Preparation method of semiconductor structure and semiconductor structure
By introducing doping elements into the first epitaxial layer of the superlattice structure to form a doped compound layer, the problem of strain accumulation caused by lattice mismatch is solved and the reliability and electrical performance of the semiconductor device are improved.
Patent Information
- Application Number
- CN202310341852.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-01
AI Technical Summary
In semiconductor devices, lattice mismatch in multi-period superlattice structures leads to strain accumulation, thereby reducing chip reliability. Especially in 3D DRAM-like devices, mismatch dislocations seriously affect electrical performance.
By introducing a doping element with a smaller atomic radius than the first element into the first epitaxial layer for doping, a doped compound layer is formed to reduce the lattice mismatch in the superlattice structure, reduce stress accumulation, and avoid mismatching sites. Error occurs.
It effectively reduces the misfit dislocations of the superlattice structure, improves the reliability of the chip, extends the critical thickness of the superlattice structure, and improves the crystal quality.
Smart Images

Figure CN118738099A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor technology, and in particular to a method for preparing a semiconductor structure and a semiconductor structure. Background Art
[0002] With the development of semiconductor technology, multi-period superlattice structures have been widely studied and applied in semiconductor advanced process nodes and 3D dynamic random access memory (DRAM). However, lattice mismatch is usually generated in superlattice structures. For example, for silicon / silicon germanium superlattice structures, the lattice mismatch between germanium and silicon is as high as 4%. Therefore, during the formation of the superlattice structure, the strain in the superlattice structure continues to accumulate. When its thickness exceeds a certain critical value, mismatch dislocations will be generated to reduce the strain. Especially for semiconductor devices similar to 3D DRAM, the more layers of the superlattice structure are required, the better, so its mismatch dislocations are more serious. The mismatch dislocations generated in the superlattice structure will seriously affect the electrical properties of the superlattice structure, thereby resulting in low reliability of the chip. Summary of the invention
[0003] Based on this, it is necessary to provide a method for preparing a semiconductor structure and a semiconductor structure to address the problem of low chip reliability.
[0004] In order to achieve the above objectives, on the one hand, the present application provides a method for preparing a semiconductor structure, comprising:
[0005] providing a substrate, the substrate comprising a first element;
[0006] A superlattice structure is formed on the substrate, the superlattice structure comprising a first epitaxial layer and a second epitaxial layer alternately stacked from bottom to top; wherein the first epitaxial layer is a doped compound layer comprising the first element, the second element and a doping element, the atomic diameter of the second element is larger than the atomic diameter of the first element, and the atomic diameter of the doping element is smaller than the atomic diameter of the first element; and the second epitaxial layer comprises the first element.
[0007] The method for preparing the semiconductor structure includes: providing a substrate, the substrate including a first element; forming a superlattice structure on the substrate, the superlattice structure including a first epitaxial layer and a second epitaxial layer alternately stacked from bottom to top; wherein the first epitaxial layer is a doped compound layer including the first element, the second element and a doping element, the atomic diameter of the second element is larger than the atomic diameter of the first element, and the atomic diameter of the doping element is smaller than the atomic diameter of the first element; the second epitaxial layer includes the first element. Since a doping element with an atomic radius smaller than that of the first element is introduced into the first epitaxial layer for doping, the doping element replaces the position of part of the second element and / or part of the first element, thereby reducing the lattice mismatch between the first epitaxial layer and the substrate and the second epitaxial layer, thereby reducing the stress accumulation of the superlattice structure during the formation process to reduce the mismatch dislocation of the superlattice structure, thereby avoiding the reduction of chip reliability.
[0008] In one embodiment, forming the superlattice structure on the substrate comprises: performing a plurality of epitaxial cycles, each of the epitaxial cycles comprising:
[0009] forming the first epitaxial layer;
[0010] The second epitaxial layer is formed on the upper surface of the first epitaxial layer.
[0011] In one embodiment, the forming of the first epitaxial layer includes: forming the first epitaxial layer by an in-situ doping process.
[0012] In one embodiment, forming the first epitaxial layer includes:
[0013] forming a first sub-epitaxial layer including the first element and the second element;
[0014] forming a second sub-epitaxial layer including the first element, the second element and the doping element on the upper surface of the first sub-epitaxial layer by an in-situ doping process;
[0015] A third sub-epitaxial layer including the first element and the second element is formed on an upper surface of the second sub-epitaxial layer, and the third sub-epitaxial layer, the second sub-epitaxial layer and the first sub-epitaxial layer together constitute the first epitaxial layer.
[0016] In one embodiment, forming the first epitaxial layer includes: forming the first epitaxial layer by an in-situ doping process at a first preset temperature, wherein the first preset temperature is less than 600°C.
[0017] In one embodiment, the first element includes silicon, the second element includes germanium, and the doping element includes boron or carbon; the substrate includes a silicon substrate, the first epitaxial layer includes a doped silicon germanium layer, and the second epitaxial layer includes a silicon layer.
