Method and apparatus for bonding chips

Through direct metal-metal solid bonding, the problem of increased chip thickness and use of additional materials caused by solder balls is solved, efficient chip communication and throughput improvement are achieved, and high-strength liquid-free bonding is achieved at low temperatures.

CN118737997APending Publication Date: 2024-10-01EV GRP E THALLNER GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410800033.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2017-03-02
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

In the existing technology, solder balls or copper pillars with solder caps increase the thickness of the chip, and additional materials are required during the soldering process, which affects chip communication efficiency and throughput.

Method used

Using the direct metal-metal solid bonding method, by cleaning the chip surface and performing self-alignment, direct bonding without liquid phase is achieved, reducing or eliminating dependence on solder, and improving bonding strength and efficiency.

Benefits of technology

It achieves smaller chip stacking thickness, improves chip communication efficiency and throughput, and achieves high-strength direct bonding at lower temperatures, avoiding liquid phase formation and the use of additional materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118737997A_ABST
    Figure CN118737997A_ABST
Patent Text Reader

Abstract

The invention relates to a method for bonding a chip (7) to a substrate (11 ') or to a further chip, characterized in that the chip (7) is bonded to the substrate (11') or to the further chip by direct bonding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method and a device for bonding chips. Background Art

[0002] The prior art describes the implementation of chip-to-wafer (C2W) or chip-to-chip (C2C) processes via solder balls or copper pillars with solder caps. However, the solder balls or copper pillars with solder caps are very large and increase the thickness of the resulting chip. Summary of the invention

[0003] It is therefore an object of the present invention to specify an improved bonding method or an improved bonding device or an improved product.

[0004] This object is solved by the subject matter of the parallel patent claims. Advantageous expansion schemes of the invention are described in the dependent claims. All combinations consisting of at least two of the features described in the specification, the claims and / or the drawings also fall within the scope of protection of the invention. In the case of the described value ranges, the values ​​within the mentioned limits should also be obviously regarded as limit values ​​and should be able to claim protection in any combination.

[0005] According to the present invention, a method for bonding a chip to a substrate, in particular a semiconductor substrate, or to another chip is provided, wherein the chips are bonded to the substrate or the other chip by direct bonding. Direct bonding is understood to be a bonding that is constructed directly via the interaction of two surfaces and does not form a liquid phase. According to another term definition, direct bonding is understood to be a bonding in which no additional material is required. Direct bonding is understood in particular to be a metal-metal solid bonding, in particular a diffusion bond, a pre-bond, or a fusion bond or a hybrid bond caused by a pre-bond, that is, a bond based on a fusion bond part and a metal bond part.

[0006] According to the invention, a device for bonding chips to a substrate or another chip is also provided, wherein the chips can be bonded to the substrate or another chip by direct bonding.

[0007] According to the invention, a chip stack is also provided which consists of chips, wherein the chips are bonded to one another by direct bonding.

[0008] According to the invention, a substrate (product) is also provided with chips, wherein the chips are bonded to the substrate by direct bonding.

[0009] According to the invention, direct bonding possibilities at the C2C or C2W level are enabled. Advantageously, solder balls or copper pillars with solder caps are no longer required. The thickness of the resulting chip stack or product becomes smaller, the throughput is increased and the efficiency of chip communication is increased. Direct bonding has in particular a thermal conductivity greater than 0.1 J / m 2 , preferably greater than 0.5 J / m 2 , and more preferably greater than 1.0 J / m 2 , most preferably greater than 2.0 J / m 2 , especially preferably greater than 2.5 J / m 2 The direct bonding is carried out in particular at a temperature of less than 400° C., preferably less than 300° C., more preferably less than 200° C., most preferably less than 150° C., and most preferably less than 100° C. Furthermore, the direct bonding is carried out without generating a liquid phase.

[0010] The idea behind the invention is to keep the surface of the chip clean so that the next direct bonding step can be performed. The chip prepared in this way, including the contamination-free bonding surface, can then be bonded to a substrate (C2W) or to another chip (C2C).

[0011] In the further course of the present disclosure, a substrate or semiconductor substrate is understood to be a semi-finished product of the semiconductor industry that has not yet been separated, in particular a round product. The substrate is particularly advantageously a wafer. The substrate can have any arbitrary shape, but is preferably round. The diameter of the substrate is in particular standardized by the industry. For wafers, diameters commonly used in the industry are 1 inch, 2 inches, 3 inches, 4 inches, 5 inches, 6 inches, 8 inches, 12 inches and 18 inches. However, according to embodiments of the present invention, in principle any substrate can be used, regardless of the diameter of the substrate.

[0012] In the further course of the disclosure, a chip is understood to be a mostly rectangular component obtained by separating a semiconductor substrate (wafer). A chip usually contains an integrated circuit which is formed during the processing of the semiconductor substrate.

[0013] In the present disclosure, a bonding surface is understood to be a surface which will become part of the bonding interface at a certain point during the process. In particular, a bonding surface is understood to be a surface of a chip which must be treated, in particular cleaned, according to the invention before the chip is bonded. If the chip is bonded to a substrate, the substrate surface may also be referred to as a bonding surface.

[0014] In a preferred embodiment, the bonding surface is a hybrid bonding surface. A hybrid bonding surface is understood to be a bonding surface that consists of a metal region and a dielectric region and thereby consists of a metal bonding surface portion and a dielectric bonding surface portion. Therefore, all methods and / or devices generally referred to in this disclosure that relate to direct bonding can be applied to the bonding of hybrid surfaces. Preferably, the metal surface portion and the dielectric surface portion are located in one plane as far as possible. In particular, the metal surface portion is recessed relative to the dielectric surface portion or protrudes relative to the dielectric surface portion by less than 0.5 μm, preferably less than 100 nm, more preferably less than 50 nm, and most preferably less than 10 nm.

[0015] Cleaning Methods

[0016] In the further disclosure, cleaning is understood to be the removal of contamination from the bonding surface by one and / or more of the following methods:

[0017] ● Wet chemical cleaning, especially

[0018] ○ Use water, especially

[0019] ■Water containing CO2

[0020] ○ Use alcohol

[0021] ○ Use acid, especially

[0022] ■Formic acid

[0023] ■Citric acid

[0024] ■Peroxymonosulfate

[0025] ●Standard Cleaning 1 (SC1)

[0026] -Standard Clean 2 (SC2)

[0027] ○ Use alkali, especially

[0028] ■NH4OH

[0029] Plasma cleaning

[0030] Plasma ashing

[0031] ● Mechanical cleaning, especially

[0032] ○Brush.

[0033] Plasma cleaning is understood to be the bombardment of a surface with the ionized part of a plasma, generally with high energy. In this case, the ions of the plasma are accelerated by electric and / or magnetic fields and have a non-negligible penetration depth. Plasma cleaning can be accompanied by plasma activation of the surface.

[0034] Plasma ashing is understood to be a cleaning process for organic matter on the surface, generally a low-energy cleaning process. Cleaning is achieved here, in particular, by oxidation of organic matter, in particular with oxygen and / or fluorine or any other suitable and ionizable oxidant. Preferably, the organic components oxidized by plasma ashing are discharged from the reaction chamber. This is achieved either by the continuous flow of plasma or by continuous gassing and exhausting of the plasma chamber. However, in a more preferred embodiment, the ashed and oxidized organic components are bonded within the plasma chamber by chemical and / or physical methods to prevent these organic components from returning to the substrate surface. Thus, complex devices based on the circulation of plasma are avoided.

