Method and equipment for preparing electrode of silicon heterojunction battery
Preparing fine gate lines through the imprinting process solves the problems of high cost and poor conductivity of traditional silicon-based heterojunction battery electrode gate lines, improves photovoltaic conversion efficiency, reduces preparation costs, and avoids the use of high-cost equipment.
Patent Information
- Application Number
- CN202410816919.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-01
AI Technical Summary
The electrode grid lines of traditional silicon-based heterojunction cells have high cost and poor conductivity, resulting in low photoelectric conversion efficiency. The existing electroplated copper grid line technology requires expensive laser or photolithography equipment, which increases the cost and equipment complexity.
The imprinting process is used to prepare the imprinting layer, and the metal layer is imprinted and removed through the imprinting template to form fine grid lines, avoiding the use of photoresist and laser equipment, reducing costs and improving preparation accuracy.
It achieves high photovoltaic conversion efficiency and the preparation of fine gate lines, reduces the metallization cost of silicon heterojunction cells, and avoids the use of high-cost copper electroplating equipment to increase the height of the gate lines.
Smart Images

Figure CN118738211A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor or photovoltaic material processing, and specifically to a method and equipment for preparing electrodes of a silicon heterojunction battery. Background Art
[0002] Traditional silicon-based heterojunction cells require the use of expensive low-temperature silver paste to prepare the electrode grid lines of the cell. However, the cost of silver paste is high, and the silver paste contains a high proportion of resin particles as a curing agent. The resin particles themselves have poor conductivity. Therefore, the resistivity of the grid lines of traditional silicon-based heterojunction cells is high and the photoelectric conversion efficiency is low.
[0003] To address this issue, the industry is currently using electroplated copper grid lines to prepare copper electrodes, replacing the traditional low-temperature silver paste screen-printed electrode solution. Specifically, electroplated copper grid lines typically involve the following steps: first, a copper seed layer is preformed on the transparent conductive film of the silicon heterojunction cell using physical vapor deposition equipment. Then, a pattern is formed on the copper seed layer using dry film exposure and development. Subsequently, copper grid lines are electroplated. Finally, the dry film is removed by etching and cleaning to complete the preparation of the copper grid lines. The process of forming the pattern on the copper seed layer using dry film exposure and development requires the use of laser equipment or photolithography equipment. However, the cost of laser equipment or photolithography equipment increases significantly with the improvement of preparation accuracy, resulting in high costs. In addition, the grid lines produced by traditional laser equipment or photolithography equipment used to prepare metal grid lines are relatively wide, with large line spacing between grid lines, resulting in low photoelectric conversion efficiency. Therefore, the electroplated copper grid line technology requires the use of copper electroplating equipment to increase the height of the patterned grid lines, but the cost of copper electroplating equipment is also high. Therefore, how to improve the photoelectric conversion efficiency of solar cells and reduce the preparation cost of solar cell grid lines has become an urgent problem to be solved. Summary of the Invention
[0004] In order to solve the above technical problems, the present application is proposed. The embodiments of the present application provide a method and device for preparing electrodes of a silicon heterojunction battery.
[0005] In a first aspect, an embodiment of the present application provides a method for preparing an electrode of a silicon heterojunction battery, comprising: providing a substrate, the substrate having a silicon wafer and a metal layer; coating an imprinting adhesive on the metal layer to obtain an imprinting adhesive layer; imprinting the imprinting adhesive layer using an imprinting template to obtain an imprinted layer, wherein the imprinted layer comprises a plurality of first regions and a plurality of second regions, and the thickness of the first region is greater than the thickness of the second region; removing the imprinting layer located in the second region to expose the metal layer covered by the second region; removing the exposed metal layer to form a gate line on the unexposed metal layer; and removing the imprinting layer located in the first region to obtain a substrate having a gate line.
[0006] In some embodiments, the substrate further has a transparent conductive layer located between the silicon wafer and the metal layer, and the metal layer includes a copper layer and a tin layer. The substrate is provided, including: providing a substrate having a silicon wafer and a transparent conductive layer; preparing a copper layer on the transparent conductive layer; and preparing a tin layer on the copper layer to obtain the substrate.
[0007] In some embodiments, coating the embossed adhesive on the metal layer to obtain the embossed adhesive layer includes: coating the embossed adhesive on the metal layer by blade coating or spraying to obtain the embossed adhesive layer.
[0008] In some embodiments, after the embossing adhesive layer is embossed using the embossing template to obtain the embossed layer, the method further includes: curing the embossed layer by light curing or heat curing.
[0009] In some embodiments, removing the imprinting layer located in the second region includes: isotropically etching the imprinting layer by plasma etching to remove the imprinting layer located in the second region.
[0010] In some embodiments, the ratio of the thickness of the embossed layer in the first region to the thickness of the embossed layer in the second region is in a range of 3-10.
[0011] In some embodiments, removing the exposed metal layer includes: removing the exposed metal layer by wet etching.