[0018] In one of the embodiments, before forming the superlattice structure on the substrate, the method further includes: pre-treating the substrate to remove organic matter, metal ions and / or a surface oxide layer on the surface of the substrate.
[0019] In one embodiment, providing a substrate comprises:
[0020] providing an initial substrate;
[0021] The upper surface of the initial substrate is patterned to obtain a substrate having a patterned structure on the upper surface.
[0022] On the other hand, the present application also provides a semiconductor structure, comprising:
[0023] a substrate comprising a first element;
[0024] A superlattice structure, the superlattice structure comprising a first epitaxial layer and a second epitaxial layer alternately stacked from bottom to top; wherein the first epitaxial layer is a doped compound layer comprising the first element, the second element and a doping element, the atomic diameter of the second element is larger than the atomic diameter of the first element, and the atomic diameter of the doping element is smaller than the atomic diameter of the first element; and the second epitaxial layer comprises the first element.
[0025] The semiconductor structure includes a substrate and a superlattice structure, wherein the substrate includes a first element, and the superlattice structure includes a first epitaxial layer and a second epitaxial layer alternately stacked from bottom to top; wherein the first epitaxial layer is a doped compound layer including the first element, the second element and a doping element, the atomic diameter of the second element is larger than the atomic diameter of the first element, the atomic diameter of the doping element is smaller than the atomic diameter of the first element, and the second epitaxial layer includes the first element. Since a doping element with an atomic radius smaller than that of the first element is introduced into the first epitaxial layer for doping, the doping element replaces the position of part of the second element and / or part of the first element, thereby reducing the lattice mismatch between the first epitaxial layer and the substrate and the second epitaxial layer, thereby reducing the stress accumulation of the superlattice structure during the formation process to reduce the mismatch dislocation of the superlattice structure, thereby avoiding the reduction of chip reliability.
[0026] In one embodiment, the first epitaxial layer comprises:
[0027] a first sub-epitaxial layer, wherein the first sub-epitaxial layer is a compound layer including the first element and the second element;
[0028] a second sub-epitaxial layer, located on an upper surface of the first sub-epitaxial layer, the second sub-epitaxial layer being a doped compound layer including the first element, the second element and the doping element;
[0029] The third sub-epitaxial layer is located on an upper surface of the second sub-epitaxial layer, and the third sub-epitaxial layer is a compound layer including the first element and the second element.
[0030] In one embodiment, the first element includes silicon, the second element includes germanium, and the doping element includes boron or carbon; the substrate includes a silicon substrate, the first epitaxial layer includes a doped silicon germanium layer, and the second epitaxial layer includes a silicon layer.
[0031] In one embodiment, the substrate comprises a patterned substrate having a patterned structure on its upper surface. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the technical solutions in the embodiments of the present application or the conventional technology, the drawings required for use in the embodiments or the conventional technology descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0033] Figure 1 is a flow chart of a method for preparing a semiconductor structure provided in an embodiment;
[0034] Figure 2 A schematic diagram of a cross-sectional structure of a structure obtained in step S101 in a method for preparing a semiconductor structure provided in an embodiment;
[0035] Figure 3 A schematic diagram of a cross-sectional structure of a structure obtained in step S102 in a method for preparing a semiconductor structure provided in an embodiment;
[0036] Figure 4 A flowchart of the steps of forming a superlattice structure on a substrate in a method for preparing a semiconductor structure provided in an embodiment;
[0037] Figure 5 A schematic diagram of a cross-sectional structure of a structure obtained in step S1021 in a method for preparing a semiconductor structure provided in an embodiment;
[0038] Figure 6 A schematic diagram of a cross-sectional structure of a structure obtained in step S1022 in a method for preparing a semiconductor structure provided in an embodiment;
[0039] Figure 7 is a flowchart of step S1021 in a method for preparing a semiconductor structure provided in an embodiment;
[0040] Figure 8 A schematic diagram of a cross-sectional structure of a structure obtained in step S1021a of a method for preparing a semiconductor structure provided in an embodiment;
[0041] Fig. 9 A schematic diagram of a cross-sectional structure of a structure obtained in step S1021b of a method for preparing a semiconductor structure provided in an embodiment;
[0042] Fig.10 A schematic diagram of a cross-sectional structure of a structure obtained in step S1021c of a method for preparing a semiconductor structure provided in an embodiment;
[0043] Fig.11 FIG. 1 is a flow chart of step S101 in a method for preparing a semiconductor structure provided in an embodiment.
[0044] Explanation of the reference numerals: 10 - substrate, 20 - superlattice structure, 201 - first epitaxial layer, 2011 - first sub-epitaxial layer, 2012 - second sub-epitaxial layer, 2013 - third sub-epitaxial layer, 202 - second epitaxial layer. DETAILED DESCRIPTION
[0045] In order to facilitate understanding of the present application, the present application will be described more fully below with reference to the relevant drawings. Embodiments of the present application are provided in the drawings. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present application more thorough and comprehensive.