[0035] Optionally, after the plasma ashing, wet chemical cleaning is performed with one or more of the liquids mentioned above in order to thereby further improve the cleanliness of the surface and / or the surface chemistry of the surface to be cleaned, in particular by terminating the surface with suitable substances known to those skilled in the art to optimize the cleanliness of the surface and / or the surface chemistry of the surface to be cleaned. Advantageously, the method serves to remove particles, in particular particles formed and / or remaining on the surface during the plasma ashing.

[0036] Therefore, the cleaning of the bonding surface can also be performed by a plurality of the methods mentioned. The cleaning can be performed on one chip or on a plurality of chips simultaneously. In particular, the individual chips can be cleaned during transport between two stages.

[0037] Self-alignment

[0038] In a preferred embodiment, the chip is positioned and self-alignment of the chip is performed. Self-alignment is understood to be a positioning process of an object, in the present case a chip, driven by the physical laws of minimization.

[0039] Self-alignment is preferably achieved by driving the chip onto the bonding surface with minimal stiction, particularly due to liquid deposited on the bonding surface, into a position between, particularly in the center of, features of the bonding surface.

[0040] For example, it is conceivable that, for example, four metal areas, in particular metal bonding surfaces such as contact pads, are located on the bonding surface, in particular as parts or channels of a hybrid bonding surface. The chip also has four areas on its bonding surface. If such a chip is placed on a liquid, the starting point should be that the more hydrophilic areas will be positioned above the more hydrophilic areas, and the more hydrophobic areas will be positioned above the more hydrophobic areas. Thus, an alignment will occur in which the metal areas of the hybrid bonding surface will be covered.

[0041] It is clear to those skilled in the art that the higher the symmetry of the structure participating in self-alignment, the better this self-alignment can be achieved. This includes the geometry of the chip, the distance between the metal areas of the hybrid bonding surface, the shape of the metal areas, etc. Preferably, the chip should be square. In addition, the metal areas of the hybrid bonding surface should preferably also be located at the corners of the envisioned square. If the difference between the hydrophilicity and the hydrophobicity of the corresponding hybrid bonding area is as large as possible, there will be another advantage. The contact angle constructed between the test droplet, especially water and the surface to be measured is a measure of hydrophilicity or hydrophobicity. The hydrophilic surface flattens the droplet because the adhesion between the liquid and the surface exceeds the cohesion of the liquid and dominates, and therefore forms a small contact angle. The hydrophobic surface causes the spherical morphology of the droplet because the cohesion of the liquid exceeds the adhesion between the liquid and the surface and dominates. Preferably, the contact angle difference between the two different mentioned hybrid bonding areas is greater than 1°, preferably greater than 5°, more preferably greater than 25°, most preferably greater than 50°, and most preferably greater than 100°.

[0042] The layer of liquid applied to the bonding surface has a thickness of less than 2 mm, preferably less than 1.5 mm, even more preferably less than 1 mm, most preferably less than 0.5 mm, and most preferably less than 0.1 mm. The liquid is preferably water. However, it is also conceivable to use any other liquid, such as

[0043] ●Alcohol

[0044] Ether

[0045] ●Acid

[0046] ●Alkali.

[0047] In particular, ethers have a very high vapor pressure and therefore evaporate from the surface with little residue, which automatically leads to the removal of the liquid after the self-alignment has been achieved. Advantageously, a pre-bond is automatically formed between the surfaces after the removal of the liquid.

[0048] In a special embodiment according to the invention, recesses are provided on the bonding surface of the substrate and / or chip, in particular in the dielectric region, which facilitate or enable the removal of the liquid after the self-alignment of the chip. These recesses preferably lead from the region of the chip surface to the edge of the chip, so that the liquid can be removed outwards by flow and / or evaporation, preferably automatically, more preferably with the aid of gravity, which causes the liquid to be pressed out.

[0049] Bonding device and bonding method

[0050] A plurality of devices and processes for bonding chips according to the invention are disclosed. The method according to the invention can be divided into individual bonding methods and collective bonding methods. Therefore, the corresponding device is a device for individual bonding or for collective bonding. What all methods and devices according to the invention have in common is that the bonding surface of the chip must be free of contamination until the bonding process. The process steps and equipment according to the invention for achieving this goal are described in more detail below.

[0051] Individual bonding device and individual bonding method

[0052] Individual bonding methods are understood to be processes common in the prior art for placing chips individually, that is, one after another, on other chips (C2C) or on a wafer (C2W). This method has the advantage that chips of different sizes and / or different functions can be bonded.

[0053] Separation on tape

[0054] In an exemplary first method according to the invention, the substrate is fixed on a carrier, in particular an adhesive tape, and there it is separated into chips. In the further course of the disclosure, the adhesive tape is used as an exemplary example. However, it is also conceivable to use a rigid carrier. Therefore, the chips are not produced until the substrate has been successfully fixed on the adhesive tape.

[0055] In the first process step of the method, the carrier, in particular the adhesive tape, is fixed to a fixing frame, in particular a dicing frame. If the carrier is a rigid carrier, this process step can be omitted or the rigid carrier can be fixed to a substrate holder / carrier holder.

[0056] In an optional second process step, the bonding surface of the substrate is cleaned, from which the later bonding surface of the chip is formed. The cleaning can be one of the cleaning methods already mentioned. In particular, the cleaning is achieved by plasma and / or liquid and / or gas. Additionally, the plasma treatment preferably results in plasma activation of the bonding surface. The bonding surface must only be cleaned if the bonding surface has been soiled by a previous process, so that contamination is also transferred to the adhesive tape or there is contamination that will later prevent and / or hinder the construction of direct bonding. However, the cleaning of the bonding surface of the substrate is preferably always performed before fixing.

[0057] In the third process step according to the invention, the substrate is fixed to a carrier with its, in particular, cleaned, preferably plasma-activated, bonding surface. In this case, according to the invention, the adhesive tape is designed such that contamination of the bonding surface is as small as possible after the substrate has been removed from the carrier. If the carrier is a rigid carrier, it may be necessary to provide the carrier surface with a protective layer before the substrate is fixed. In the case of adhesive tapes, such a protective layer is usually already present.

[0058] Furthermore, from the point in time of contact with the bonding surface, the carrier also serves as a protection for the bonding surface and prevents contamination of the bonding surface. Preferably, the carrier is coated at least in the center of the substrate for the most part, so that there is low adhesion between the bonding surface of the substrate and the carrier, while the carrier can definitely have adhesive properties in the peripheral area of ​​the substrate. Areas of high adhesion strength, i.e. areas with higher adhesion, can potentially cause contamination in the periphery of the substrate, which can preferably be ignored as long as it does not involve areas of the bonding surface from which the chip is later manufactured. Preferably, the adhesive tape is designed so that the adhesion is reduced due to the input of energy into the adhesive tape (UV, heat), and this makes it easier to remove the chip later. Such adhesive tapes are known in the prior art.

[0059] However, preferably, in particular low-contamination adhesive tapes are used for the process according to the invention.

