-sectional view taken along line BB in FIG.
[0008] Figure 4 Seen through the external electrodes Figure 1 a schematic diagram of a first surface of
[0009] Figure 5 Seen through the external electrodes Figure 1 a schematic diagram of a second surface of
[0010] Figure 6 The multilayer ceramic capacitor of comparison object 1 is Figure 1 The cross-sectional view corresponding to the AA section in FIG.
[0011] Figure 7 The multilayer ceramic capacitor of comparison object 2 is Figure 1 The cross-sectional view corresponding to the AA section in FIG.
[0012] Fig. 8A and Figure 8Bis a schematic diagram of a laminated ceramic capacitor of comparison object 1 and comparison object 2 mounted on a mounting substrate;
[0013] Figure 8C is a schematic diagram of a laminated ceramic capacitor according to an embodiment when mounted on a mounting substrate;
[0014] Fig. 9 is a schematic diagram of the first surface of the multilayer ceramic capacitor of Comparative Object 3 seen through the external electrode;
[0015] Fig.10 is a flowchart of an example of a manufacturing process of a laminated ceramic capacitor;
[0016] Figures 11A to 11C is a cross-sectional view of a method for manufacturing a laminated ceramic capacitor according to an embodiment;
[0017] Figures 12A to 12C is a cross-sectional view of a method for manufacturing a laminated ceramic capacitor according to an embodiment;
[0018] FIG. 13A to FIG. 13D are cross-sectional views of various examples of external electrodes in the embodiments; and
[0019] Fig.14 Seen through the external electrodes Fig. 13B Schematic diagram of the first surface. DETAILED DESCRIPTION
[0020] When a multilayer ceramic electronic device is mounted on a mounting substrate, if stress is concentrated at the end where the external electrode and the component body are in contact, problems such as cracking of the component body or peeling of the external electrode may occur.
[0021] Hereinafter, exemplary embodiments will be described with reference to the accompanying drawings.
[0022] (Implementation Method)
[0023] Figure 1 is a partial cross-sectional perspective view of a multilayer ceramic capacitor 100 according to an embodiment. Figure 2 is along Figure 1 Cross-sectional view taken along line AA. Figure 3 is along Figure 1 Cross-sectional view taken along line BB in FIG. Figure 4 Seen through the external electrodes Figure 1 Schematic diagram of the first surface.
[0024] Figure 5 Seen through the external electrodes Figure 1 Schematic diagram of the second surface of Figure 4 and Figure 5In FIG. 1 , the region where the metal layers 21 a and 21 b are provided is indicated by a thick dotted line.
[0025] exist Figure 1 to Figure 5 , the Z direction (first direction) is the stacking direction of the stacked dielectric layer 14 and the internal electrodes 12a, 12b, and the fifth surface 55 and the sixth surface 56 of the element body 10 are opposite to each other. The X direction (second direction) is the length direction of the element body 10, and is also the direction in which the first surface 51 and the second surface 52 of the element body 10 are opposite to each other. The Y direction (third direction) is the width direction of the internal electrodes 12a, 12b, and is also the direction in which the third surface 53 and the fourth surface 54 of the element body 10 are opposite to each other. The X direction, the Y direction, and the Z direction are perpendicular to each other.
[0026] The multilayer ceramic capacitor 100 includes a device body 10 having a substantially rectangular parallelepiped shape, and external electrodes 20 a and 20 b .
[0027] The element body 10 has a plurality of dielectric layers 14 and a plurality of internal electrodes 12a, 12b, and a covering dielectric layer 16. The plurality of internal electrodes 12a and the plurality of internal electrodes 12b are alternately stacked in the Z direction. One of the plurality of dielectric layers 14 is provided between one of the plurality of internal electrodes 12a and one of the plurality of internal electrodes 12b. The outermost layer in the stacking direction (Z direction) of the stacked body 40 in which the dielectric layers 14 and the internal electrodes 12a, 12b are stacked is the internal electrodes 12a, 12b. In the Z direction of the stacked body 40, a pair of covering dielectric layers 16 are provided to sandwich the stacked body 40. The portion in which the dielectric layer 14 is sandwiched between the internal electrodes 12a, 12b and facing each other is the capacitor portion 15. Figure 2 In FIG. 1 , the portion sandwiching the capacitor portion 15 in the X direction of the element body 10 is a pair of edge portions 42. Figure 3 to Figure 5 In the diagram, the portion sandwiching the capacitor portion 15 in the Y direction is a pair of side edge portions 18 .