[0046] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0047] It should be understood that when an element or layer is referred to as being "on, adjacent to, connected to or coupled to other elements or layers, it may be directly on, adjacent to, connected to or coupled to other elements or layers, or there may be intervening elements or layers. On the contrary, when an element is referred to as being "directly on, directly adjacent to, directly connected to or directly coupled to other elements or layers, there are no intervening elements or layers. It should be understood that although the terms first, second, third, etc. may be used to describe various elements, components, regions, layers, doping types and / or parts, these elements, components, regions, layers, doping types and / or parts should not be limited by these terms. These terms are merely used to distinguish one element, component, region, layer, doping type or part from another element, component, region, layer, doping type or part. Therefore, without departing from the teachings of the present application, the first element, component, region, layer, doping type or portion discussed below may be represented as a second element, component, region, layer or portion; for example, the first doping type may be P-type and the second doping type may be N-type, or the first doping type may be N-type and the second doping type may be P-type.
[0048] Spatially relative terms such as "under," "beneath," "below," "under," "on the surface of," "above," and the like, may be used herein to describe the relationship of an element or feature shown in the figures to other elements or features. It should be understood that, in addition to the orientations shown in the figures, spatially relative terms also include different orientations of the device in use and operation. For example, if the device in the accompanying drawings is flipped, an element or feature described as "under other elements" or "under it" or "under it" will be oriented as being "on" the other elements or features. Thus, the exemplary terms "under" and "under" may include both upper and lower orientations. In addition, the device may also include additional orientations (e.g., rotated 90 degrees or other orientations), and the spatial descriptors used herein are interpreted accordingly.
[0049] When used herein, the singular forms "a", "an", and "said / the" may also include plural forms, unless the context clearly indicates otherwise. It should also be understood that the terms "include / comprise" or "have" and the like specify the presence of stated features, wholes, steps, operations, components, parts, or combinations thereof, but do not exclude the possibility of the presence or addition of one or more other features, wholes, steps, operations, components, parts, or combinations thereof. At the same time, in this specification, the term "and / or" includes any and all combinations of the relevant listed items.
[0050] With the development of semiconductor technology, multi-period superlattice structures have been widely studied and applied in semiconductor advanced process nodes and 3D dynamic random access memory (DRAM).
[0051] An epitaxial period of a superlattice structure is usually composed of a first epitaxial layer and a second epitaxial layer. In conventional technology, the constituent elements of the first epitaxial layer are only the first element and the second element whose atomic radius is larger than the first element. At this time, in conventional technology, when a superlattice structure is formed on a substrate, since the constituent elements of the substrate and the second epitaxial layer are the first element, and the constituent elements of the first epitaxial layer are the first element and the second element, and since the atomic radius of the second element is larger than the atomic radius of the first element, the lattice constants of the substrate and the second epitaxial layer are not the same as those of the first epitaxial layer. Therefore, in conventional technology, when the first epitaxial layer is formed on the substrate, stress is generated near the interface of growth, and the stress accumulates continuously. When the thickness of the first epitaxial layer exceeds a certain critical value, misfit dislocations are generated to reduce the stress.
[0052] For example, for the traditional silicon / silicon germanium superlattice structure, the lattice mismatch between germanium and silicon is as high as 4%. Therefore, during the formation of the superlattice structure, the strain in the superlattice structure continues to accumulate. When its thickness exceeds a certain critical value, mismatch dislocations will be generated to reduce the strain, especially for semiconductor devices similar to 3DDRAM, which require the number of superlattice structures to be as large as possible, so its mismatch dislocations are more serious. The mismatch dislocations generated in the superlattice structure will seriously affect the electrical properties of the superlattice structure, thereby resulting in low chip reliability.
[0053] See also Figure 1 , the present application provides a method for preparing a semiconductor structure, comprising the following steps:
[0054] S101: providing a substrate, wherein the substrate includes a first element;
[0055] S102: forming a superlattice structure on a substrate, the superlattice structure comprising a first epitaxial layer and a second epitaxial layer alternately stacked from bottom to top; wherein the first epitaxial layer is a doped compound layer comprising a first element, a second element and a doping element, the atomic diameter of the second element is larger than the atomic diameter of the first element, and the atomic diameter of the doping element is smaller than the atomic diameter of the first element; the second epitaxial layer comprises the first element.
[0056] In step S101, refer to Figure 1 Step S101 in Figure 2 , a substrate 10 is provided, and the substrate 10 includes a first element.