[0012] In some embodiments, removing the imprinted layer in the first region to obtain the substrate having the gate lines includes: removing the imprinted layer in the first region by a solvent to obtain the substrate having the gate lines.
[0013] In some embodiments, the substrate has two transparent conductive layers and two metal layers; wherein one transparent conductive layer and one metal layer are located on a first side of the silicon wafer, and another transparent conductive layer and another metal layer are located on a second side of the silicon wafer.
[0014] In some embodiments, the gate lines include a plurality of main gate lines and a plurality of fine gate lines, the line width of the fine gate lines ranges from 0.5 micrometers to 5 micrometers, and / or the line spacing between adjacent fine gate lines ranges from 60 micrometers to 100 micrometers.
[0015] In some embodiments, the gate line has a thickness ranging from 1 micron to 2 microns.
[0016] In a second aspect, an embodiment of the present application provides an electrode preparation device for a silicon heterojunction battery, comprising: a metal plating device configured to prepare a metal layer on a pre-provided substrate surface to obtain a substrate, wherein the substrate has a silicon wafer and a transparent conductive layer; a coating device configured to coat an embossing glue on the metal layer to obtain an embossing glue layer; an imprinting device configured to imprint the embossing glue layer using an imprinting template to obtain an imprinted layer, wherein the imprinted layer includes a plurality of first regions and a plurality of second regions, and the thickness of the first region is greater than the thickness of the second region; a first removal device configured to remove the imprinting layer located in the second region to expose the metal layer covered by the second region; a second removal device configured to remove the exposed metal layer so that the unexposed metal layer forms a gate line; and a third removal device configured to remove the imprinting layer located in the first region to obtain a substrate having a gate line.
[0017] The electrode preparation method and apparatus for silicon heterojunction cells proposed in this application utilize an imprinting process to prepare an imprinted layer, thereby fabricating grid lines through the imprinted layer without the need for photoresist, laser equipment, or photolithography equipment. This reduces the metallization cost of silicon heterojunction cells. Furthermore, the imprinting process achieves high fabrication precision, enabling the production of thinner grid lines, allowing for the formation of more dense grid lines on the substrate surface, thereby improving photovoltaic conversion efficiency. This eliminates the need for copper electroplating equipment to increase grid line height, further reducing the metallization cost of silicon heterojunction cells. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The above and other purposes, features, and advantages of the present application will become more apparent through a more detailed description of the embodiments of the present application in conjunction with the accompanying drawings. The accompanying drawings are intended to provide a further understanding of the embodiments of the present application and constitute a part of the specification. Together with the embodiments of the present application, they are used to explain the present application and do not constitute a limitation of the present application. In the drawings, the same reference numerals generally represent the same components or steps.
[0019] Figure 1 Shown is a schematic flow chart of a method for preparing an electrode for a silicon heterojunction battery provided by an exemplary embodiment of the present application.
[0020] Figure 2 Shown is a schematic structural diagram of a copper layer prepared on a substrate provided by an exemplary embodiment of the present application.
[0021] Figure 3 Shown is a schematic structural diagram of a substrate provided by an exemplary embodiment of the present application.
[0022] Figure 4 FIG2 is a schematic structural diagram of a substrate with an embossed adhesive layer provided by an exemplary embodiment of the present application.
[0023] Figure 5 FIG2 is a schematic diagram showing an exemplary embodiment of the present application showing an embossing template embossing an embossing adhesive layer.
[0024] Figure 6 Shown is a schematic diagram of demoulding of an imprint template provided by an exemplary embodiment of the present application.
[0025] Figure 7 Shown is a schematic structural diagram of a copper layer on the other side of a substrate provided by an exemplary embodiment of the present application.
[0026] Figure 8 It is a schematic diagram of preparing a tin layer on a copper layer on the other side of a substrate provided by an exemplary embodiment of the present application.
[0027] Figure 9 Shown is a schematic structural diagram of an exemplary embodiment of the present application after an embossed adhesive layer is prepared on the other side of the substrate.
[0028] Figure 10 FIG2 is a schematic diagram showing an exemplary embodiment of the present application showing an imprint template imprinting an imprinting adhesive layer on the other side of a substrate.
[0029] Figure 11 Schematic diagram showing demoulding of the imprint template on the other side of the substrate provided by an exemplary embodiment of the present application.
[0030] Figure 12 FIG. 1 is a schematic structural diagram of a substrate provided by an exemplary embodiment of the present application, in which both sides have an imprinting layer.
[0031] Figure 13 Shown is a schematic structural diagram of a substrate after removing the exposed metal layer provided by an exemplary embodiment of the present application.
[0032] Figure 14 FIG2 is a schematic diagram of a structure after removing the embossing layer located in the first area provided by an exemplary embodiment of the present application.
[0033] Figure 15 Shown is a schematic flow chart of a method for preparing an electrode for a silicon heterojunction battery provided by another exemplary embodiment of the present application.
[0034] Figure 16 Shown is a schematic structural diagram of an electrode preparation device for a silicon heterojunction battery provided by an exemplary embodiment of the present application.