[0028] The internal electrodes 12a and 12b are alternately exposed on the first surface 51 and the second surface 52. The internal electrode 12a is exposed on the first surface 51, but the internal electrode 12b is not exposed on the first surface 51. The internal electrode 12b is exposed on the second surface 52, but the internal electrode 12a is not exposed on the second surface 52. That is, each of the internal electrodes 12a and 12b is connected to different first surfaces 51 and second surfaces 52, respectively.
[0029] like Figure 2 , Figure 4 and Figure 5As shown, the external electrode 20a (and 20b) (a pair of external electrodes) includes a metal layer 21a (and 21b) (a first metal layer) and a metal layer 22a (and 22b) (a second metal layer). On the first surface 51 (and the second surface 52), the portion surrounding the internal electrode 12a (and 12b) and located on the side of the internal electrode 12a (and 12b) covering the dielectric layer 16 and the side edge portion 18 is a portion 57a (and 57b) (a first portion). The portion covering the dielectric layer 16 and the side edge portion 18 other than the portion 57a (and 57b) is a portion 58a (and 58b) (a second portion). The metal layer 21a (and 21b) is in contact with the internal electrode 12a (and 12b), covers and contacts the portion 57a (and 57b), and does not cover the portion 58a (and 58b), respectively.
[0030] Metal layer 22a (and 22b) covers metal layer 21a (and 21b) and covers and contacts portion 58a (and 58b) at first surface 51 (and second surface 52). Metal layer 22a (and 22b) is not provided on third surface 53 and fourth surface 54.
[0031] The size of the laminated ceramic capacitor 100 is, for example, 0.25 mm in length (length in the X direction), 0.125 mm in width (width in the Y direction), and 0.125 mm in height (height in the Z direction), or 0.4 mm in length, 0.2 mm in width, and 0.2 mm in height, or 0.6 mm in length, 0.3 mm in width, and 0.3 mm in height, or 1.0 mm in length, 0.5 mm in width, and 0.5 mm in height, or 3.2 mm in length, 1.6 mm in width, and 1.6 mm in height, or 4.5 mm in length, 3.2 mm in width, and 2.5 mm in height. The size of the laminated ceramic capacitor 100 is not limited to these sizes.
[0032] The width of the side edge portion 18 in the Y direction is, for example, 10 μm to 30 μm. The length of the end edge portion 42 in the X direction is, for example, 10 μm to 50 μm.
[0033] The internal electrodes 12a and 12b are mainly composed of base metals such as nickel (Ni), copper (Cu) or tin (Sn). As the internal electrodes 12a and 12b, precious metals such as platinum (Pt), palladium (Pd), silver (Ag), gold (Au) or alloys containing these metals can be used. The thickness of the internal electrodes 12a and 12b is, for example, not less than 0.1 μm and not more than 1 μm.
[0034] For example, the main component of the dielectric layer 14 is a ceramic material having a perovskite structure represented by the general formula ABO3. It is worth noting that the perovskite structure includes ABO3 having a non-stoichiometric composition. 3-αFor example, the ceramic material is barium titanate (BaTiO3), calcium zirconate (CaZrO3), calcium titanate (CaTiO3), strontium titanate (SrTiO3), magnesium titanate (MgTiO3) and Ba 1-x- y Ca x Sr y Ti 1-z Zr z At least one of O3 (0≤x≤1, 0≤y≤1, 0≤z≤1). 1-x-y Ca x Sr y Ti 1-z Zr z O3 is, for example, barium strontium titanate, barium calcium titanate, barium zirconate, barium titanate zirconate, calcium titanate zirconate, and barium calcium titanate zirconate. For example, the main component of dielectric layer 14 is 90 atomic % or more of ceramic. The thickness of dielectric layer 14 is, for example, 2 μm or more and 5 μm or less.