[0057] The material of the substrate 10 may be any suitable substrate material known in the art, for example, at least one of the following materials: silicon (Si), germanium (Ge), red phosphorus, silicon germanium (SiGe), silicon carbide (SiC), carbon germanium silicon (SiGeC), indium arsenide (InAs), gallium arsenide (GaAs), indium phosphide (InP) or other III / V compound semiconductors, including multilayer structures composed of these semiconductors, or silicon on insulator (SOI), stacked silicon on insulator (SSOI), stacked silicon germanium on insulator (S-SiGeOI), silicon germanium on insulator (SiGeOI) and germanium on insulator (GeOI), or double-side polished silicon wafers (DSP), ceramic substrates such as aluminum oxide, quartz or glass substrates, etc., which are not limited in this embodiment. The first element may refer to the most important element in the substrate 10. For example, when the material of the substrate 10 is silicon, the first element may be silicon.
[0058] In step S101, refer to Figure 1 Step S102 in Figure 3 A superlattice structure 20 is formed on a substrate 10, and the superlattice structure 20 includes a first epitaxial layer 201 and a second epitaxial layer 202 alternately stacked from bottom to top; wherein the first epitaxial layer 201 is an impurity compound layer including a first element, a second element and an impurity element, the atomic diameter of the second element is larger than the atomic diameter of the first element, and the atomic diameter of the impurity element is smaller than the atomic diameter of the first element; the second epitaxial layer 202 includes the first element.
[0059] The superlattice structure 20 refers to a multilayer film structure in which thin layers of two different components are alternately grown and maintain a strict periodicity, and can be understood as a specific form of layered fine composite material. The main semiconductor properties of the first epitaxial layer 201 and the second epitaxial layer 202, such as the band gap or doping level, can be independently controlled, and the number of layers of the first epitaxial layer 201 and the second epitaxial layer 202 can also be artificially controlled during growth.
[0060] Among them, the second element and the doping element can be determined after the first element is determined. For example, when the first element is silicon, the second element can be an element with an atomic radius larger than silicon, such as phosphorus (P), sulfur (S), germanium (Ge), arsenic (As), selenium (Se), etc., and the doping element can be an element with an atomic radius smaller than silicon, such as boron (B), carbon (C), nitrogen (N), fluorine (F), etc. In actual application scenarios, the types of the first element, the second element, and the doping element can be determined by comprehensively considering the actual process requirements and costs, and this embodiment is not limited here.
[0061] By introducing an doping element with an atomic radius smaller than that of the first element into the first epitaxial layer 201, the doping element replaces part of the second element and / or part of the first element, so that the lattice mismatch between the first epitaxial layer 201 and the substrate 10 and the second epitaxial layer 202 is reduced, thereby reducing the stress accumulation of the superlattice structure 20 during the formation process to reduce the mismatch dislocations of the superlattice structure 20, thereby avoiding a decrease in the reliability of the chip.
[0062] The method for preparing the semiconductor structure includes: providing a substrate, the substrate includes a first element; forming a superlattice structure on the substrate, the superlattice structure includes a first epitaxial layer and a second epitaxial layer alternately stacked from bottom to top; wherein the first epitaxial layer is a doped compound layer including a first element, a second element and a doping element, the atomic diameter of the second element is larger than the atomic diameter of the first element, and the atomic diameter of the doping element is smaller than the atomic diameter of the first element; the second epitaxial layer includes the first element. Since a doping element with an atomic radius smaller than that of the first element is introduced into the first epitaxial layer for doping, the doping element replaces the position of part of the second element and / or part of the first element, thereby reducing the lattice mismatch between the first epitaxial layer and the substrate and the second epitaxial layer, thereby reducing the stress accumulation of the superlattice structure during the formation process to reduce the mismatch dislocation of the superlattice structure, thereby avoiding the reduction of chip reliability.
[0063] In one embodiment, Figure 4 As shown, forming a superlattice structure 20 on a substrate 10 includes: performing a plurality of epitaxial cycles, each of which includes:
[0064] S1021: forming a first epitaxial layer 201, such as Figure 5 shown.
[0065] To facilitate understanding of this program, Figure 5 Schematic diagram of forming the first epitaxial layer 201 in the first epitaxial cycle. The first epitaxial layer 201 can be formed by introducing a precursor corresponding to a compound composed of a first element and a second element, and in the process of forming the first epitaxial layer 201, a corresponding doping process is simultaneously used to introduce the doping element into the compound, so as to finally form a doped compound layer, i.e., the first epitaxial layer 201.
[0066] Optionally, the thickness of the first epitaxial layer 201 may be 1 nm-300 nm.
[0067] S1022: forming a second epitaxial layer 202 on the upper surface of the first epitaxial layer 201, such as Figure 6 shown.
[0068] To facilitate understanding of this program, Figure 6FIG. 2 is a schematic diagram of forming the second epitaxial layer 202 in the first epitaxial cycle. Figure 5 as well as Figure 6 For example, in the second epitaxial cycle, the first epitaxial layer 201 of the second epitaxial cycle is formed on the second epitaxial layer 202 of the first epitaxial cycle, and so on, to finally form the first epitaxial layer 201 and the second epitaxial layer 202 alternately stacked from bottom to top. Optionally, the number of the epitaxial cycles can be 1-300.