[0060] The adhesive tape preferably has an adhesive which cannot penetrate into the bonding surface, in particular into the reservoir which is produced as a result of the previously performed plasma activation. Preferably, this is ensured in the following manner: the adhesive has a very high viscosity which prevents penetration into the nanoporous surface. Still more preferably, the molecules of the adhesive are so large that penetration into the pores is not possible due to the large size of the molecules. These pores are in particular less than 10 nm, still more preferably less than 5 nm, most preferably less than 1 nm, still more preferably less than 0.5 nm, and most preferably less than 0.2 nm. The pore size is also disclosed in WO2012100786A1. Most preferably, the adhesive is a solid bonded in a polymer matrix. Preferably, by this form of the adhesive, cleaning with a solvent can be omitted after the adhesive tape is removed, and this prevents the solvent from being embedded in the reservoir which is produced due to the plasma activation on the surface of the bonding surface. This leads to an improved bonding result, since the escape of solvent after bonding and thus the formation of bubbles in the bonding interface can be prevented.

[0061] The production of such a reservoir is disclosed in publications WO2012100786A1, WO2012136267A1, WO2012136268A1, WO2012136266A1 and WO2014015899A1.

[0062] In a very preferred embodiment according to the invention, however, the carrier is coated in such a way that it can hold the substrate over its entire surface, without leaving any contamination on the substrate and the chips produced later can be easily removed.

[0063] In a fourth process step according to the invention, the substrates are separated. The separation can be performed by any arbitrary method, as long as the method does not dirty the bonding surface. In the further course of the present disclosure, some separation methods will be discussed in more detail, with the help of which the cleaning according to the invention of the bonding surface during the separation is ensured.

[0064] In the fifth process step according to the invention, the separated chip is removed from the carrier by a machine, in particular a chip bonder. In a particularly preferred embodiment according to the invention, the bonding surface of the chip is continuously, in particular continuously, cleaned during the removal of the chip and / or during the transport of the chip to other locations, in particular bonding locations. The cleaning is preferably achieved using plasma. Here, the chip is either removed from the carrier through an area in which the cleaning occurs, or in a space in which the cleaning properties are automatically achieved. Thus, for example, it is conceivable that the chip is removed from the carrier in a plasma chamber of a chip bonder. More preferably, the chip is moved through an atmospheric plasma source after being removed from the carrier. In particular, oxygen plasma is used, which preferably leads to ashing of residues.

[0065] In the sixth process step according to the invention, the bonding surface of the transported, separated chip is bonded to the second bonding surface by bonding, in particular direct bonding or hybrid bonding. The bonding process is preceded by an alignment process of the chip relative to the second bonding surface to which the chip is to be bonded, an alignment process which is generally performed relatively smoothly. In other areas of the present disclosure, the improvement according to the invention with respect to optimal bonding is mentioned in more detail: the alignment process preferably lasts less than 5 seconds, more preferably less than 2 seconds, most preferably less than 1 second.

[0066] Methods used for separation

[0067] An important aspect of the embodiments according to the invention is to keep the bonding surfaces of the substrate or the chip separated therefrom clean. In order to ensure the cleanliness of the bonding surfaces, the separation process must also cause as little contamination as possible. In particular, burrs must not be allowed to form when separating the substrates. According to the invention, this can be ensured by a number of different processes.

[0068] In the first possible process, so-called stealth dicing, a focused laser beam changes the material properties so that the chips can be easily separated. The advantage is that mechanical separation devices such as cutting wheels are omitted. The basic operating principle of the stealth dicing process is known in the prior art.

[0069] In a possible second process, the chips are separated from each other by using plasma.

[0070] In a possible third process, the chips are separated from each other by using a mechanical separation device. Here, in a very preferred embodiment according to the invention, gaps are produced on the bonding side before the optional cleaning of the bonding surfaces and the fixing of the substrate on the carrier. During the separation process from the rear side of the substrate, the mechanical separation device then encounters the pre-made gaps. Thereby, these gaps prevent contamination of the bonding surfaces of the individual chips by allowing the mechanical separation device to reach the empty space in advance.

[0071] These gaps can preferably also be used in the above-mentioned separation methods, since these separation methods can also lead to contamination and / or burrs at the edges. This is especially true if the break, especially during stealth dicing, does not extend vertically through the wafer, for example due to the layer structure of the chip. The gaps are provided in particular to at least avoid the formation of burrs on the bonding surface.

[0072] These gaps may also be the result of a masking process that is used to deposit material on the surface. In this process, no material is deposited at the masked locations. The masked areas then form these gaps.

[0073] Collective bonding device and collective bonding method

[0074] In certain situations, it may be disadvantageous to bond the chips by a separate bonding method. In particular, when the bonding surfaces of the chips must be cleaned in order to achieve a high bonding quality, it may be advantageous to first place all the chips on a carrier so that the later bonding surfaces point upward. In this preliminary fixation, all the bonding surfaces of the chips can then be cleaned and pretreated simultaneously, in particular in a machine provided for this purpose. In a further process step, all the chips are then bonded simultaneously to the substrate to be actually bonded or the chip to be actually bonded.

[0075] The quality feature that must be met primarily in the case of such collective bonding is the flatness of the bonding plane formed by all bonding surfaces of all chips. In the ideal case, the bonding surfaces of all chips must all coincide with one another.

[0076] Temporary carrier

[0077] The following process describes the production of a temporary carrier with a plurality of chips whose bonding surfaces coincide with each other in order to perform a collective bonding process.

[0078] In a first process step according to the invention, a first carrier, in particular a carrier substrate, most preferably a carrier wafer, and even more preferably an adhesive tape, is coated with a protective layer on a dicing frame. In particular, when using an adhesive tape, it is conceivable that the protective layer is already applied to the adhesive tape. In other cases, the coating of the carrier can be carried out using common, known coating methods, such as spin coating, spray coating, lamination, etc.

[0079] Alternatively, it is also conceivable to provide the surface of the chip with a protective layer. This can be done even before the chips are cut out of the wafer.

[0080] In the second process step according to the invention, a plurality of chips are fixed on a first carrier with high alignment accuracy. In particular, the alignment is performed with the aid of alignment marks and an optical system. Here, the alignment accuracy is better than 1 mm, preferably better than 100 μm, more preferably better than 10 μm, most preferably better than 1 μm, and most preferably better than 100 nm.

[0081] The fixing is carried out via the later bonding surface of the chip. The bonding surfaces of the chips should overlap each other as much as possible. In addition, the protective layer should be as thin as possible, have as little viscosity as possible and have as high elasticity as possible in order to prevent the chips from penetrating into the layer to different depths and destroying the overlap of the bonding surfaces of the chips. The thickness of the protective layer should preferably be as small as possible in order to eliminate the elastic properties as much as possible. The first carrier thus acts as an infinitely hard resistance and the protective layer acts only as a separator between the bonding surface and the first carrier.

[0082] The elastic modulus of the adhesive tape is between 1 GPa and 1000 GPa, preferably between 1 GPa and 500 GPa, more preferably between 1 GPa and 100 GPa, most preferably between 1 GPa and 50 GPa, and most preferably between 1 GPa and 20 GPa. For example, the elastic modulus of polyamide is between 3 GPa and 6 GPa.

[0083] Here, the elastic modulus of the harder carrier is between 1 GPa and 1000 GPa, preferably between 10 GPa and 1000 GPa, more preferably between 25 GPa and 1000 GPa, most preferably between 50 GPa and 1000 GPa, and most preferably between 100 GPa and 1000 GPa. For example, the elastic modulus of some steel grades is around 200 GPa.