[0035] An additive may be added to the dielectric layer 14. As the additive in the dielectric layer 14, an oxide of zirconium (Zr), hafnium (Hf), magnesium (Mg), manganese (Mn), molybdenum (Mo), vanadium (V), chromium (Cr), or a rare earth element (yttrium (Y), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), and ytterbium (Yb)), or an oxide containing cobalt (Co), nickel (Ni), lithium (Li), boron (B), sodium (Na), potassium (K), or silicon (Si), or a glass containing cobalt, nickel, lithium, boron, sodium, potassium, or silicon may be used.
[0036] The composition of the main component ceramic of the cover dielectric layer 16 may be the same as or different from the main component ceramic of the dielectric layer 14. The side edge portion 18 may be a side dielectric layer different from the dielectric layer 14. In this case, the composition of the main component ceramic of the side dielectric layer may be the same as or different from the composition of the main component ceramic of the dielectric layer 14.
[0037] The metal layers 21a, 21b of the external electrodes 20a, 20b are mainly composed of metals such as copper, nickel, aluminum (Al) and zinc (Zn) or alloys of two or more of these metals (for example, an alloy of copper and nickel). In order to densify the metal layers 21a, 21b, the metal layers 21a, 21b may include a glass component. When the metal layers 21a, 21b are fired, a ceramic of a common material, for example, for controlling the sinterability of the metal layers 21a, 21b is included. The glass component is an oxide of barium (Ba), strontium (Sr), calcium (Ca), zinc, aluminum, silicon or boron. The common material is, for example, a ceramic component whose main component is the same as the main component of the dielectric layer 14.
[0038] In the external electrodes 20a and 20b, the main component of the metal layers 22a and 22b is tin, etc. The metal layers 22a and 22b are softer than the metal layers 21a and 21b. That is, the Young's modulus of the metal layers 22a and 22b is smaller than that of the metal layers 21a and 21b.
[0039] Figure 6 The multilayer ceramic capacitor of comparison object 1 is Figure 1 The cross-sectional view corresponding to the AA section in FIG. Figure 6 As shown, in the multilayer ceramic capacitor 110 of the comparative object 1, the external electrodes 20a are respectively provided at the ends of the first surface 51, the third surface 53, the fourth surface 54, the fifth surface 55, and the sixth surface 56. The external electrodes 20b are respectively provided at the ends of the second surface 52, the third surface 53, the fourth surface 54, the fifth surface 55, and the sixth surface 56. The metal layers 22a and 22b are respectively provided on the metal layers 21a and 21b. The metal layers 22a and 22b are respectively provided so as not to contact the first surface 51 and the second surface 52.
[0040] Figure 7 The multilayer ceramic capacitor of comparison object 2 is Figure 1 The cross-sectional view corresponding to the AA section in FIG. Figure 7 As shown, in the multilayer ceramic capacitor 112 of the comparative object 2, the external electrodes 20a and 20b are respectively provided on the first surface 51 and the second surface 52, but not provided on the third surface 53, the fourth surface 54, the fifth surface 55, and the sixth surface 56. The metal layers 21a and 21b are provided on the entire first surface 51 and the entire second surface 52, and the metal layers 22a and 22b are provided outside the metal layers 21a and 21b and in contact with the first surface 51 and the second surface 52.
[0041] Fig. 8A and Figure 8B This is a schematic diagram of the multilayer ceramic capacitors of Comparison Object 1 and Comparison Object 2 mounted on a mounting substrate. Figure 8C Schematic diagram of a laminated ceramic capacitor according to an embodiment when mounted on a mounting substrate. Fig. 8A As shown, the multilayer ceramic capacitor 110 of the comparative object 1 is mounted on the pad 31 on the mounting substrate 30. The external electrodes 20a, 20b are connected to the pad 31 by a connecting material 32 (for example, solder). When thermal stress is applied to the element body 10 due to the difference in linear expansion coefficient between the mounting substrate 30 and the element body 10, the stress is concentrated at the end 60 of the external electrodes 20a, 20b on the fifth surface 55. This may cause cracks 62 to appear in the element body 10.