[0069] The second epitaxial layer 202 may be formed by introducing a precursor corresponding to the first element. Optionally, the thickness of the second epitaxial layer 202 may be 1 nm-500 nm.
[0070] In one embodiment, the above step S1021 includes: forming the first epitaxial layer 201 by adopting an in-situ doping process.
[0071] The in-situ doping process can make the doping element replace the original second element and / or the first element, thereby forming a doped compound layer. By using the in-situ doping process from the beginning to the end of the formation process of the first epitaxial layer 201, the first epitaxial layer 201 is entirely composed of a doped compound layer.
[0072] In one embodiment, Figure 7 As shown, the above step S1021 includes:
[0073] S1021a: forming a first sub-epitaxial layer 2011 including a first element and a second element, such as Figure 8 shown.
[0074] The first sub-epitaxial layer 2011 may be formed by introducing a precursor corresponding to a compound composed of the first element and the second element.
[0075] S1021b: forming a second sub-epitaxial layer 2012 including a first element, a second element and a doping element on the upper surface of the first sub-epitaxial layer 2011 by an in-situ doping process, such as Fig. 9 shown.
[0076] Among them, a precursor corresponding to a compound composed of the first element and the second element can be introduced, and an in-situ doping process can be used to introduce the doping element during the introduction of the precursor, thereby finally forming a second sub-epitaxial layer 2012 including the first element, the second element and the doping element.
[0077] S1021c: forming a third sub-epitaxial layer 2013 including the first element and the second element on the upper surface of the second sub-epitaxial layer 2012, the third sub-epitaxial layer 2013, the second sub-epitaxial layer 2012 and the first sub-epitaxial layer 2011 together constitute the first epitaxial layer 201, such as Fig.10 shown.
[0078] The third sub-epitaxial layer 2013 can be formed by introducing a precursor corresponding to a compound composed of the first element and the second element. At this time, the first sub-epitaxial layer 2011, the second sub-epitaxial layer 2012 and the third sub-epitaxial layer 2013 together constitute the first epitaxial layer 201 in a sandwich-like structure. The advantage of the sandwich structure formed in this embodiment is that, since some doping elements may have a tendency to diffuse toward the substrate 10 and the second epitaxial layer 202, the formation of the sandwich structure can prevent the doping elements from diffusing toward the substrate 10 and the second epitaxial layer 202 while avoiding stress accumulation in the superlattice structure 20, thereby ensuring the stability of the entire superlattice structure 20, thereby further avoiding a decrease in the reliability of the chip.
[0079] In one embodiment, the step S1021 includes: forming the first epitaxial layer 201 by an in-situ doping process at a first preset temperature, wherein the first preset temperature is less than 600°C.
[0080] Among them, the first preset temperature is usually lower than the temperature of the first epitaxial layer 201 formed by directly using the precursors of the first element and the second element. Since the first preset temperature is relatively low, the strain relaxation of the crystal composed of the first element and the second element will be slower during the growth of the first epitaxial layer 201, so that the strain accumulation of the first epitaxial layer 201 can be further slowed down, thereby further avoiding the reliability of the chip from being reduced. In addition, since the strain relaxation of the crystal composed of the first element and the second element is slow at the lower first preset temperature, a smaller amount of doping elements can be used to achieve the same effect of reducing stress, thereby saving costs. For example, taking the first element as silicon, the second element as germanium, and the doping element as boron as an example, the first epitaxial layer 201 is a boron-doped silicon germanium layer. Assuming that the doping concentration of boron under normal circumstances needs to reach the first concentration to fully compensate for the strain of the silicon germanium layer, under the condition of the first preset temperature, since the strain relaxation of the silicon germanium layer slows down, it is only necessary to dope the boron element less than the first concentration to achieve the effect of fully compensating for the strain of the silicon germanium layer, thereby saving costs.
[0081] In one embodiment, the first element includes silicon, the second element includes germanium, and the doping element includes boron or carbon; the substrate 10 includes a silicon substrate 10, the first epitaxial layer 201 includes a doped silicon germanium layer, and the second epitaxial layer 202 includes a silicon layer.
[0082] For example, the first element is silicon, the second element is germanium, and the doping element is boron. In this case, the substrate 10 is a silicon substrate, the first epitaxial layer 201 is a boron-doped silicon germanium layer, and the second epitaxial layer 202 is a silicon layer. When forming the first epitaxial layer 201, the silicon germanium (SiGe) grown by using a silicon germanium precursor is used. 1-x Ge x , 0<x<1) The thickness of the layer can be 1nm-200nm, and the boron doping concentration can be 5E19cm -3 -1E21cm -3 When forming the second epitaxial layer 202, the thickness of the silicon layer grown using the silicon precursor may be 1 nm-500 nm.