[0084] In the third process step according to the invention, a second carrier, in particular a carrier substrate, most preferably a carrier wafer, is coated with an adhesive. The second carrier is a temporary carrier. In contrast to the protective layer from the second process step according to the invention, the adhesive should have elastic and / or plastic adaptability in order to compensate for possible height differences of the chips so that the overlap of the bonding surfaces of the chips is not lost. Therefore, the adhesive should have as little stickiness as possible and the possibility of permanent deformation.

[0085] At room temperature, the viscosity of the adhesive is between 10E6 mPa*s and 1 mPa*s, preferably between 10E5 mPa*s and 1 mPa*s, still more preferably between 10E4 mPa*s and 1 mPa*s, most preferably between 10E3 mPa*s and 1 mPa*s.

[0086] In the fourth process step according to the present invention, the back side surface of the chip opposite to the bonding surface of the chip is connected to a temporary carrier. Here, the overlap of the bonding surface of the chip is maintained on the first carrier side, and the back side surface makes the adhesive on the temporary carrier deform accordingly if necessary, especially the adhesive on the temporary carrier deforms accordingly due to the preferably low viscosity. Therefore, after the bonding process, the thickness of the adhesive between the chip and the temporary carrier can vary from chip to chip. In an extension scheme according to the present invention, it is possible to remove the adhesive between the chips. The alignment between the first carrier and the temporary carrier is preferably achieved by the alignment marks located on the first carrier and the temporary carrier. It is also conceivable that: the alignment marks are located on the surface of the chip and these alignment marks are aligned with the alignment marks on the temporary carrier. The aligner (English: aligner) for aligning the substrate is described in detail in the published documents US6214692B1, WO2015082020A1, and WO2014202106A1.

[0087] In the fifth process step according to the invention, the first carrier with the protective layer is removed. Therefore, the adhesion between the adhesive, the temporary carrier and the chip is in particular higher than the static friction between the protective layer and the bonding surface of the chip. In a particularly preferred embodiment according to the invention, the protective layer is designed so that the detachment of the bonding surface of the chip is carried out without contamination, in particular completely without contamination. If the first carrier is an adhesive tape, the tape can be peeled off, which makes removal easier. It may also be necessary to change the protective layer chemically or with respect to mechanical properties by means of chemicals and / or electromagnetic radiation, in particular UV light, visible light or infrared light and / or heat, so that the protective layer loses or at least reduces its adhesive properties.

[0088] Here, the bonding strength between the protective layer and the chip is less than 1J / m 2 , preferably less than 0.1 J / m 2, and more preferably less than 0.01 J / m 2 , most preferably less than 0.001 J / m 2 , especially preferably less than 0.0001 J / m 2 .

[0089] In the optional sixth process step, in particular the exposed bonding surfaces of the chips are cleaned and / or plasma activated simultaneously. This measure is important in particular when the removal of the first carrier from the bonding surfaces of the chips is not completely contamination-free. In particular, the cleaning of all chips can be carried out simultaneously at this time, which increases the throughput of the method according to the invention.

[0090] Then, in the seventh process step according to the invention, the bonding process of all chips fixed on the temporary carrier is carried out simultaneously on the product substrate, in particular the wafer. This also includes the possibility of bonding the chips on the temporary carrier to the chips already on the product substrate. Thus, the possibility of gradually constructing the chip stack on the product substrate is provided. The alignment between the temporary carrier and the product substrate is preferably achieved by alignment marks located on the carrier and the product substrate. It is also conceivable that the alignment marks are located on the bonding surface of the chip and these alignment marks are aligned with the alignment marks on the product substrate.

[0091] In an eighth process step according to the invention, the temporary carrier is removed from the chip. It may be necessary to change the adhesive chemically or with respect to mechanical properties, especially viscosity, by means of chemicals and / or electromagnetic radiation, in particular UV light, visible light or infrared light and / or heat, so that the adhesive loses its adhesive properties. Particularly preferably, the temporary carrier is a carrier that is transparent to photons from a specific wavelength range of the EM spectrum. Preferably, it is a glass carrier. Thus, according to the invention, an adhesive can be used that can be destroyed from the rear side by means of a laser, so that the possibility of debonding the temporary carrier from the rear side of the temporary carrier is possible.

[0092] In the ninth process step according to the invention, the adhesive on the rear surface of the chip is cleaned by one of the cleaning methods mentioned. After this process step, any other chips can be stacked on the existing chips to construct a chip stack on the product substrate.

[0093] Preferably, the positioning accuracy of the chip on the first carrier according to the second process step and the positioning of the chip on the temporary carrier by the collective bonding process according to the seventh process step can be achieved or at least assisted by self-alignment of the chip. Here, the positioning accuracy is better than 1 mm, preferably better than 100 μm, more preferably better than 10 μm, most preferably better than 1 μm, and most preferably better than 100 nm. Assistance by self-alignment is only achieved when a lateral movement of the chip relative to the first carrier and / or relative to the temporary carrier is possible. To this end, the protective layer on the first carrier and / or the adhesive on the temporary carrier must have a correspondingly small shear modulus or must even be able to achieve plastic deformation so that the chip can be moved laterally.

[0094] Fixed carrier

[0095] Instead of using the temporary carrier just mentioned, it is conceivable to fix the chip on a fixing carrier which has corresponding fixing elements. These fixing elements can be

[0096] Vacuum fixing parts

[0097] ●Electrostatic fixing parts

[0098] Magnetic fixings

[0099] Gel pack fastener

[0100] The chips can be fixed directly with their rear surfaces on the fixing carrier. The disadvantage is that, in contrast to the temporary carrier mentioned, there is no adhesive with which the bonding surfaces of all chips can be unified in one plane. The elasticity of the gel pack of the gel pack holder mentioned can at most achieve a similar effect. The ejection device described later can also be used as a fixing carrier.

[0101] Ejector

[0102] In the further course of the disclosure, a number of devices and methods are described, in which the picking up and fixing of chips is required. Therefore, all disclosed methods and devices relate to already separated chips and the handling of these chips, which, according to the invention, should always be carried out in such a way that the bonding surfaces are as far as possible no longer contaminated. These embodiments, which are called ejection devices, have the following tasks in particular: to fix a number of already separated chips in order to carry out a cleaning process on these chips and to prepare the bonding surfaces of these chips for the actual bonding process.

[0103] Ejector with recessed design

[0104] In order to process the bonding surface of the chip and to feed it directly to the bonding process, the first ejection device according to the invention is to place the chip in a carrier having a recess in which the chip can be positioned and / or fixed.

[0105] In a preferred embodiment, the contour of the recess is exactly the same as the contour of the chip. In another variant according to the present invention, the contour of the recess may also be different from the contour of the chip. In particular, the recess is larger than the chip. This facilitates the entry of the cleaning fluid and / or plasma into one side of the chip. Here, the distance between the contour of the chip and the contour of the recess is less than 5 mm, preferably less than 1 mm, more preferably less than 0.5 mm, most preferably less than 0.1 mm, and most preferably less than 0.05 mm.