[0042] like Figure 8BAs shown, in the multilayer ceramic capacitor 112 of the comparative object 2, the external electrodes 20a and 20b are not provided on the fifth surface 55, so the stress concentration on the fifth surface 55 of the element body 10 is reduced. However, the portion 64 of the end portion where the external electrodes 20a and 20b contact the first surface 51 is the end portion of the metal layer 21a and 21b. Since the metal layer 21a and 21b is a hard metal, if the stress is concentrated in this portion 64, the metal layer 21a and 21b may be peeled off from the element body 10.
[0043] like Figure 8C As shown, in the laminated ceramic capacitor 100, the metal layers 22a and 22b cover the portions 58a and 58b of the first surface 51 and the second surface 52 that are not covered by the metal layers 21a and 21b. The metal layers 22a and 22b are softer than the metal layers 21a and 21b. Therefore, even if the stress is concentrated on the portion 64, the metal layers 22a and 22b are less likely to be peeled off from the element body 10 than the laminated ceramic capacitor 112 of the comparative object 2. Since the stress is less likely to be concentrated on the portion 66 at the end of the metal layers 21a and 21b than on the portion 64, the metal layers 21a and 21b are less likely to be peeled off from the element body 10.
[0044] Fig. 9 Schematic diagram of the first surface of the multilayer ceramic capacitor of Comparative Object 3 seen through the external electrodes. The area where the metal layer 21a is provided is indicated by a thick dotted line. Fig. 9 As shown, in the multilayer ceramic capacitor 114 of the comparative object 3, the metal layer 21a does not cover the end region 70 of the internal electrode 12a in the Y direction. Therefore, the metal layer 22a is in contact with the internal electrode 12a in the region 70. If the contact resistance between the metal layer 22a and the internal electrode 12a is high, the contact resistance between the external electrode 20a and the internal electrode 12a will also be high.
[0045] like Figure 4 and Figure 5 As shown, in the multilayer ceramic capacitor 100 of the embodiment, the metal layers 21a and 21b are in contact with the internal electrodes 12a and 12b and cover the portions 57a and 57b. Therefore, the contact resistance between the external electrode 20a and the internal electrode 12a can be reduced.
[0046] (Method for Manufacturing Multilayer Ceramic Capacitor)
[0047] A method of manufacturing the laminated ceramic capacitor 100 will be described. Fig.10 This is a flowchart showing an example of a manufacturing process of a multilayer ceramic capacitor.
[0048] (Green sheet forming process) First, a green sheet is formed (step S10). For example, in step S10, a dielectric material obtained by adding various additive compounds (sintering aids, etc.) to ceramic powder is mixed with a binder (for example, polyvinyl butyral (PVB) resin), and an organic solvent (for example, ethanol or toluene) and a plasticizer are added, and then wet-mixed. Using the obtained slurry, a dielectric green sheet is coated on a substrate by, for example, a die coater method or a doctor blade method, and then dried. The substrate is, for example, a PET (polyethylene terephthalate) film.
[0049] (Internal electrode printing process) Next, the internal electrodes are printed on the green sheet (step S12). In step S12, a metal conductive paste containing an organic binder for forming the internal electrodes is printed on the green sheet on the substrate using, for example, a gravure printing method. As a result, a plurality of internal electrode patterns spaced apart from each other corresponding to the internal electrodes 12a and 12b are formed on the green sheet. Ceramic particles are added to the metal conductive paste as a co-material. Although the main component of the ceramic particles is not particularly limited, it is preferably the same as the main component ceramic of the dielectric layer 14.