[0035] Reference numerals:
[0036] 200, substrate; 210, silicon wafer; 220, metal layer; 221, copper layer; 222, tin layer; 300, imprinting glue layer; 400, imprinting template; 500, imprinting layer; 510, first region; 520, second region; 700, electrode preparation equipment for silicon heterojunction battery; 701, metal plating device; 702, coating device; 703, imprinting device; 704, first removal device; 705, second removal device; 706, third removal device. DETAILED DESCRIPTION
[0037] The following will be combined with the drawings in the embodiments of this application to clearly and completely describe the technical solutions in the embodiments of this application. Obviously, the embodiments described are only part of the embodiments of this application, not all of the embodiments. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.
[0038] Application Overview
[0039] With technological advancements, solar photovoltaic (PV) power generation has become the second largest energy source after traditional coal-fired power generation due to its sustainability, pollution-free nature, widespread availability, and low cost. Every 1% increase in PV power generation efficiency translates to a 7% decrease in cost. Therefore, improving the efficiency of PV cells and reducing the cost per kilowatt-hour (COE) are key technological goals for PV power generation. Silicon-based heterojunction (HJT) cells, with their unique bifacial symmetry and the excellent passivation properties of the amorphous silicon layer, offer numerous advantages, including high conversion efficiency, high bifaciality, near-zero light-induced degradation (LID), excellent temperature characteristics, the ability to use thin wafers, and the ability to stack perovskites. Furthermore, their relatively short manufacturing process has led to their increasing interest within the industry. However, traditional HJT cells rely on low-temperature manufacturing processes, requiring the use of expensive low-temperature silver paste to fabricate the cell's electrode grid lines, resulting in high costs. Furthermore, the high proportion of resin particles in the silver paste, which act as a curing agent and have poor conductivity, contributes to the high resistivity of the HJT grid lines in conventional HJT cells.
[0040] In order to reduce the cost of electrode materials and improve the conductivity of heterojunction battery electrodes, the industry has begun to focus on the use of electroplating copper to prepare copper electrodes to replace the traditional low-temperature silver paste screen printing solution. Because copper electrodes do not contain non-conductive components, the resistivity of copper electrodes is low. Using copper electrodes instead of traditional low-temperature silver paste electrodes can not only significantly reduce the material cost of silver paste, but also effectively improve the photoelectric conversion efficiency of heterojunction battery cells. In related technologies, electroplating copper grid lines usually involves the following steps: first, a physical vapor deposition device is used to prefabricate a copper seed layer on the transparent conductive film of the silicon heterojunction battery, and then a dry film exposure and development is used on the copper seed layer to form a pattern, followed by electroplating of the copper grid lines, and finally, the dry film is removed by etching and cleaning to complete the preparation of the copper grid lines.
[0041] Among them, the process of forming a pattern on the copper seed layer using dry film exposure and development requires the use of laser equipment or photolithography equipment. However, the cost of laser equipment or photolithography equipment will increase significantly with the improvement of preparation precision, resulting in high costs. In addition, the line width of the gate lines produced by traditional laser equipment or photolithography equipment used to prepare metal gate lines is generally 15 to 25 microns. The gate line width is relatively wide, the line spacing between the gate lines is large, and the photoelectric conversion efficiency is low. Therefore, the electroplated copper gate line technology requires the use of copper electroplating equipment to increase the height of the patterned gate lines, but the copper electroplating equipment is also expensive. Therefore, how to improve the photoelectric conversion efficiency of solar cells and reduce the preparation cost of solar cell gate lines has become an urgent problem to be solved.
[0042] In view of this, the present application proposes a method for preparing electrodes for a silicon heterojunction cell. The method includes first providing a substrate having a silicon wafer, a transparent conductive layer, and a metal layer, and coating the metal layer with an imprinted adhesive to obtain an imprinted adhesive layer. The imprinted adhesive layer is then imprinted using an imprinting template to obtain an imprinted layer, wherein the imprinted layer includes a plurality of first regions and a plurality of second regions, and the thickness of the first regions is greater than that of the second regions. The imprinted layer located in the second regions is then removed to expose the metal layer covered by the second regions. The exposed metal layer is then removed to form grid lines in the unexposed metal layer. Finally, the imprinted layer located in the first regions is removed to obtain a substrate having grid lines. In the present application, since the imprinted layer is prepared using an imprinting process, the grid lines can be prepared using the imprinted layer without the need to use photoresist, laser equipment, or photolithography equipment to prepare the grid lines, thereby reducing the cost of metallization of the silicon heterojunction cell. In addition, the imprinting process can achieve higher preparation accuracy and can produce thinner grid lines, so that more and denser grid lines can be formed on the substrate surface, thereby improving the photovoltaic conversion efficiency. This eliminates the need to use copper electroplating equipment to increase the height of the grid lines, further reducing the cost of metallization of silicon heterojunction cells.