[0083] After calculation, for a silicon germanium layer with a germanium content of 20%, the boron doping concentration reaches 3E20cm -3 The entire strain of the SiGe layer can be compensated when the boron doping concentration reaches 1.5E20cm -3 When the boron is added to the silicon germanium layer, 50% of the strain of the silicon germanium layer can be compensated. That is to say, for the same silicon / silicon germanium layer superlattice structure 20, the crystal quality will be greatly improved after boron compensation. Similarly, this method can double the critical thickness of the silicon / silicon germanium layer superlattice structure 20.
[0084] In addition, for 3D DRAM and similar semiconductor devices, the substrate 10 is usually a silicon substrate, the first epitaxial layer 201 is a silicon germanium layer, and the second epitaxial layer 202 is a silicon layer to form a superlattice structure 20. In order to ensure the performance and process feasibility requirements of the above-mentioned semiconductor device, the thickness of the silicon germanium layer used as the first epitaxial layer 201 is usually required to reach a certain level (for example, >60nm), and the number of epitaxial cycles of the superlattice structure 20 formed by the first epitaxial layer 201 and the second epitaxial layer 202 is as large as possible, that is, for the above-mentioned semiconductor device, the thicker the thickness of the superlattice structure 20 is, the better. The thicker the superlattice structure 20 is, the more serious the stress accumulation is. By using the semiconductor structure preparation method of the present application to dope the first epitaxial layer 201 with doping elements (for example, boron or phosphorus), the stress accumulation in the first epitaxial layer 201 can be reduced, thereby avoiding the reduction of the reliability of 3D DRAM and similar semiconductor devices.
[0085] In one embodiment, before the above step S102 , the method for preparing the semiconductor structure further includes: pre-treating the substrate 10 to remove organic matter, metal ions and / or a surface oxide layer on the surface of the substrate 10 .
[0086] In one embodiment, Fig.11 As shown, the above step S101 includes:
[0087] S1011: providing an initial substrate 10.
[0088] S1012: performing patterning on the upper surface of the initial substrate 10 to obtain a substrate 10 having a patterned structure on the upper surface.
[0089] Among them, after corresponding device and chip design, the upper surface of the initial substrate 10 can be patterned using Fabrication (Fab) technology on the initial substrate 10 to obtain a substrate 10 with a patterned structure on the upper surface. The substrate 10 with a patterned structure can further reduce the stress accumulation of the superlattice structure 20, reduce the lattice mismatch inside the superlattice structure 20, and thus can further improve the crystal quality of the superlattice structure 20.
[0090] On the other hand, Figure 3 As shown, the present application also provides a semiconductor structure, which includes a substrate 10 and a superlattice structure 20, wherein the substrate 10 includes a first element, and the superlattice structure 20 includes a first epitaxial layer 201 and a second epitaxial layer 202 alternately stacked from bottom to top; wherein the first epitaxial layer 201 is an impurity compound layer including a first element, a second element and an impurity element, the atomic diameter of the second element is larger than the atomic diameter of the first element, the atomic diameter of the impurity element is smaller than the atomic diameter of the first element, and the second epitaxial layer 202 includes the first element.
[0091] The material of the substrate 10 may be any suitable substrate material known in the art, for example, at least one of the following materials: silicon (Si), germanium (Ge), red phosphorus, silicon germanium (SiGe), silicon carbide (SiC), carbon germanium silicon (SiGeC), indium arsenide (InAs), gallium arsenide (GaAs), indium phosphide (InP) or other III / V compound semiconductors, including multilayer structures composed of these semiconductors, or silicon on insulator (SOI), stacked silicon on insulator (SSOI), stacked silicon germanium on insulator (S-SiGeOI), silicon germanium on insulator (SiGeOI) and germanium on insulator (GeOI), or double-side polished silicon wafers (DSP), ceramic substrates such as aluminum oxide, quartz or glass substrates, etc., which are not limited in this embodiment. The first element may refer to the most important element in the substrate 10. For example, when the material of the substrate 10 is silicon, the first element may be silicon.
[0092] The superlattice structure 20 refers to a multilayer film structure in which thin layers of two different components are alternately grown and maintain a strict periodicity, and can be understood as a specific form of layered fine composite material. The main semiconductor properties of the first epitaxial layer 201 and the second epitaxial layer 202, such as the band gap or doping level, can be independently controlled, and the number of layers of the first epitaxial layer 201 and the second epitaxial layer 202 can also be artificially controlled during growth.
[0093] Optionally, the thickness of the first epitaxial layer 201 may be 1 nm-300 nm.
[0094] Optionally, the thickness of the second epitaxial layer 202 may be 1 nm-500 nm.
[0095] Among them, the second element and the doping element can be determined after the first element is determined. For example, when the first element is silicon, the second element can be an element with an atomic radius larger than silicon, such as phosphorus (P), sulfur (S), germanium (Ge), arsenic (As), selenium (Se), etc., and the doping element can be an element with an atomic radius smaller than silicon, such as boron (B), carbon (C), nitrogen (N), fluorine (F), etc. In actual application scenarios, the types of the first element, the second element, and the doping element can be determined by comprehensively considering the actual process requirements and costs, and this embodiment is not limited here.