[0050] (Compression bonding process) Subsequently, the raw sheets are stacked and pressed together (step S14). In step S14, a laminated sheet is formed by stacking raw sheets printed with internal electrode patterns that will become the internal electrodes 12a, 12b. The raw sheets corresponding to the covering dielectric layer 16 are stacked on both end surfaces of the laminated sheet in the stacking direction. Subsequently, by applying pressure to the laminated sheet, the plurality of raw sheets are press-bonded together. As a press bonding means, for example, hydrostatic pressure can be used. Subsequently, by cutting the laminated sheet along a predetermined cutting line in the stacking direction using a cutting blade, a plurality of element bodies 10 are formed.
[0051] (Firing process) Subsequently, the element body 10 is fired (step S16). In step S16, the element body 10 is subjected to a binder removal treatment at 250°C to 500°C in an N2 atmosphere, and then fired at 1300°C to 1400°C for about 1 hour in a reducing atmosphere. As a result, the particles in the element body 10 and the side dielectric layers 18a and 18b are sintered.
[0052] (First Metal Layer Formation Process) Subsequently, metal layers 21a and 21b are formed (step S18). Figures 11A to 12B Step S18 is described.
[0053] Figures 11A to 12C is a cross-sectional view of a method for manufacturing a laminated ceramic capacitor according to an embodiment. Fig.11A As shown, the metal sheet 28 is placed on the flat elastic body 24. The metal sheet 28 covers the first surface 51. The adhesive tape 26 is attached to the second surface 52 of the element body 10.
[0054] Then, if Fig. 11B As shown, the tape 26 is pressed downward (along the -X direction) by a pressing device (not shown). As a result, the first surface 51 of the component body 10 is pressed against the surface of the metal sheet 28. At this time, the pressed portion of the metal sheet 28 is recessed under the pressure of the component body 10, and the elastomer 24 below the component body 10 is also recessed. The recessed portion of the metal sheet 28 is pressed toward the first surface 51 of the component body 10 under the restoring force of the elastomer 24. Therefore, a portion of the metal sheet 28 is attached to the first surface 51. At this time, the metal sheets 28 at both ends of the first surface 51 in the stacking direction (Z direction) are attached along the corners of the component body 10. Thereafter, when the pressing force of the component body 10 increases, a shear force is generated between the attached portion and other portions of the metal sheet 28, thereby separating the attached portion and other portions from each other.
[0055] Then, if Fig. 11C As shown, the adhesive tape 26 is moved upward (along the +X direction) by the pressing device (not shown). As a result, the component body 10 is separated from the elastic body 24. At this time, the separated portion of the metal sheet 28 is attached to the first surface 51 of the component body 10.
[0056] Then, the metal sheet 28 is Figures 11A to 11C The same method is used to attach the second surface 52 of the component body 10. Fig. 12A As shown, the metal sheet 28 is attached to the entire surface of the first surface 51 and the second surface 52 .
[0057] Then, if Fig. 12B As shown, the metal sheet 28 is subjected to roller grinding. As a result, the outer portion of the metal sheet 28 is ground, and the metal sheet 28 at the outer peripheral portions 58a, 58b of the first surface 51 and the second surface 52 is removed to form metal layers 21a, 21b. At this time, the corners of the element body 10 can be ground and the corners of the element body 10 can be rounded. By selecting the roller grinding conditions, the metal sheet 28 can be ground to a higher degree than the element body 10.
[0058] (Second Metal Layer Formation Process) Subsequently, metal layers 22a and 22b are formed (step S20). Fig. 12C Step S20 is described.
[0059] like Fig. 12CAs shown, by plating the surfaces of the metal layers 21a and 21b, metal layers 22a and 22b are formed on the surfaces of the metal layers 21a and 21b. By appropriately selecting the plating conditions, the metal layers 22a and 22b can also be formed on the end faces of the metal layers 21a and 21b, thereby forming the metal layers 22a and 22b in contact with the portions 58a and 58b. By appropriately selecting the plating time, the metal layers 22a and 22b can cover the entire surfaces of the portions 58a and 58b. After a thin seed layer is formed on the surfaces of the metal layers 21a and 21b and the portions 58a and 58b by electroless plating or sputtering, the metal layers 22a and 22b can be formed on the surface of the seed layer by plating.