[0043] Exemplary Methods
[0044] Figure 1Shown is a schematic flow chart of a method for preparing an electrode for a silicon heterojunction battery provided by an exemplary embodiment of the present application. Figure 2 Shown is a schematic structural diagram of a copper layer prepared on a substrate provided by an exemplary embodiment of the present application. Figure 3 Shown is a schematic structural diagram of a substrate provided by an exemplary embodiment of the present application. Figure 4 FIG2 is a schematic structural diagram of a substrate with an embossed adhesive layer provided by an exemplary embodiment of the present application. Figure 5 FIG2 is a schematic diagram showing an exemplary embodiment of the present application showing an embossing template embossing an embossing adhesive layer. Figure 6 Shown is a schematic diagram of demoulding of an imprint template provided by an exemplary embodiment of the present application. Figure 7 Shown is a schematic structural diagram of a copper layer on the other side of a substrate provided by an exemplary embodiment of the present application. Figure 8 It is a schematic diagram of preparing a tin layer on a copper layer on the other side of a substrate provided by an exemplary embodiment of the present application. Figure 9 Shown is a schematic structural diagram of an exemplary embodiment of the present application after an embossed adhesive layer is prepared on the other side of the substrate. Figure 10 FIG2 is a schematic diagram showing an exemplary embodiment of the present application showing an imprint template imprinting an imprinting adhesive layer on the other side of a substrate. Figure 11 Schematic diagram showing demoulding of the imprint template on the other side of the substrate provided by an exemplary embodiment of the present application. Figure 12 FIG. 1 is a schematic structural diagram of a substrate provided by an exemplary embodiment of the present application, in which both sides have an imprinting layer. Figure 13 Shown is a schematic structural diagram of a substrate after removing the exposed metal layer provided by an exemplary embodiment of the present application. Figure 14 FIG2 is a schematic diagram of a structure after removing the embossing layer located in the first area provided by an exemplary embodiment of the present application.
[0045] like Figures 1 to 14 As shown, the method for preparing an electrode of a silicon heterojunction battery provided in an embodiment of the present application includes the following steps 101 to 106.
[0046] Step 101: Provide a substrate.
[0047] Among them, Figure 2 and Figure 3 As shown, the substrate 200 includes a silicon wafer 210 and a metal layer 220 . The metal layer 220 may exemplarily include a copper layer 221 . The copper layer 221 has the characteristics of low cost and low resistivity.
[0048] In some embodiments, the copper layer 221 has a thickness ranging from 0.5 micrometers to 10 micrometers. Preferably, the copper layer 221 has a thickness ranging from 1 micrometer to 2 micrometers.
[0049] In some embodiments, the substrate 200 further has a transparent conductive layer (not shown) located between the silicon wafer 210 and the metal layer 220, and the metal layer 220 includes a copper layer 221 and a tin layer 222. When providing the substrate, a substrate can be provided first, and the substrate has a silicon wafer 210 and a transparent conductive layer; then, a copper layer 221 is prepared on the transparent conductive layer; and a tin layer 222 is prepared on the copper layer 221 to obtain the substrate 200.
[0050] Specifically, the transparent conductive layer can be exemplarily a transparent conductive oxide film layer (Transparent Conductive Oxide, TCO). When preparing the copper layer 221 on the transparent conductive layer, exemplarily a physical vapor deposition (PVD) device can be used for preparation, that is, the copper layer 221 is deposited on the transparent conductive layer by a physical vapor deposition method; when preparing the tin layer 222 on the copper layer 221, exemplarily a PVD device can be used for preparation, that is, the tin layer 222 is deposited on the copper layer 221 by a physical vapor deposition method. The thickness of the tin layer 222 is exemplarily in the range of 0.5 to 5 microns. By providing the tin layer 222 on the surface of the copper layer 221, the copper layer 221 can be prevented from being oxidized, thereby preventing the gate line made of the copper layer 221 from failing.
[0051] Step 102: Coat embossed adhesive on the metal layer to obtain an embossed adhesive layer.
[0052] The embossed adhesive layer 300 is exemplarily as follows: Figure 4 shown.
[0053] In some embodiments, the embossed adhesive can be applied to the metal layer 220 by blade coating or spraying to obtain the embossed adhesive layer 300. The embossed adhesive can be evenly applied to the metal layer 220 by blade coating or spraying, so that the embossed adhesive layer 300 evenly covers the metal layer 220.
[0054] Step 103: Use an embossing template to emboss the embossed adhesive layer to obtain an embossed layer.
[0055] The embossing template 400 is embossed as follows: Figure 5 As shown, the imprint template 400 can be a nanoimprint template, and the imprint layer 500 can be a nanoimprint template. Figure 6 Specifically, the embossing template 400 is designed based on the gate line morphology. After the embossing adhesive layer 300 is embossed with the embossing template 400, the embossing layer 500 includes a plurality of first regions 510 and a plurality of second regions 520. The thickness of the first regions 510 is greater than that of the second regions 520. The first regions 510 are used to cover the regions of the metal layer 220 where the gate lines are to be formed, and the second regions 520 are used to cover the regions of the metal layer 220 where the gate lines are to be formed.