[0106] On the bottom surface of the depression there is a channel (hereinafter also referred to as a sleeve), in particular a hole, through which a lifting device can lift the chips so that they can be touched by a fixture (hereinafter also referred to as a chuck). In a particularly preferred embodiment according to the present invention, the height of the chip corresponds exactly to the depth of the depression. Thereby, the bonding surface to be cleaned coincides with the carrier surface. This embodiment is particularly helpful for the mechanical cleaning process. Because the chips do not extend from the depression, these chips cannot be mechanically damaged. In addition, these chips are not sunken in the depression and can therefore be optimally reached by all types of cleaning equipment. In addition, the embodiment according to the present invention is optimally suitable for plasma cleaning of the chip, because the uniformity of the plasma used is very high due to the seamless flatness generated between the bonding surface and the carrier surface. Due to the high uniformity, high reproducibility of the bonding surface and especially uniform cleaning of the bonding surface, especially uniform plasma activation, are ensured.

[0107] All carriers used in the plasma chamber specified in this disclosure should have specific characteristics. In particular, these carriers must be composed of conductive materials. Therefore, these carriers are preferably composed of the following materials:

[0108] ●Electrics, especially

[0109] ○Metals, especially

[0110] ○ Alloys, especially

[0111] -steel

[0112] Aluminum

[0113] ■Stainless steel alloy

[0114] Titanium

[0115] ○ Conductive ceramics, especially

[0116] ■Doped SiC

[0117] ■Doped Si3N4

[0118] The metal carrier is preferably coated in order to prevent contamination of the chip by the metal. Dielectrics, in particular oxides, nitrides or carbides, are preferably used as coatings.

[0119] The carrier is preferably also made of two parts, so that the chip rests on a metal sheet and then a mesh is laid on for plasma activation, which consists of a dielectric, in particular Si, SiC or Si3N4. In this case, the mesh has similar or identical dielectric properties as the chip. Thus, a plasma that is as uniform as possible can be ensured. In particular, the mesh even consists of the same dielectric material as the chip.

[0120] The absolute value of the difference between the chip height h and the depth t of the recess is less than 1 mm, preferably less than 0.5 mm, even more preferably less than 0.1 mm, most preferably less than 0.05 mm, and most preferably less than 0.01 mm.

[0121] By means of the embodiments according to the present invention, the bonding surfaces of a plurality of chips can be processed simultaneously, which leads to a significant improvement in the efficiency of cleaning the already separated chips.

[0122] After the chip has been ejected to a clearly defined height, a chuck is used to pick up and transport the chip. In this case, the chuck does not hold the chip on the bonding surface that has just been cleaned, but on a fixing surface that is opposite to the bonding surface. The fixing surface can be contaminated in particular during these process steps. However, in other process steps, this fixing surface can become a new bonding surface on which other chips can be placed and must then be cleaned accordingly.

[0123] In the case of the described ejection device, the depth t of the recess is predetermined. If chips with slightly different chip heights h are fixed according to the invention, the bonding surfaces of these chips to be cleaned no longer coincide with each other. In this case, it is conceivable that the lifting device performs a height correction for some chips, in particular for chips whose chip height h is smaller than the depth t of the recess.

[0124] Ejector with accessory design

[0125] Another second ejection device according to the invention consists of a carrier in which there are channels, in particular holes. In contrast to the previous first ejector design, this ejection device has no recesses. The chip to be cleaned is fixed directly on the carrier surface. The surrounding atmosphere is separated from the channel, in particular by means of a seal. This makes it possible to clean the chip without contaminating the channel due to cleaning agents, such as chemicals, such as liquids or ions from plasma. The fixing elements that fix the chip can be located within the sealed space. These fixing elements are at least one of the following fixings:

[0126] ●Vacuum fixing (preferred)

[0127] ●Electrostatic fixing parts

[0128] Magnetic fixings

[0129] ●Adhesive fixings,

[0130] Mechanical fasteners (least preferred)

[0131] Most preferably, a vacuum fixture is used, which can evacuate the space between the channel and the seal and thus cause the chip to be pressed against the seal. These seals can either be solid, especially polymers, or can be especially highly viscous and / or time-hardening polymers. Then, these seals are preferably waxes, adhesives, glues, etc. These polymers need to be replaced regularly because they are removed over time, especially due to the cleaning process performed.

[0132] Mask

[0133] In one embodiment of the invention, in particular for the ejection device mentioned, a mask with apertures is used to protect the bonding surfaces of the chips from contamination. The chips are always gripped by machine components, which must necessarily be moved over the chips. In addition to the actual gripper and the corresponding arm at one end of the gripper, cables and wires must also be moved. When all these machine elements are moved over the chips, they inevitably contribute to the contamination of the bonding surfaces of the chips.

[0134] In a particularly preferred embodiment according to the present invention, a relative movement between a mask with apertures and a chip is achieved. Preferably, the device on which the chip is located moves. It is also conceivable that the mask moves. In order to remove the chip, the aperture is positioned above the chip to be removed. The lifting device lifts the chip to be bonded over the mask. On the upper side of the mask, the chuck removes the chip through the rear surface of the chip without touching the bonding surface of the chip, and transports the chip to a position for further processing. In particular, the alignment mark of the chip is detected by the first optical system as a next step. Then, the chip is moved below the position to be bonded, and then is positioned and bonded with high precision relative to the position to be bonded, especially by means of the second optical system. Therefore, according to the present invention, it is possible that the position where the chip is bonded is far outside the chip removal. The chip can also go through multiple stages, especially alignment and / or measurement and / or cleaning and / or testing stages, etc., until the actual bonding process. According to the present invention, during the entire chip transportation, only the rear surface of the chip is touched, and the bonding surface of the chip is never touched. The collet thus preferably holds the chip in place from the point in time when the lifting device is removed until the bonding is complete.

[0135] In a special embodiment, the product substrate on which the chip is to be bonded is located directly above the chip to be bonded. All other chips and thereby the bonding surfaces of these chips are protected from contamination by the mask surface. The ejector removes the chip from the ejector device and bonds the chip directly to the product substrate or to the chip / chip stack directly bonded to the product substrate. Here, the bonding surface of the product substrate or the chip of the product substrate is directly facing the ejector and therefore points in the direction of gravity. The mask prevents contamination of the bonding surface of the chip that is still to be ejected on the ejector device. Compared with the above-mentioned embodiment in which the chuck transports the chip to another location and bonds the chip there, this embodiment according to the invention is less preferred because no other process steps can be performed on the chip in this variant.

[0136] For all embodiments, the mask itself must be free of contamination. In particular, the mask can be cleaned between assembly processes using one of the cleaning methods mentioned. The mask according to the invention is mainly used for bonding processes, in which the substrate to be equipped with the chip is placed with the bonding surface of the substrate in the direction of gravity. In this case, the mask according to the invention prevents the transfer of contamination of the substrate to the chip located below the substrate or the transfer of contamination of moving machine elements to the chip located below the substrate. These masks are used in particular in conjunction with the ejection device described in detail in the present disclosure. In these embodiments, in particular, the rotation of the chips and thereby the contacting of the chips on their bonding surfaces can be omitted. The exact embodiments are explained in detail elsewhere in the present disclosure and in the drawings and the associated figure descriptions.

[0137] Furthermore, there is a top-down flow in the clean room. Therefore, the air always circulates from a higher position to a lower position and attracts dust particles there. The flow direction also has a negative influence on the contamination of the bonding surfaces. According to the invention, it is conceivable that machines are arranged near the device in which a plurality of chips are fixed with exposed bonding surfaces, in particular in the mentioned ejection device or the fixing carrier, which machines generate a lateral flow in order to remove dust particles laterally.