[0096] By introducing an doping element with an atomic radius smaller than that of the first element into the first epitaxial layer 201, the doping element replaces part of the second element and / or part of the first element, so that the lattice mismatch between the first epitaxial layer 201 and the substrate 10 and the second epitaxial layer 202 is reduced, thereby reducing the stress accumulation of the superlattice structure 20 during the formation process to reduce the mismatch dislocations of the superlattice structure 20, thereby avoiding a decrease in the reliability of the chip.
[0097] The semiconductor structure includes a substrate 10 and a superlattice structure 20, wherein the substrate 10 includes a first element, and the superlattice structure 20 includes a first epitaxial layer 201 and a second epitaxial layer 202 alternately stacked from bottom to top; wherein the first epitaxial layer 201 is a doped compound layer including a first element, a second element and a doping element, the atomic diameter of the second element is larger than the atomic diameter of the first element, the atomic diameter of the doping element is smaller than the atomic diameter of the first element, and the second epitaxial layer 202 includes the first element. Since a doping element with an atomic radius smaller than that of the first element is introduced into the first epitaxial layer 201 for doping, the doping element replaces the position of part of the second element and / or part of the first element, thereby reducing the lattice mismatch between the first epitaxial layer 201 and the substrate 10 and the second epitaxial layer 202, thereby reducing the stress accumulation of the superlattice structure 20 during the formation process to reduce the mismatch dislocation of the superlattice structure 20, thereby avoiding the reduction of chip reliability.
[0098] In one embodiment, Fig.10 As shown, the first epitaxial layer 201 includes: a first sub-epitaxial layer 2011, a second sub-epitaxial layer 2012, and a third sub-epitaxial layer 2013, wherein the first sub-epitaxial layer 2011 is a compound layer including a first element and a second element, the second sub-epitaxial layer 2012 is located on the upper surface of the first sub-epitaxial layer 2011, the second sub-epitaxial layer 2012 is a doped compound layer including the first element, the second element and a doping element, the third sub-epitaxial layer 2013 is located on the upper surface of the second sub-epitaxial layer 2012, and the third sub-epitaxial layer 2013 is a compound layer including the first element and the second element.
[0099] The first epitaxial layer 2011, the second epitaxial layer 2012 and the third epitaxial layer 2013 together constitute the first epitaxial layer 201 in a sandwich-like structure. The advantage of the sandwich structure formed in this embodiment is that since some doping elements may have a tendency to diffuse toward the substrate 10 and the second epitaxial layer 202, the formation of the sandwich structure can prevent the doping elements from diffusing toward the substrate 10 and the second epitaxial layer 202 while avoiding stress accumulation in the superlattice structure 20, thereby ensuring the stability of the entire superlattice structure 20, thereby further avoiding the reduction of chip reliability.
[0100] In one embodiment, the first element includes silicon, the second element includes germanium, and the doping element includes boron or carbon; the substrate 10 includes a silicon substrate 10, the first epitaxial layer 201 includes a doped silicon germanium layer, and the second epitaxial layer 202 includes a silicon layer.
[0101] For example, the first element is silicon, the second element is germanium, and the doping element is boron. In this case, the substrate 10 is a silicon substrate 10, the first epitaxial layer 201 is a boron-doped silicon germanium layer, and the second epitaxial layer 202 is a silicon layer. When forming the first epitaxial layer 201, the silicon germanium (SiGe) grown by using a silicon germanium precursor is used. 1-x Ge x , 0<x<1) The thickness of the layer can be 1nm-200nm, and the boron doping concentration can be 5E19cm -3 -1E21cm -3 When forming the second epitaxial layer 202, the thickness of the silicon layer grown using the silicon precursor may be 1 nm-500 nm.
[0102] After calculation, for a silicon germanium layer with a germanium content of 20%, the boron doping concentration reaches 3E20cm -3 The entire strain of the SiGe layer can be compensated when the boron doping concentration reaches 1.5E20cm -3 When the boron is added to the silicon germanium layer, 50% of the strain of the silicon germanium layer can be compensated. That is to say, for the same silicon / silicon germanium layer superlattice structure 20, the crystal quality will be greatly improved after boron compensation. Similarly, this method can double the critical thickness of the silicon / silicon germanium layer superlattice structure 20.
[0103] In addition, for 3D DRAM and similar semiconductor devices, the substrate 10 is usually a silicon substrate 10, the first epitaxial layer 201 is a silicon germanium layer, and the second epitaxial layer 202 is a silicon layer to form a superlattice structure 20, wherein, in order to ensure the performance and process feasibility requirements of the above-mentioned semiconductor device, the thickness of the silicon germanium layer as the first epitaxial layer 201 is usually required to reach a certain level (for example, > 60nm), and the number of epitaxial cycles of the superlattice structure 20 formed by the first epitaxial layer 201 and the second epitaxial layer 202 is as large as possible, that is, for the above-mentioned semiconductor device, the thicker the thickness of the superlattice structure 20 is, the better. The thicker the superlattice structure 20 is, the more serious the stress accumulation is. By using the semiconductor structure preparation method of the present application to dope the first epitaxial layer 201 with doping elements (for example, boron or phosphorus), the stress accumulation in the first epitaxial layer 201 can be reduced, thereby avoiding the reduction of the reliability of 3D DRAM and similar semiconductor devices.
