Phosphate positive electrode material and preparation method and application thereof
By doping high-valence metal elements and Li-site doping with Mg and Zr in the phosphate cathode material, and forming a carbon coating layer, the problems of low conductivity and high Fe/Mn ion elution rate are solved, significantly improving the lithium Kinetic and electrochemical properties of batteries.
Patent Information
- Application Number
- CN202410867967.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-28
AI Technical Summary
Existing phosphate cathode materials in lithium batteries have problems such as low conductivity, poor ion diffusion performance, poor rate performance and low temperature performance, and the dissolution of Fe and Mn ions leads to unsatisfactory self-discharge rate and cycle performance.
Doping high-valence metal elements such as Ti, V, Cr, Co, Ni, Nb, Mo, W, and Li-site doping Mg and Zr is used to form a carbon coating layer to improve the lithium diffusion coefficient and conductivity, and through control The disorder and doping amount of carbon materials reduce the dissolution rate of Fe/Mn ions and inhibit side reactions.
It significantly improves the rate performance, low-temperature performance and cycle performance of phosphate cathode materials, reduces the dissolution rate of Fe/Mn ions, and improves the self-discharge rate and storage performance of lithium batteries.
Smart Images

Figure CN118738336A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium batteries, and in particular to a phosphate-based positive electrode material and a preparation method and application thereof. Background Art
[0002] Lithium-ion batteries have the advantages of high energy density, low self-discharge, long cycle life, safety and environmental protection, and are therefore widely used in consumer electronics, electric vehicles, power and communication energy storage and other fields. According to the different positive electrode materials, lithium-ion batteries can be divided into lithium cobalt oxide batteries, lithium manganese oxide batteries, ternary lithium batteries, lithium iron phosphate batteries, etc., corresponding to the positive electrode materials lithium cobalt oxide (LCO), lithium manganese oxide (LMO), ternary nickel cobalt manganese oxide (NMC) and ternary nickel cobalt aluminum oxide (NCA), etc. Among them, the preparation cost of lithium cobalt oxide LCO, ternary nickel cobalt manganese oxide NMC and ternary nickel cobalt aluminum oxide NCA is relatively high, which limits their application scope to a certain extent. Although the price of spinel lithium manganese oxide LMO is relatively low, its energy density and cycle life are slightly lower, which is not conducive to the application of LMO in high-end products.
[0003] In order to reduce the cost of lithium batteries and maintain good application performance, research on phosphate-based active materials that do not contain precious metal elements (nickel, cobalt, manganese) has gradually attracted attention. Currently, the commonly used phosphate-based active materials mainly include lithium iron phosphate (LFP), lithium manganese phosphate (LMP), lithium manganese iron phosphate (LMFP), etc.
[0004] Lithium iron phosphate (LFP) is widely used in passenger car power batteries, commercial vehicle power batteries, power communication energy storage batteries and other fields due to its stable structure, abundant reserves of the main elements Fe and P, low price, ultra-long cycle life and high safety. However, due to its olivine structure (such as Figure 1 As shown in the figure, LFP has low conductivity, poor ion diffusion performance, and poor rate performance and low temperature performance.
[0005] The crystal structure of lithium manganese phosphate LMP is basically the same as that of lithium iron phosphate LFP, and there is obvious polarization phenomenon during the charging process. When used in lithium batteries, it will significantly reduce the capacity and power density of lithium batteries.
[0006] Lithium manganese iron phosphate LMFP is a product of lithium manganese iron phosphate LFP and lithium manganese phosphate LMP. The crystal structure of lithium manganese iron phosphate LMFP and lithium iron phosphate LFP is basically the same. LMFP has the same advantages as LFP, and has a higher discharge voltage than LFP, and has a higher energy density at a similar discharge capacity. However, the constant voltage ratio of lithium manganese iron phosphate LMFP is relatively large, so it is not suitable for energy storage batteries, and the cycle life is short and the capacity is difficult to exert.
[0007] Moreover, after the above-mentioned phosphate-based active materials are used in lithium batteries, there is still the problem of Fe and Mn dissolution. The dissolved iron ions and / or manganese ions will migrate to the negative electrode to form heterogeneous catalytic active centers, catalyzing the decomposition of the electrolyte and the negative electrode SEI film, affecting the self-discharge rate, cycle performance and storage performance of the lithium-ion battery, which is not conducive to the improvement of the ion conductivity and rate performance of the lithium battery.
[0008] Therefore, it is urgent to develop a phosphate-based positive electrode active material that can have both excellent electrochemical properties and low ion dissolution rate, thereby significantly improving the kinetic and electrochemical properties of lithium batteries. Summary of the invention
[0009] In order to improve the electrochemical performance of phosphate-based positive electrode materials and reduce their ion dissolution rate, the present application provides a phosphate-based positive electrode material and a preparation method and application thereof.