[0138] Bonding head

[0139] In another embodiment according to the present invention, a fixture for fixing and bonding a chip is described. The fixture is also referred to as a bonding head (English: bondhead) and describes the following machine component, which is responsible for fixing, transporting and bonding a single chip to a bonding surface. In order to be able to fully utilize the advantages of the clean bonding surface on the chip according to the present invention, it is necessary to control the bonding process as much as possible. In particular, it is absolutely necessary that the chip is not first bonded at the edge, but that the bonding wave propagates outward from the center of the chip. The concept of bonding waves is already known to those skilled in the art from wafer-to-wafer (English: W2W) bonding. Here, refer to the publications WO2014191033A1, PCT / EP2016053268, PCT / EP2016056249 and PCT / EP2016069307, just to name a few examples.

[0140] However, in contrast to the W2W method mentioned, the C2W method has an extremely high throughput. The fixture moves at extremely high speed from the pick-up position of the chip to the bonding position and back. Since the high speeds have to be reached quickly, the acceleration is also relatively high. In particular, the acceleration in the z direction, that is to say perpendicular to the bonding surface, is also high. This desired physical fact can be used to construct a completely new fixture, with the help of which the chip can be deformed convexly based solely on inertia, in order to ensure that the center of the bonding surface of the chip first contacts the second bonding surface.

[0141] The idea according to the invention is that the fixing device has spring elements at the periphery whose spring constant is smaller than the spring constant of the spring elements located in the center. In a very special embodiment according to the invention, the fixing surface is completely unsupported at the periphery, that is to say, the spring elements are omitted at the periphery.

[0142] Here, the ratio of the spring constant of the peripheral spring elements to the spring constant of the centrally located spring element is less than 1, preferably less than 0.1, even more preferably less than 0.01, most preferably less than 0.0001, particularly most preferably less than 0.00001. BRIEF DESCRIPTION OF THE DRAWINGS

[0143] Further advantages, features and details of the present invention are obtained from the following description of preferred embodiments and with reference to the accompanying drawings. In particular:

[0144] Figure 1a A first process step according to the invention is shown,

[0145] Figure 1b A second process step according to the invention is shown according to the first process according to the invention,

[0146] Figure 1c A third process step according to the invention is shown according to the first process according to the invention,

[0147] Figure 1d A fourth process step according to the invention is shown according to the first process according to the invention,

[0148] Figure 1e A fifth process step according to the invention of the first process according to the invention is shown,

[0149] Figure 1f A sixth process step according to the invention of the first process according to the invention is shown,

[0150] Figure 1g shows a seventh process step according to the invention of the first process according to the invention,

[0151] Figure 2a The first process steps according to the invention are shown for the second process according to the invention,

[0152] Figure 2b The second process steps according to the invention are shown,

[0153] Figure 2c A third process step according to the invention is shown according to the second process according to the invention,

[0154] Figure 2d A fourth process step according to the invention is shown according to the second process according to the invention,

[0155] Figure 2e A fifth process step according to the invention is shown according to the second process according to the invention,

[0156] Figure 2f A sixth process step according to the invention of the second process according to the invention is shown,

[0157] Figure 2g A seventh process step according to the invention is shown according to the second process according to the invention,

[0158] Figure 2h An eighth process step according to the invention of the second process according to the invention is shown,

[0159] Figure 2i The ninth process step according to the invention of the second process according to the invention is shown,

[0160] Figure 3 A first ejection device according to the present invention is shown,

[0161] Figure 4 A second ejection device according to the present invention is shown,

[0162] Figure 5 shows a mask according to the invention with apertures in a first embodiment according to the invention,

[0163] Figure 6 shows a mask according to the invention with apertures in a second embodiment according to the invention,

[0164] Figure 7a The first process step of the self-alignment according to the present invention is shown,

[0165] Figure 7b The second process step of the self-alignment according to the present invention is shown,

[0166] Figure 8ashows a first process step according to the invention of a bonding process using a bonding head according to the invention,

[0167] Figure 8b The second process step according to the invention of a bonding process using a bond head according to the invention is shown.

[0168] In the figures, identical components or components with identical functions are denoted by the same reference numerals. DETAILED DESCRIPTION

[0169] Figure 1a The first process step according to the invention of the first process according to the invention is shown for producing the final product 19 after the first process according to the invention. All preparations for producing a plurality of chips are carried out on the substrate 11. These preparations include all functional features of the manufactured chips, in particular the contacts 13. In addition, the gaps 12 can be pre-cut in order to facilitate the later separation process. Due to all the preparation steps carried out, the bonding surface 7b may have been contaminated.

[0170] Figure 1b The second process step of the first process according to the invention is shown, namely the step of cleaning the bonding surface 7b. In particular, the bonding surface 7b is cleaned and / or activated by plasma and / or wet chemical methods.

[0171] Figure 1c The third process step of the first process according to the invention is shown, in which the substrate 11 is fixed to a carrier, in particular an adhesive tape 15. The adhesive tape surface 15o is preferably constructed such that the substrate 11 is fixed via the bonding surface 7b, but the later removal of the adhesive tape 15 leaves no residue on the bonding surface 7b.

[0172] Figure 1d The fourth process step of the first process according to the invention is shown, in which the substrate 11 is separated into individual chips 7. According to the invention, the bonding surfaces 7b of the chips 7 must not be contaminated here. Therefore, preferably, in particular in the case of mechanical separation by a separation device 16, a gap 12 is provided in the substrate 11 so that the separation process can already be ended above the bonding surface 7b. It is also conceivable that the separation is carried out by laser, in particular by known stealth technology, by chemicals, in particular by etching, preferably by dry etching, by plasma, etc.

[0173] Figure 1e The fifth process step of the first process according to the invention is shown, in which the chip 7 is removed from the tape 15 by the bonding head 9 on which the fixture 6 is located. Here, the bonding head 9 fixes the chip 7 on the back side surface 7r of the chip so that there is no contamination on the bonding surface 7b.

[0174] Figure 1f The sixth process step of the first process according to the invention is shown, in which the bonding head 9 is bonded to the further substrate 11' after the chip 7 has been aligned relative to the further substrate 11'. Here, the bonding surface 7b is preferably a hybrid surface, which consists of a dielectric surface area 20 and an electrical surface area represented by the contact 13. In the case of such a hybrid bonding surface, a so-called pre-bonding is performed between the dielectric surface area 20 of the bonding surface 7b of the chip 7 and the dielectric surface area 20' of the substrate 11'.

[0175] Figure 1g The final product 19 according to the invention is shown according to the first process according to the invention, which consists of a substrate 11 ′ and a plurality of chips 7 . It is conceivable to repeat the mentioned process steps in order to stack further layers of chips 7 onto the first layer of chips 7 .

[0176] Figure 2a The first process step according to the invention of the second process according to the invention is shown, wherein a plurality of already separated chips 7 are fixed to a carrier, in particular a tape 15, with a bonding surface 7b. The bonding surface 7b of the chip 7 must have been cleaned and / or activated in a previous process. Preferably, the chip 7 is aligned and positioned by a bonding head 9 of a chip bonder. The enlarged view shows the interface between the bonding surface 7b of the chip 7 and the tape surface 15o of the tape 15. There may be a protective layer 17 on the tape surface 15o, which preferably also has adhesive properties. However, it is particularly preferred that the adhesive properties between the protective layer 17 and the tape surface 15o are greater than the adhesive properties between the protective layer 17 and the bonding surface 7b, so that when the tape 15 is removed in a later process step, a bonding surface 7b that is as uncontaminated as possible is retained.