[0060] The metal layers 21a and 22a form the external electrode 20a, and the metal layers 21b and 22b form the external electrode 20b.
[0061] (Another Example of External Electrode Forming Process) Fig.10 Before the step of firing the element body 10 in step S16, a paste is applied on the first surface 51 and the second surface 52 as the metal sheet 28, such as Fig. 12A Then, Fig.10 The firing of step S16 in the embodiment. Fig. 12B As shown, the metal sheet 28 shrinks to form portions 58a and 58b that are not covered by the metal layers 21a and 21b at the outer peripheries of the first surface 51 and the second surface 52. Fig. 12C As shown, metal layers 22a and 22b are formed. External electrodes 20a and 20b can be formed in this way. The method of forming external electrodes 20a and 20b is not limited to the above method.
[0062] (Example of external electrode) FIG. 13A to FIG. 13D 2 are cross-sectional views of various examples of external electrodes in the embodiments. Fig.13A As shown, metal layer 22a (and 22b) may completely cover portion 58a (and portion 58b).
[0063] Fig.14 Seen through the external electrodes Fig. 13B The area covered by the metal layers 21a and 22a is indicated by thick dashed lines. Fig. 13B and Fig.14 As shown, the metal layer 22a (and 22b) may cover the inner portion of the portion 58a (and the portion 58b) and may not cover the outer portion 59a. In this case, since the soft metal layer 22a (and 22b) and the element body 10 are in contact with each other at the end portion 64 of the external electrode 20a (and 20b) where the stress is most concentrated, the metal layer 22a (and 22b) can be prevented from being peeled off from the element body 10.
[0064] like Fig. 13C As shown, a metal layer 23a may be provided between the metal layer 22a (and 22b) and the metal layer 21a (and 21b). It is sufficient as long as the outermost metal layers 22a, 22b of the external electrode 20a (and 20b) are softer than the metal layers 21a, 21b in contact with the internal electrode 12a (and 12b).
[0065] like Fig.13D As shown in FIG. 1 , the metal layer 22a (and 22b) may cover the ends of the fifth surface 55 and the sixth surface 56. In this case, since the relatively soft metal layer 22a (and 22b) and the element body 10 are in contact with each other at the end portion 60 of the external electrode 20a (and 20b) where the stress is most concentrated, the metal layer 22a (and 22b) can be prevented from peeling off from the element body 10. In addition, the Fig. 8A Furthermore, since the end portion 64 of the metal layer 21a (and 21b) is not provided at the corner of the element body 10, stress concentration at the end portion 64 can be suppressed.
[0066] exist FIG. 13A to FIG. 13D In the embodiment, the main component of the internal electrode 12a (and 12b) is, for example, nickel. The main component of the metal layer 21a (and 21b) is, for example, nickel or copper. The main component of the metal layer 22a (and 22b) is, for example, tin. When the metal layer 23a is provided as a diffusion barrier layer, for example, the main component of the metal layer 21a (and 21b) is copper, the main component of the metal layer 22a (and 22b) is tin, and the main component of the metal layer 23a is nickel.
[0067] As described above, in an embodiment, Figure 2 and Figure 4 As shown, metal layer 21a (and 21b) covers portion 57a (and 57b) but does not cover portion 58a (and 58b). Metal layer 22a (and 22b) has a Young's modulus smaller than that of metal layer 21a (and 21b), covers metal layer 21a (and 21b), and covers at least a portion of portion 58a (and 58b) on the side of metal layer 21a (and 21b) on first surface 51 (and second surface 52). Therefore, as Figure 8C As shown, defects such as cracks in the element body 10 or peeling of the external electrodes 20a and 20b can be suppressed. From the perspective of suppressing defects, the Young's modulus of the metal layer 22a (and 22b) is preferably less than 3 / 4 of the Young's modulus of the metal layer 21a (and 21b), and more preferably less than 1 / 2. The metal layers 21a and 21b are in contact with all the internal electrodes 12a and 12b exposed on the first surface 51 and the second surface 52, respectively. Therefore, the contact resistance between the external electrodes 20a and 20b and the internal electrodes 12a and 12b can be reduced.