[0056] In some embodiments, after the embossing adhesive layer 300 is embossed using the embossing template 400 to obtain the embossing layer 500 , the embossing layer 500 may be cured by light curing or heat curing to prevent deformation of the embossing layer 500 .
[0057] In some embodiments, after the embossing adhesive layer 300 is embossed into the embossing layer 500 using the embossing template 400 , the embossing template 400 needs to be demolded.
[0058] In some embodiments, the ratio of the thickness of the imprinting layer 500 located in the first region 510 to the thickness of the imprinting layer 500 located in the second region 520 is in a range of 3 to 10. By making the thickness of the imprinting layer 500 located in the first region 510 much thicker than the thickness of the imprinting layer 500 located in the second region 520, it is ensured that when the imprinting layer 500 located in the second region 520 is removed using an isotropic etching method, the imprinting layer 500 located in the first region 510 is not completely removed.
[0059] If gate lines need to be prepared on both sides of the substrate 200, in some embodiments, the substrate 200 has two transparent conductive layers and two metal layers 220; wherein, one transparent conductive layer and one metal layer 220 are located on the first side of the silicon wafer 210, and the other transparent conductive layer and another metal layer 220 are located on the second side of the silicon wafer 210.
[0060] Specifically, a transparent conductive layer can be first prepared on both sides of the silicon wafer 210. Then, according to the above steps 101 to 103, a metal layer 220, an imprinted adhesive layer 300, and an imprinted layer 500 are sequentially prepared on one surface of the silicon wafer 210. Then, according to the above steps 101 to 103, a metal layer 220, an imprinted adhesive layer 300, and an imprinted layer 500 are sequentially prepared on the other surface of the silicon wafer 210. Thus, both sides of the silicon wafer have a transparent conductive layer, a metal layer 220, and an imprinted layer 500, and then subsequent steps 104 to 106 are performed.
[0061] Step 104 : removing the imprint layer located in the second area to expose the metal layer covering the second area.
[0062] Specifically, the imprinting layer 500 can be processed by an isotropic etching method. Since the thickness of the first region 510 is greater than the thickness of the second region 520, when the imprinting layer 500 located in the first region 510 and the imprinting layer 500 located in the second region 520 are removed equally, the imprinting layer 500 in the second region 520 can be removed while the imprinting layer 500 in the first region 510 still remains.
[0063] In some embodiments, when removing the imprinted layer in the second region 520, the imprinted layer 500 can be isotropically etched using plasma etching to remove the imprinted layer 500 in the second region 520. That is, the substrate 200 having the imprinted layer 500 can be placed in a plasma etching device for processing. Using plasma etching, the imprinted layer 500 in the first region 510 and the second region 520 can be etched to the same thickness. Thus, while the thinner imprinted layer 500 in the second region 520 is removed, the thicker portion of the imprinted layer 500 in the first region 510 remains, thereby protecting the portion of the metal layer 220 where the gate lines are to be formed.
[0064] In some embodiments, if gate lines need to be formed on both sides of the substrate 200 , the imprinting layer 500 located in the second region on both sides of the substrate 200 may be removed simultaneously in step 104 .
[0065] Step 105 : removing the exposed metal layer to form gate lines on the unexposed metal layer.
[0066] The gate lines formed by the metal layer 220 are as follows: Figure 13 As shown (i.e. Figure 13 Specifically, the imprinted layer 500 in the first region 510 can protect the covered metal layer 220. When the substrate 200 having the imprinted layer 500 in the first region 510 is etched, only the metal layer 220 not covered by the imprinted layer 500 in the first region 510 is etched, thereby forming the protected metal layer 220 into a gate line shape.
[0067] In some embodiments, when removing the exposed metal layer 220, the exposed metal layer 220 can be removed by wet etching. Specifically, the substrate 200 after removing the imprinted layer 500 located in the second region can be placed in a wet etching device for processing. The wet etching device contains a solution that can dissolve the metal layer 220. Therefore, the exposed metal layer 220 will be etched, while the imprinted layer 500 located in the first region 510 can protect the covered metal layer 220, so that the covered metal layer 220 forms a gate line.
[0068] In a specific example, a solution capable of dissolving copper and tin is contained in the wet etching equipment, and the metal layer 220 includes a copper layer 221 and a tin layer 222 , so that the exposed copper layer 221 and the tin layer 222 can be etched.
[0069] In some embodiments, if gate lines need to be formed on both sides of the substrate 200 , the exposed metal layers 220 on both sides of the substrate 200 may be removed simultaneously in step 105 .
[0070] Step 106 : removing the imprinted layer in the first area to obtain a substrate with gate lines.
[0071] Among them, the substrate with gate lines is as follows Figure 14 As shown (the grid lines are Figure 14 The copper layer 221 in the embodiment of the present invention.
[0072] In some embodiments, when removing the imprinting layer 500 located in the first region 510 to obtain the substrate 200 with gate lines, the imprinting layer 500 located in the first region 510 may be removed by a solvent to obtain the substrate 200 with gate lines.