[0177] Figure 2b A second process step according to the invention is shown, in which a substrate 11 ″ is prepared as a temporary carrier. An adhesive 18 is applied to the substrate 11 ″ by known methods, in particular by a spin coating process.

[0178] Figure 2cThe third process step according to the invention of the second process according to the invention is shown, in which the rear surface 7r of the chip 7 is brought into contact with the bonding adhesive. Prior to this contact, in particular, all chips 7 fixed relative to each other are aligned relative to the substrate 11'. In this process step, it is also conceivable that mechanical pressure is applied from the rear side 15r of the tape, which should cause the bonding surfaces 7b of all chips 7 to coincide in a plane E. Here, plane E is the plane in which all bonding surfaces 7b of the chips 7 should be located. Plane E should be identical in particular to the surface of the protective layer 17 in the direction of the chip 7. This is important in particular when the carrier 15 is an adhesive tape. For example, it is conceivable that a roller rolls over the rear side 15r of the tape. However, it is preferred that the entire surface is loaded, which results in a uniform pressure distribution.

[0179] Figure 2d The fourth process step according to the invention of the second process according to the invention is shown, in which the adhesive tape 15 has been removed from the bonding surface 7b of the chip 7. The adhesive tape 15 is preferably peeled off. According to the enlarged view Z1, it can be seen that after the adhesive tape 15 is removed, the remnants of the protective layer 17 may remain on the bonding surface 7b. In this less preferred case, the chip must be cleaned again in another process step. Preferably, after the adhesive tape 15 is removed, the bonding surface 7b is free of contamination. The enlarged view Z2 shows an exaggerated illustration of two side-by-side chips, which differ in their thickness d1 and d2. However, the elasticity of the adhesive 18 causes the bonding surface 7b to be located in the same plane E, which is an important aspect of the process according to the invention.

[0180] Figure 2e The optional, less preferred fifth process step according to the invention of the second process according to the invention is shown, in which the bonding surface 7b of the chip 7 has been cleaned by a cleaning method. The protective layer 17 can no longer be seen in the enlarged view Z1.

[0181] Figure 2f The sixth process step according to the invention of the second process according to the invention is shown, in which a temporary carrier 11 ″ equipped with chips 7 is aligned relative to a further substrate 11 ′ and bonding is performed. According to the invention, bonding of all chips 7 is performed simultaneously.

[0182] Figure 2gThe seventh process step according to the invention of the second process according to the invention is shown, in which the adhesive 18 is treated. The treatment can be carried out chemically and / or thermally and / or by means of EM waves, in particular by means of UV light or infrared rays. In a particularly preferred embodiment according to the invention, the treatment is carried out by means of a temporary carrier 11 ″. The treatment preferably has the effect that the adhesive properties of the adhesive 18 are reduced or even completely eliminated, so that the temporary carrier 11 ″ can be detached from the chip 7.

[0183] Figure 2h The eighth process step according to the invention of the second process according to the invention is shown, in which the carrier substrate 11 ″ is removed.

[0184] Figure 2i A ninth process step according to the invention of the second process according to the invention is shown, in which a cleaning of the rear side surface 7r of the chip 7 is carried out. The result is once again a final product 19.

[0185] Figure 3 A first embodiment according to the invention for batch cleaning and / or plasma activation and / or bonding of chips 7 is shown. The chip 7 is located in an ejection device 1 having a recess 2. A sleeve 3, in particular a simple hole, is mounted at the bottom of the recess 2, through which a lifting device 4 can raise and lower the chip 7. The loading and / or unloading of the chip 7 can be achieved by a chuck 5, which can fix the chip 7 only on its rear side surface 7r by means of a fixing 6 in order to transport the chip. Preferably, all bonding surfaces 7b of all chips 7 coincide within the plane E during batch cleaning and / or plasma activation. The coincidence of all bonding surfaces 7b has the advantage of uniform treatment. As a result, it is ensured, in particular in the case of plasma treatment, that the plasma density is uniform over the entire surface. If the chip 7 should differ slightly in its thickness, the lifting device can make slight corrections in order to ensure the coincidence of the bonding surfaces 7b again.

[0186] Figure 4 A second embodiment according to the invention is shown for batch cleaning and / or plasma activation and / or bonding of chips 7 .

[0187] The chip 7 is located in the ejection device 1' with the seal 8. The chip 7 can be loaded and / or unloaded by means of a lifting device 4, which can be moved in translation through the sleeve 3. The fixing is preferably carried out by means of a fixing element 6, in particular a vacuum channel, which allows a vacuum to be generated in the intermediate space when the chip 7 is in contact with the seal 8. For the sake of clarity, the chuck 5 has not been drawn in this figure.

[0188] Therefore, the ejection devices 1, 1' are used for general batch cleaning and / or plasma activation and / or bonding of separated chips 7. It is also conceivable that the ejection devices 1, 1' themselves are constructed compactly so that they can be used as carrier wafers 11" for the second process according to the invention. In this case, at least before the bonding process with the substrate 11, the bonding surface 7b of the chip 7 must slightly protrude beyond the ejector surface 1o, 1o', which is automatically satisfied in terms of structural technology for the ejector surface 1o' of the ejector 1'. The ejection device 1' is thereby particularly suitable as a fixed carrier. The fixing element 6 can then also be an electrostatic fixing element, a magnetic fixing element or a gel pack fixing element.

[0189] Figure 5 A first embodiment of the bonding according to the invention is shown, in which, by way of example, an ejection device 1 can be used so that a chip 7 can be picked up by a chuck 5 through an aperture 24 of a mask 23. The picked-up chip 7 is transported, in particular transported over a plurality of stages. In this case, an optical system 25 can measure the bonding surface 7b and / or the backside surface 7r of the chip 7 and / or the substrate 11'. In particular, alignment marks (not shown) on the chip 7 and / or the substrate 11' can be found in order to position the transported chip 7 correctly. Therefore, in this embodiment, the substrate 11' to be equipped is not directly above the chip.

[0190] Figure 6 A second embodiment of the bonding according to the invention is shown, in which an ejection device 1' can be used by way of example in order to bond a chip 7 through the apertures 24 of a mask 23 to a chip 7 of a carrier 11'. The idea according to the invention is that the mask 23, which consists in particular of a high-purity material, preferably without surface contamination, protects the chip 7 on the ejection device 1' used by way of example from contamination. Hereby, according to the invention, it is shown again how the bonding surface 7b of the chip 7 can be protected from contamination. Of course, instead of the ejection device 1' used by way of example, any other type of device can be used in order to guide the chip 7 through the apertures 24 and to bond the chip to another chip 7 or to the surface of the substrate 11' which is located on the other side of the mask 23.

[0191] Figure 7a The first process step according to the invention for the self-alignment according to the invention of the chip 7 on the substrate 1' is shown. The chip 7 is placed on the liquid film 21 by the bonding head 9. In a special embodiment, the liquid film 21 is not distributed continuously over the entire substrate 1', but is only present as droplets or puddles at the locations where the self-alignment of the chip 7 is to take place.

[0192] It can be seen that the contacts 13 of the chip 7 are not aligned optimally with the contacts 13 of the substrate 1 ′.