[0068] The Young's modulus of soft metals is low. The Young's modulus of nickel, copper and tin are 204GPa, 130GPa and 41GPa respectively. Therefore, the metal layers 21a and 21b are mainly composed of nickel or copper, and the metal layers 22a and 22b are mainly composed of tin. The metal layers 21a and 21b may contain a common material, such as nickel or copper. The metal layers 22a and 22b may be made of a tin-based solder (e.g., tin-silver-copper solder or tin-silver solder). Here, the main component allows other elements or compounds to be added intentionally or unintentionally, for example, the content is more than 50 atomic %, more than 80 atomic %, or 90 atomic %.
[0069] like Fig.13D As shown in FIG. 1 , the metal layers 22a and 22b of the external electrodes 20a and 20b may cover the ends of the third surface 53, the fourth surface 54, the fifth surface 55, and the sixth surface 56. However, the multilayer ceramic capacitor becomes larger. Figures 13A to 13C As shown, external electrodes 20a (and 20b) do not cover surfaces other than first surface 51 (and second surface 52) of element body 10. This enables miniaturization of the multilayer ceramic capacitor.
[0070] like Fig.13A As shown, the metal layer 22a (and 22b) may cover the first surface 51 (and the second surface 52) to the end, or, as shown in FIG. Fig. 13B As shown, the metal layer 22a (and 22b) need not cover at least a portion 59a (third portion) of the outer periphery of the first surface 51 (and the second surface 52).
[0071] exist Figure 4 and Figure 5 In the embodiment, if the area of the portions 58a and 58b is too large, when the metal layers 21a and 21b are not aligned with the internal electrodes 12a and 12b, the internal electrodes 12a and 12b may be exposed from the metal layers 21a and 21b. From this point of view, the area of the portion 58a is preferably less than 9 / 10 of the total area of the portions 57a and 58a, and more preferably less than 4 / 5. The area of the portion 58b is preferably less than 9 / 10 of the total area of the portions 57b and 58b, and more preferably less than 4 / 5.
[0072] If the area of the portions 58a, 58b is too small, the end portions 66 (see Figure 8C) will be close to the end portion 64 of the first surface 51 and the second surface 52. In this case, the stress concentration on the portion 66 will become large, and the metal layers 21a and 21b may be peeled off from the element body 10. From this point of view, the area of the portion 58a is preferably 1 / 10 or more of the total area of the portions 57a and 58a, and more preferably 1 / 5 or more. The area of the portion 58b is preferably 1 / 10 or more of the total area of the portions 57b and 58b, and more preferably 1 / 5 or more.
[0073] like Figure 4 and Figure 5 As shown, the width of the portions 57a and 57b in the side edge portion 18 in the Y direction is L1b, the width of the portions 58a and 58b in the Y direction is L2b, and the width of the side edge portion 18 in the Y direction is L3b. The width of the portions 57a and 57b in the cover dielectric layer 16 in the Z direction is L1a, the width of the portions 58a and 58b in the Z direction is L2a, and the width of the cover dielectric layer 16 in the Z direction is L3a.
[0074] From the perspective of not exposing the internal electrode 12a (and 12b) from the metal layer 21a (and 21b), the width L1a (and L1b) is preferably 1 / 10 or more of the width L3a (and L3b), and more preferably 1 / 5 or more. From the perspective of suppressing the metal layer 21a (21b) and peeling, the width L1a (and L1b) is preferably 9 / 10 or less of the width L3a (and L3b), and more preferably 4 / 5 or less.
[0075] exist Fig.14 In the embodiment, if the widths L4a and L4b of the metal layer 22a are not set to a large value, stress will be concentrated on the end of the metal layer 21a, and the metal layer 21a is easily peeled off from the element body 10. From this perspective, the widths L4a and L4b are preferably less than 1 / 2 of the widths L2a and L2b, and more preferably less than 1 / 3. The same applies to the second surface 52.