[0073] The solvent is exemplarily water, which has a low cost for removing the imprint layer 500 located in the first region 510. The solvent may also be a high-temperature solvent, which can remove the imprint layer 500 located in the first region 510 more quickly.
[0074] In some embodiments, if gate lines need to be formed on both sides of the substrate 200 , the imprinting layer 500 located in the first region 510 on both sides of the substrate 200 may be removed simultaneously in step 106 .
[0075] In the above embodiment, since the imprinting process is used to prepare the imprinted layer 500, the gate lines can be formed through the imprinted layer 500 without the need to use photoresist, laser equipment, or photolithography equipment to prepare the gate lines, thereby reducing the metallization cost of the silicon heterojunction cell. In addition, the imprinting process can achieve higher preparation accuracy and can produce thinner gate lines, so that more and denser gate lines can be formed on the surface of the substrate 200, thereby improving the photovoltaic conversion efficiency. This eliminates the need to use copper electroplating equipment to increase the height of the gate lines, further reducing the metallization cost of the silicon heterojunction cell.
[0076] In some embodiments, the grid lines include multiple main grid lines and multiple fine grid lines. The width of the fine grid lines ranges from 0.5 microns to 5 microns, and / or the spacing between adjacent fine grid lines ranges from 60 microns to 100 microns. By manufacturing finer and denser grid lines, the photoelectric conversion efficiency of the photovoltaic cell can be greatly improved.
[0077] In some embodiments, the distance between adjacent main grid lines ranges from 6 mm to 12 mm.
[0078] In some embodiments, the gate line has a thickness ranging from 1 micron to 2 microns. The gate line prepared by the electrode preparation method of the silicon heterojunction cell provided by the embodiment of the present application is thinner, which reduces the degree of light blocking by the gate line, thereby improving the photovoltaic conversion efficiency of the cell.
[0079] In a specific example, a 182 mm Taking a cell of millimeters as an example, there are 1035 fine grid lines arranged in parallel on the surface of the cell, the line spacing between adjacent fine grid lines is 86 microns, the length of the fine grid lines is 180 mm, and the width is 2 microns. At the same time, there are main grid lines perpendicular to the fine grid lines on the surface of the cell, and there are 18 main grid lines arranged in parallel on the surface of the cell, the line spacing between adjacent main grid lines is 9.58 mm, the length of the main grid lines is 89 mm, the height of the main grid lines is 1.5 microns, and the line width of the main grid lines is 300 microns. That is, the electrode preparation method of the silicon heterojunction battery provided by the embodiment of the present application, the manufactured cell has an extremely fine grid line width and a smaller line spacing between the grid lines, thereby greatly improving the photoelectric conversion efficiency of the cell.
[0080] Figure 15 FIG. 1 is a flow chart of a method for preparing an electrode of a silicon heterojunction battery provided by another exemplary embodiment of the present application. Figures 2 to 15 As shown, another method for preparing an electrode for a silicon heterojunction battery provided in an embodiment of the present application includes the following steps 601 to 614. To facilitate distinguishing the transparent conductive layer, copper layer 221, tin layer 222, imprint layer 500, imprint adhesive layer 300, and imprint template 400 located on both sides of the substrate 200, the following description uses the terms first and second to distinguish the transparent conductive layer, copper layer 221, tin layer 222, imprint layer 500, imprint adhesive layer 300, and imprint template 400 located on different sides of the substrate 200.
[0081] Step 601: Provide a substrate.
[0082] The substrate includes a silicon wafer 210 , a first transparent conductive layer disposed on the upper surface of the silicon wafer 210 , and a second transparent conductive layer disposed on the lower surface of the silicon wafer 210 .
[0083] Step 602: Prepare a first copper layer on the first transparent conductive layer by physical vapor deposition.
[0084] Step 603: Prepare a first tin layer on the first copper layer by physical vapor deposition.
[0085] Step 604 : Coat embossing adhesive on the first tin layer to obtain a first embossing adhesive layer.
[0086] Step 605 : Use a first embossing template to emboss the first embossed adhesive layer to obtain a first embossed layer.
[0087] Step 606 : Curing the first embossing layer and removing the first embossing template.
[0088] Step 607: Prepare a second copper layer on the second transparent conductive layer by physical vapor deposition.
[0089] Step 608 : Prepare a second tin layer on the second copper layer by physical vapor deposition.
[0090] Step 609 : Coat embossing adhesive on the second tin layer to obtain a second embossing adhesive layer.
[0091] Step 610: Use a second embossing template to emboss the second embossed adhesive layer to obtain a second embossed layer.
[0092] Step 611 : Curing the second embossing layer and removing the second embossing template.
[0093] Step 612: Etch the substrate having the first imprinting layer and the second imprinting layer by a plasma etching method to remove the first imprinting layer located in the second area and the second imprinting layer located in the second area.