[0104] In one embodiment, the substrate 10 includes a patterned substrate 10 having a pattern structure on its upper surface.
[0105] The substrate 10 with the patterned structure can further reduce the stress accumulation of the superlattice structure 20 , thereby reducing the lattice mismatch inside the superlattice structure 20 , thereby further improving the crystal quality of the superlattice structure 20 .
[0106] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features of the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0107] The above embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.
Claims
1. A method for preparing a semiconductor structure, characterized in that: include: providing a substrate, the substrate comprising a first element; A superlattice structure is formed on the substrate, the superlattice structure comprising a first epitaxial layer and a second epitaxial layer alternately stacked from bottom to top; wherein the first epitaxial layer is a doped compound layer comprising the first element, the second element and a doping element, the atomic diameter of the second element is larger than the atomic diameter of the first element, and the atomic diameter of the doping element is smaller than the atomic diameter of the first element; and the second epitaxial layer comprises the first element.
2. The method for preparing a semiconductor structure according to claim 1, characterized in that: The forming of the superlattice structure on the substrate comprises: performing a plurality of epitaxial cycles, each of the epitaxial cycles comprising: forming the first epitaxial layer; The second epitaxial layer is formed on the upper surface of the first epitaxial layer.
3. The method for preparing a semiconductor structure according to claim 2, characterized in that: The forming of the first epitaxial layer includes: forming the first epitaxial layer by adopting an in-situ doping process.
4. The method for preparing a semiconductor structure according to claim 2, characterized in that: The forming of the first epitaxial layer comprises: forming a first sub-epitaxial layer including the first element and the second element; forming a second sub-epitaxial layer including the first element, the second element and the doping element on the upper surface of the first sub-epitaxial layer by an in-situ doping process; A third sub-epitaxial layer including the first element and the second element is formed on an upper surface of the second sub-epitaxial layer, and the third sub-epitaxial layer, the second sub-epitaxial layer and the first sub-epitaxial layer together constitute the first epitaxial layer.
5. The method for preparing a semiconductor structure according to claim 2, characterized in that: The first epitaxial layer is formed, comprising: forming the first epitaxial layer by an in-situ doping process at a first preset temperature, wherein the first preset temperature is less than 600°C.
6. The method for preparing a semiconductor structure according to claim 1, characterized in that: The first element includes silicon, the second element includes germanium, and the doping element includes boron or carbon; the substrate includes a silicon substrate, the first epitaxial layer includes a doped silicon germanium layer, and the second epitaxial layer includes a silicon layer.
7. The method for preparing a semiconductor structure according to claim 1, characterized in that: Before forming the superlattice structure on the substrate, the method further includes: pre-treating the substrate to remove organic matter, metal ions and / or a surface oxide layer on the surface of the substrate.
8. The method for preparing a semiconductor structure according to any one of claims 1 to 6, characterized in that: The providing of a substrate comprises: providing an initial substrate; The upper surface of the initial substrate is patterned to obtain a substrate having a patterned structure on the upper surface.
9. A semiconductor structure, characterized in that: include: a substrate comprising a first element; A superlattice structure, the superlattice structure comprising a first epitaxial layer and a second epitaxial layer alternately stacked from bottom to top; wherein the first epitaxial layer is a doped compound layer comprising the first element, the second element and a doping element, the atomic diameter of the second element is larger than the atomic diameter of the first element, and the atomic diameter of the doping element is smaller than the atomic diameter of the first element; and the second epitaxial layer comprises the first element.
10. The semiconductor structure according to claim 9, characterized in that: The first epitaxial layer comprises: a first sub-epitaxial layer, wherein the first sub-epitaxial layer is a compound layer including the first element and the second element; a second sub-epitaxial layer, located on an upper surface of the first sub-epitaxial layer, the second sub-epitaxial layer being a doped compound layer including the first element, the second element and the doping element; The third sub-epitaxial layer is located on an upper surface of the second sub-epitaxial layer, and the third sub-epitaxial layer is a compound layer including the first element and the second element.
11. The semiconductor structure according to claim 9, characterized in that: The first element includes silicon, the second element includes germanium, and the doping element includes boron or carbon; the substrate includes a silicon substrate, the first epitaxial layer includes a doped silicon germanium layer, and the second epitaxial layer includes a silicon layer.
12. The semiconductor structure according to any one of claims 9 to 11, characterized in that: The substrate comprises a patterned substrate having a pattern structure on its upper surface.
Citation Information