[0010] In a first aspect, the present application provides a phosphate-based positive electrode material, which adopts the following technical solution:
[0011] A phosphate-based positive electrode material, comprising a base particle and a carbon coating layer coated on the surface of the base particle; the chemical formula of the base particle is Li x M y PO 4 , 0.96≤x≤1.08, 0.96≤y≤1, M includes at least one of Fe and Mn;
[0012] Wherein, the M position is doped with a first metal element, the first metal element includes at least one of Ti, V, Cr, Co, Ni, Nb, Mo, and W; and / or, the Li position is doped with a second metal element, the second metal element includes at least one of Mg and Zr;
[0013] The carbon coating layer includes a carbon material, and the disorder degree of the carbon material is D / I G ≤1.2.
[0014] There are two typical scattering peaks in the Raman spectrum of carbon materials, one is the D peak, located at 1350cm -1 Nearby, there is a peak called G, located at 1580cm -1 Nearby, I D 1300cm in Raman spectrum -1 Up to 1400cm -1 The peak intensity of the inner D peak, I G 1530cm in Raman spectrum -1 To 16300cm -1 Peak intensity of inner G peak.
[0015] First, on the one hand, by doping high-valent metal elements at the M position, not only can local lithium vacancies be created to increase the lithium diffusion coefficient, but also vacancy defects can be formed in the material lattice and a narrower TDOS band gap can be generated, thereby improving the ionic conductivity of the positive electrode material and improving its rate performance and low-temperature performance; on the other hand, by doping Mg and Zr elements at the Li position, not only local lithium vacancies can be created to increase the lithium diffusion coefficient, but also the lithium layer channel can be expanded and the lithium ion deintercalation resistance can be reduced, thereby improving the rate performance and ionic conductivity of the positive electrode material. Second, due to I D and I G Corresponding to the sp 3 Hybridization and sp 2 hybridization, where the highest peak intensity ratio of D peak and G peak (I D / I G ) is smaller, indicating that the disorder degree of the carbon material is lower and the degree of graphitization is higher. By coating the substrate with a carbon material with low disorder and high graphitization, the electrochemical activity of the positive electrode material can be significantly improved. The coating layer has a high degree of graphitization, which can reduce the impedance of the material interface, thereby significantly reducing the charge transfer impedance of the material, which helps to further improve the rate performance and low temperature performance of the positive electrode material. Third, the defect pairs in the carbon coating layer will promote the side reactions of the phosphate-based positive electrode materials in the electrolyte to a certain extent, and the doping of the first metal element and the second metal element can inhibit the above-mentioned promotion effect, and also help to reduce the degree of degradation of the materials in the carbon coating layer caused by the side reactions, avoid the increase of disorder in the carbon coating layer during the cycle of the lithium battery, and improve the stability of the carbon coating layer; and the stable carbon coating layer can stably coat the matrix particles, reduce the dissolution of Mn and Fe in the matrix particles, thereby reducing the deposition amount of Fe / Mn ions dissolved and migrated from the positive electrode to the negative electrode, reduce the catalytic decomposition of the electrolyte and the catalytic decomposition of the negative electrode SEI film, and thus improve the self-discharge rate and cycle performance of the lithium battery. Fourth, the doping of high-valent metal elements and the presence of the carbon coating layer can significantly reduce the dissolution of Fe / Mn in the positive electrode material, which will largely avoid the negative impact of the dissolution of Fe / Mn ions on the electrolyte and the negative electrode SEI film, and improve the self-discharge rate, cycle performance and storage performance of the lithium-ion battery.
[0016] Preferably, the carbon content in the phosphate-based positive electrode material is 1 wt%-2 wt%.
[0017] By controlling the carbon content in the phosphate-based positive electrode material and increasing the content of graphitized carbon in the phosphate-based positive electrode material, the electrochemical performance of the phosphate-based positive electrode material can be significantly improved; when the mass percentage of the carbon coating layer is too low, an effective conductive network structure cannot be constructed in the positive electrode active material layer formed by the phosphate-based positive electrode active material, causing the battery impedance and polarization to be too large and resulting in battery performance degradation; and when the mass percentage of the carbon coating layer is too high, the defects in the carbon material will act as active sites to aggravate the degree of side reactions of the positive electrode in the electrolyte, and the side reaction products will block the lithium ion transmission pores of the carbon coating layer, and even seriously destroy the order of the carbon coating layer, thereby significantly increasing the battery impedance and consuming active lithium to cause the lithium battery capacity to decay rapidly.
[0018] Preferably, the doping amount of the first metal element is ≤5000 ppm.
[0019] Preferably, the doping amount of the second metal is ≤3000 ppm.
[0020] By controlling the doping amounts of the first metal element and the second metal element, the generation of impurity phases can be avoided, and the occurrence of residual lithium on the positive electrode surface that causes a decrease in the initial capacity of the material can be avoided.
[0021] Preferably, the particle size D50 of the phosphate-based positive electrode material is 50-2000 nm.
[0022] Preferably, the particle size D50 of the phosphate-based positive electrode material refers to the particle size D50 of primary particles of the phosphate-based positive electrode material observed in SEM detection.