[0094] Step 613 , etching the substrate from which the first imprinted layer located in the second area and the second imprinted layer located in the second area have been removed by a wet etching method to remove the exposed first copper layer, first tin layer, second copper layer, and second tin layer.
[0095] Step 614 : remove the first embossing layer located in the first area and the second embossing layer located in the first area.
[0096] Exemplary devices
[0097] Combined with the above Figures 1 to 15 , describes the method embodiment of the present application in detail, and the following is combined with Figure 16 , the device embodiment of the present application is described in detail. It should be understood that the description of the method embodiment corresponds to the description of the device embodiment, so for parts not described in detail, reference can be made to the previous method embodiment.
[0098] Figure 16 FIG. 1 is a schematic diagram of the structure of an electrode preparation device for a silicon heterojunction battery provided by an exemplary embodiment of the present application. Figure 16As shown, the electrode preparation equipment 700 for the silicon heterojunction battery provided in the embodiment of the present application includes: a metal plating device 701, configured to prepare a metal layer on the surface of a pre-provided substrate to obtain a substrate, wherein the substrate has a silicon wafer and a transparent conductive layer; a coating device 702, configured to coat an imprinting glue on the metal layer to obtain an imprinting glue layer; an imprinting device 703, configured to imprint the imprinting glue layer using an imprinting template to obtain an imprinted layer, wherein the imprinted layer includes a plurality of first regions and a plurality of second regions, and the thickness of the first region is greater than the thickness of the second region; a first removal device 704, configured to remove the imprinting layer located in the second region to expose the metal layer covered by the second region; a second removal device 705, configured to remove the exposed metal layer so that the unexposed metal layer forms a gate line; a third removal device 706, configured to remove the imprinting layer located in the first region to obtain a substrate with a gate line.
[0099] Among them, the metal plating device 701 is exemplarily a physical vapor deposition (PVD) device, the coating device 702 is exemplarily a glue coater, the imprinting device 703 is exemplarily a glue stamper, the first removal device 704 is exemplarily a plasma etcher, the second removal device 705 is exemplarily a wet etcher, and the third removal device 706 is exemplarily a wet glue stripper.
[0100] In some embodiments, the metal layer includes a copper layer and a tin layer, the substrate has a silicon wafer and a transparent conductive layer, and the metallization device 701 is configured to: prepare a copper layer on the transparent conductive layer; prepare a tin layer on the copper layer to obtain a substrate.
[0101] In some embodiments, the coating device 702 is configured to coat the embossing adhesive on the metal layer by scraping or spraying to obtain an embossing adhesive layer.
[0102] In some embodiments, the imprinting device 703 is configured to cure the imprinting layer by light curing or heat curing.
[0103] In some embodiments, the first removal device 704 is configured to isotropically etch the imprinting layer by plasma etching to remove the imprinting layer located in the second region.
[0104] In some embodiments, the ratio of the thickness of the embossed layer in the first region to the thickness of the embossed layer in the second region is in a range of 3-10.
[0105] In some embodiments, the second removing device 705 is configured to remove the exposed metal layer by wet etching.
[0106] In some embodiments, the third removing device 706 is configured to remove the imprinting layer located in the first region by using a solvent to obtain a substrate having gate lines.
[0107] In some embodiments, the substrate has two transparent conductive layers and two metal layers; wherein one transparent conductive layer and one metal layer are located on a first side of the silicon wafer, and another transparent conductive layer and another metal layer are located on a second side of the silicon wafer.
[0108] In some embodiments, the gate lines include a plurality of main gate lines and a plurality of fine gate lines, the line width of the fine gate lines ranges from 0.5 micrometers to 5 micrometers, and / or the line spacing between adjacent fine gate lines ranges from 60 micrometers to 100 micrometers.
[0109] In some embodiments, the gate line has a thickness ranging from 1 micron to 2 microns.
[0110] The basic principles of the present application have been described above in conjunction with specific embodiments. However, it should be noted that the advantages, strengths, and effects mentioned in this application are merely illustrative and not restrictive, and it should not be assumed that these advantages, strengths, and effects are required of each embodiment of this application. In addition, the specific details disclosed above are merely illustrative and facilitating understanding, and are not restrictive. The above details do not limit this application to necessarily being implemented using the above specific details.
[0111] The block diagrams of the devices, devices, equipment, and systems involved in this application are merely illustrative examples and are not intended to require or imply that they must be connected, arranged, or configured in the manner shown in the block diagrams. As will be appreciated by those skilled in the art, these devices, devices, equipment, and systems can be connected, arranged, or configured in any manner. Words such as "include," "comprise," "have," and the like are open-ended words, meaning "including but not limited to," and can be used interchangeably therewith. The words "or" and "and" used herein refer to the words "and / or" and can be used interchangeably therewith, unless the context clearly indicates otherwise. The word "such as" used herein refers to the phrase "such as but not limited to," and can be used interchangeably therewith.
[0112] It should also be noted that in the apparatus, device, and method of the present application, each component or each step can be decomposed and / or recombined, and such decomposition and / or recombination should be regarded as equivalent solutions of the present application.