[0076] An example has been described in which a pair of external electrodes 20a, 20b each include first metal layers 21a, 21b and second metal layers 22a, 22b. At least one of the external electrodes 20a, 20b may include metal layers 21a, 21b and metal layers 22a, 22b on at least one of the corresponding fifth surface 55 and sixth surface 56.
[0077] Although the embodiments of the present invention have been described, it should be understood that the various changes, substitutions, and alterations could be made hereto without departing from the spirit and scope of the invention.
Claims
1. A laminated ceramic electronic device comprising: An element body, comprising: a stacked body in which a plurality of internal electrodes and a plurality of dielectric layers are alternately stacked in a first direction, a pair of covering dielectric layers sandwiching the stacked body in the first direction, and a pair of end faces facing each other in a second direction, the plurality of internal electrodes being alternately exposed at the pair of end faces, the plurality of dielectric layers including a pair of side edge portions, the pair of side edge portions sandwiching the plurality of internal electrodes in a third direction perpendicular to the first direction and the second direction; and a pair of external electrodes, each of which covers the end faces of the pair of end faces, wherein at least one of the pair of external electrodes comprises a first metal layer and a second metal layer, wherein, at the corresponding end surface of the element body, the first metal layer covers a portion of the plurality of internal electrodes and a first portion of the pair of dielectric layers and the pair of side edge portions located on one side of the plurality of internal electrodes, but does not cover a second portion of the pair of dielectric layers and the pair of side edge portions other than the first portion, and is in contact with a portion of the plurality of internal electrodes, and is mainly composed of nickel or copper, and The second metal layer covers the first metal layer and contacts at least a portion of the second portion located on one side of the first metal layer, and a main component of the second metal layer is tin.
2. A laminated ceramic electronic device comprising: An element body, comprising: a stacked body in which a plurality of internal electrodes and a plurality of dielectric layers are alternately stacked in a first direction, a pair of covering dielectric layers sandwiching the stacked body in the first direction, and a pair of end faces facing each other in a second direction, the plurality of internal electrodes being alternately exposed at the pair of end faces, the plurality of dielectric layers including a pair of side edge portions, the pair of side edge portions sandwiching the plurality of internal electrodes in a third direction perpendicular to the first direction and the second direction; and a pair of external electrodes, which respectively cover each end surface of the pair of end surfaces, wherein at least one of the pair of external electrodes comprises a first metal layer and a second metal layer, wherein, at the corresponding end surface of the element body, the first metal layer covers a portion of the plurality of internal electrodes and a first portion of the pair of dielectric layers and the pair of side edge portions located on one side of the plurality of internal electrodes, but does not cover a second portion of the pair of dielectric layers and the pair of side edge portions other than the first portion, and is in contact with a portion of the plurality of internal electrodes, and The second metal layer covers the first metal layer and contacts at least a portion of the second portion located on one side of the first metal layer, and the Young's modulus of the second metal layer is smaller than that of the first metal layer.
3. The multilayer ceramic electronic device according to claim 2, in, The main component of the first metal layer is nickel or copper, and Wherein, the main component of the second metal layer is tin.
4. The multilayer ceramic electronic device according to any one of claims 1 to 3, wherein The area of the first portion is not less than 1 / 10 and not more than 9 / 10 of the area of the second portion.
5. The multilayer ceramic electronic device according to any one of claims 1 to 3, wherein At least one of the pair of external electrodes does not cover other surfaces of the element body except for the corresponding end surface.
6. The laminated ceramic electronic device according to claim 5, wherein: The second metal layer extends to ends of the corresponding end surfaces.
7. The laminated ceramic electronic device according to claim 5, wherein: The second metal layer does not cover a third portion that is at least a portion of a peripheral edge portion of the corresponding end surface.
8. The laminated ceramic electronic device according to claim 7, wherein: The width of the third portion is less than 1 / 2 of the width of the second portion.
9. The multilayer ceramic electronic device according to any one of claims 1 to 3, wherein The pair of external electrodes each has the first metal layer and the second metal layer.