[0193] Figure 7b The second process step according to the invention for the self-alignment of the chip 7 on the substrate 1' is shown. The bonding head 9 releases the fixation of the chip 7. The chip is now aligned by the lateral mobility of the chip due to the presence of the liquid film 21, so that the contacts 13 of the chip 7 are as congruent as possible with the contacts 13 of the substrate 1'. The reason for this is the different bonding properties of dielectric and electrical regions. Those regions that are hydrophilic preferably attract the hydrophilic regions. Preferably, this interaction can be diffused by a medium that has at least partial polarity. Water is a dipole and is therefore particularly well suited to this task according to the invention.

[0194] Figure 8a A bond head 9 according to the invention is shown, which consists of a fixing surface 22 with a fixing part 6. Spring elements 10, 10' with different spring constants are located behind the fixing surface 22. The spring constant of the centrally built spring element 10 is preferably greater than the spring constant of the peripherally built spring element 10'. An acceleration of the bond head 9 in the transverse direction has no influence on the shape of the fixing surface 22.

[0195] Figure 8b The bonding head 9 according to the invention is shown when accelerating in the normal direction of the surface to be bonded. Due to the higher spring constant of the central spring element 10, the inertia does not act as strongly on the central part of the fixing surface 22, or in other words, the central part of the fixing surface 22 follows the peripheral part and reacts faster than the peripheral part. Advantageously, the bending is also achieved by the rapid approach to the contact surface and the air cushion present. In the case of identical spring elements, the dynamic pressure generated by the translational movement on the fixing surface 22 will press the fixing surface symmetrically backward. However, since the peripheral spring elements 10 'have a smaller spring constant than the central spring element 10, these peripheral spring elements are more likely to yield because they are more elastic. Therefore, in addition to inertia, the dynamic pressure formed also causes bending. Due to this mechanical asymmetry, the fixing surface 22 and the chip 7 fixed thereto are convexly bent and can produce the contact point 23 that is optimal for direct bonding. It is thereby excluded that the chip 7 is first contacted laterally or flatly.

[0196] Reference numerals list

[0197] 1. 1' ejector device

[0198] 1o, 1o' Ejector surface

[0199] 2 Depression

[0200] 3 Casing

[0201] 4 Lifting device

[0202] 5. Chuck

[0203] 6 Fixing parts

[0204] 7 Chip

[0205] 7b Bonding surface

[0206] 7r Rear surface

[0207] 8 Seals

[0208] 9 Bonding head

[0209] 10, 10' spring element

[0210] 11, 11', 11" substrate

[0211] 12 Gap

[0212] 13 Contact Department

[0213] 14 Frame

[0214] 15. Tape

[0215] 15o Tape surface

[0216] 15r Tape rear side

[0217] 16 Separation device

[0218] 17 Protective layer

[0219] 18 Adhesive

[0220] 19 Final Product

[0221] 20 Dielectric Surface

[0222] 21 Liquid

[0223] 22 Fixed surface

[0224] 23 Mask

[0225] 24 Porosity

[0226] 25 Optical System

[0227] d1, d2 thickness

[0228] E Coincident plane

[0229] t Depth

[0230] Z1, Z2 enlarged image

Claims

1. A method for bonding a chip (7) to a semiconductor substrate (11') or to another chip, It is characterized in that The chip (7) is bonded to the semiconductor substrate (11') or the other chip by direct bonding, wherein the direct bonding is performed on a bonding surface (7b) of the chip (7), wherein the bonding surface (7b) is a hybrid bonding surface, wherein the hybrid bonding surface consists of a metal region and a dielectric region, The method is a mass bonding method, wherein in the mass bonding method all chips are first placed on a carrier in such a way that the later bonding surfaces point upward, wherein all bonding surfaces of the chips are then cleaned and pretreated simultaneously, in particular in a machine provided for this purpose, wherein all chips are then bonded simultaneously to the substrate actually to be bonded or the chip actually to be bonded, Plasma cleaning is performed on the bonding surface (7b) of the chip (7), wherein the plasma cleaning is accompanied by plasma activation of the surface, wherein the exposed bonding surface of the chip is cleaned and plasma activated simultaneously.

2. The method according to claim 1, characterized in that: The direct bonding is performed on a bonding surface (7b) of the chip (7), wherein the bonding surface (7b) is a hybrid bonding surface.

3. The method according to claim 1 or 2, characterized in that: The chip (7) is positioned and self-alignment of the chip (7) is performed.

4. The method according to claim 1 or 2, characterized in that: To produce the chips (7), a substrate (11) is fixed to a carrier (15), in particular to an adhesive tape, and then the substrate (11) is separated into the chips (7).

5. The method according to claim 4, characterized in that Before the substrate (11) is fixed on the carrier (15), the bonding surface (7b) of the substrate (11) is cleaned.

6. The method according to claim 4, characterized in that During removal from the carrier (15) and / or during transport to another location, in particular a bonding location, the bonding surface (7b) of the chip (7) is cleaned, in particular continuously.

7. The method according to claim 4, characterized in that The chips (7) are separated by a mechanical separation device, wherein a gap (12) has been introduced into the bonding surface (7b) of the substrate (11) beforehand.

8. A device for bonding a chip (7) to a semiconductor substrate (11') or another chip, It is characterized in that The chip (7) can be bonded to the semiconductor substrate (11') or the other chip by direct bonding, wherein the direct bonding is performed on a bonding surface (7b) of the chip (7), wherein the bonding surface (7b) is a hybrid bonding surface, wherein the hybrid bonding surface consists of a metal area and a dielectric area, wherein the device is a mass bonding device, wherein in the mass bonding device all chips are first placed on a carrier so that the later bonding surfaces point upward, wherein all bonding surfaces of the chips are then cleaned and pretreated simultaneously, in particular in a machine provided for this purpose, wherein all chips are then bonded simultaneously to the substrate actually to be bonded or the chip actually to be bonded, The device is designed to perform plasma cleaning on the bonding surface (7b) of the chip (7), wherein the plasma cleaning is accompanied by plasma activation of the surface, and wherein the device is designed to simultaneously perform cleaning and plasma activation on the exposed bonding surface of the chip.

9. The device according to claim 8, comprising an ejection device (1), wherein the ejection device has a recess (2) for positioning and / or fixing the chip (7).

10. A device according to claim 8 or 9, wherein a sleeve (3), in particular a hole, is located on the bottom surface of the recess (2), and wherein a lifting device (4) can lift the chip (7) through the sleeve (3) so that the chip (7) can be touched by the clamp (5).

11. The device according to claim 8 or 9, wherein the depth (t) of the recess (2) corresponds to the height of the chip (7).

12. The device according to claim 8 or 9, wherein the clamp (5) fixes the chip (7) on a fixing surface opposite to the bonding surface (7b).

13. The device according to claim 8 or 9, wherein the device comprises a mask (23) having a hole (24), wherein the mask (23) can be moved over the ejection device (1, 1') loaded with the chip (7) until the hole (24) is located over the next chip (7) to be bonded.

14. The device according to claim 8 or 9, comprising a bonding head (9) for fixing, transporting and bonding the chip (7).

15. A chip stack consisting of chips, characterized in that: The chips are bonded to each other by direct bonding according to claim 1 .

16. A semiconductor substrate (11') having a chip, characterized in that: The chip is bonded to the semiconductor substrate (11') by direct bonding according to claim 1.