[0113] The above description of the disclosed aspects is provided to enable any person skilled in the art to make or use the present application. Various modifications to these aspects will be readily apparent to those skilled in the art, and the general principles defined herein may be applied to other aspects without departing from the scope of the present application. Therefore, the present application is not intended to be limited to the aspects shown herein, but rather to be accorded the widest scope consistent with the principles and novel features disclosed herein.
[0114] The above description has been provided for the purpose of illustration and description. Furthermore, this description is not intended to limit the embodiments of the present application to the forms disclosed herein. Although a number of example aspects and embodiments have been discussed above, those skilled in the art will recognize certain variations, modifications, alterations, additions, and sub-combinations thereof.
Claims
1. A method for preparing an electrode for a silicon heterojunction battery, characterized in that: include: Providing a substrate, wherein the substrate has a silicon wafer and a metal layer; Coating an embossed adhesive on the metal layer to obtain an embossed adhesive layer; Using an embossing template to emboss the embossed adhesive layer to obtain an embossed layer, wherein the embossed layer includes a plurality of first regions and a plurality of second regions, and the thickness of the first regions is greater than the thickness of the second regions; removing the embossing layer located in the second area to expose the metal layer covered by the second area; removing the exposed metal layer, so that the unexposed metal layer forms a gate line; The embossing layer located in the first area is removed to obtain a substrate with gate lines.
2. The method for preparing an electrode for a silicon heterojunction battery according to claim 1, characterized in that: The substrate further comprises a transparent conductive layer between the silicon wafer and the metal layer, wherein the metal layer comprises a copper layer and a tin layer. The substrate is provided, comprising: Providing a substrate, wherein the substrate has the silicon wafer and the transparent conductive layer; preparing the copper layer on the transparent conductive layer; The tin layer is prepared on the copper layer to obtain the substrate.
3. The method for preparing an electrode for a silicon heterojunction battery according to claim 1 or 2, characterized in that: The step of coating the embossed adhesive on the metal layer to obtain the embossed adhesive layer comprises: The embossed adhesive is coated on the metal layer by scraping or spraying to obtain the embossed adhesive layer.
4. The method for preparing an electrode for a silicon heterojunction battery according to claim 1 or 2, characterized in that: After the embossed adhesive layer is embossed using the embossing template to obtain the embossed layer, the method further includes: The embossing layer is cured by light curing or heat curing.
5. The method for preparing an electrode for a silicon heterojunction battery according to claim 1 or 2, characterized in that: The removing the embossing layer located in the second area comprises: The imprinting layer is isotropically etched by plasma etching to remove the imprinting layer located in the second area.
6. The method for preparing an electrode for a silicon heterojunction battery according to claim 5, characterized in that: The ratio of the thickness of the embossing layer located in the first area to the thickness of the embossing layer located in the second area is in the range of 3-10.
7. The method for preparing an electrode for a silicon heterojunction battery according to claim 1 or 2, characterized in that: The removing the exposed metal layer comprises: The exposed metal layer is removed by wet etching.
8. The method for preparing an electrode for a silicon heterojunction battery according to claim 1 or 2, characterized in that: The step of removing the imprinting layer located in the first area to obtain a substrate having gate lines comprises: The printed layer located in the first area is removed by using a solvent to obtain the substrate having the gate lines.
9. The method for preparing an electrode for a silicon heterojunction battery according to claim 1 or 2, characterized in that: The substrate has two transparent conductive layers and two metal layers; Wherein, one of the transparent conductive layers and one of the metal layers are located on a first side of the silicon wafer, and another of the transparent conductive layers and another of the metal layers are located on a second side of the silicon wafer.
10. The method for preparing an electrode for a silicon heterojunction battery according to claim 2, characterized in that: The gate lines include a plurality of main gate lines and a plurality of fine gate lines, the line width of the fine gate lines ranges from 0.5 micrometers to 5 micrometers, and / or the line spacing between adjacent fine gate lines ranges from 60 micrometers to 100 micrometers.
11. The method for preparing an electrode for a silicon heterojunction battery according to claim 1 or 2, characterized in that: The thickness of the gate line ranges from 1 micron to 2 microns.
12. An electrode preparation device for a silicon heterojunction battery, characterized in that: include: A metal plating device, configured to prepare a metal layer on a surface of a pre-provided substrate to obtain a base plate, wherein the substrate has a silicon wafer and a transparent conductive layer; A coating device, configured to coat the embossed adhesive on the metal layer to obtain an embossed adhesive layer; An embossing device, configured to emboss the embossed adhesive layer using an embossing template to obtain an embossed layer, wherein the embossed layer includes a plurality of first regions and a plurality of second regions, and a thickness of the first region is greater than a thickness of the second region; A first removing device is configured to remove the stamping layer located in the second area to expose the metal layer covered by the second area; A second removing device is configured to remove the exposed metal layer so that the unexposed metal layer forms a gate line; The third removing device is configured to remove the imprinting layer located in the first area to obtain a substrate with gate lines.