[0023] Preferably, the compaction density of the phosphate-based positive electrode material is 2-2.7 g / cm 3 .
[0024] By controlling the reasonable particle grading of the phosphate-based positive electrode material, the phosphate-based positive electrode material can obtain a relatively wide range of compaction density, thereby improving the application scope of the positive electrode material of the present application.
[0025] In a second aspect, the present application provides a method for preparing a phosphate-based positive electrode material, using the following technical solution:
[0026] A method for preparing a phosphate-based positive electrode material comprises the following steps:
[0027] S1, mixing an iron source, a manganese source, a lithium source, and a doping source, adding water, and then grinding to obtain a premixed slurry;
[0028] S2, spray-drying, sintering and then crushing the premixed slurry to obtain a phosphate-based positive electrode material.
[0029] Preferably, the iron source comprises FePO4 , Fe 2 O 3 、FeC 2 O 4 At least one of; the manganese source includes MnPO 4 、MnCO 3 , Mn 3 O 4 At least one of; the lithium source includes Li 2 CO 3 、LiOH.H 2 O, LiCl, Li 2 SO 4 , Li 2 HPO 4 , LiH 2 PO 4 , Li 3 PO 4 、LiNO 3 At least one of;
[0030] The doping source comprises an M-site doping source and a Li-site doping source, wherein the M-site doping source comprises at least one of Ti salts and oxides thereof, V salts and oxides thereof, Cr salts and oxides thereof, Co salts and oxides thereof, Ni salts and oxides thereof, Nb salts and oxides thereof, Mo salts and oxides thereof, and W salts and oxides thereof, and the Li-site doping source comprises at least one of Mg salts and oxides thereof, and Zr salts and oxides thereof;
[0031] The carbon source includes a polymer carbon source and a small molecule carbon source; wherein the polymer carbon source includes at least one of polyethylene glycol, polyvinyl pyrrolidone, graphene, and carbon nanotubes; and the small molecule carbon source includes at least one of glucose, sucrose, and conductive carbon black.
[0032] Preferably, the mass proportion of the polymer carbon source in the carbon source is less than 50%.
[0033] The composite carbon source is formed by combining the polymer carbon source with the small molecule carbon source. Since the CC bonds in the small molecule carbon source are disordered and the CC bonds in the polymer carbon source are ordered, the small molecule carbon source is more likely to form sp under the high temperature in the sintering process of preparing the positive electrode material. 3 Hybrid carbon and high molecular carbon sources are more likely to form sp 2 Hybrid carbon; by adjusting the ratio of high molecular weight carbon source to low molecular weight carbon source, the sp 2 The content of hybridized carbon, thus D / I G The ratio is regulated within an appropriate range.
[0034] Preferably, the S1 further comprises a phosphorus source, wherein the phosphorus source comprises Li2 HPO 4 , LiH 2 PO 4 , Li 3 PO 4 NH 4 ) 2 HPO 4 NH 4 H 2 PO 4 , H 3 PO 4 At least one of .
[0035] Preferably, in S1, the solid content of the premixed slurry is 20wt%-60wt%;
[0036] In S2, the grinding slurry is ground by sand milling, the particle size of the sand milling beads is 0.2-0.5 mm, and the sand milling time is 8-20 hours; the spray drying temperature is ≤300°C; the sintering temperature is 650-850°C, the sintering time is 5-20 hours, and the heating rate during the sintering process is 2-15°C / min.
[0037] Preferably, the solid content of the premixed slurry is 35wt%-50wt%.
[0038] Preferably, during the sintering process, an organic molecular liquid is added to the sintering environment; the organic molecular liquid includes at least one of ethanol, methanol and acetone; and the rate at which the organic molecules are pumped into the sintering environment is 1-100 mL / min.
[0039] By further controlling the heating rate during the sintering process and introducing organic molecular liquid that can instantly vaporize at high temperatures during the sintering process, the graphitization degree of the carbon coating layer can be further controlled, thereby increasing the sp 2 Hybridized carbon content.
[0040] In a third aspect, the present application provides a lithium-ion battery, which adopts the following technical solution:
[0041] A lithium-ion battery comprises a positive electrode sheet, wherein the positive electrode sheet comprises an active material layer, and the active material layer comprises the phosphate-based positive electrode material as described above.
[0042] The lithium-ion battery prepared in the present application has excellent rate performance, low temperature performance and cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 Schematic diagram of the crystal structure of phosphate-based positive electrode materials.
[0044] Figure 2This is the XRD spectrum of the phosphate-based positive electrode material prepared in Example 1 of the present application.
[0045] Figure 3 (a) is a SEM image of the phosphate-based positive electrode material prepared in Example 1 of the present application, and (b) is a SEM image of the phosphate-based positive electrode material prepared in Example 4.
[0046] Figure 4 The charge and discharge curve test diagram (a) of the LFP lithium battery in Example 1 and the charge and discharge curve test diagram (b) of the LMFP lithium battery in Example 4. DETAILED DESCRIPTION
[0047] For better understanding and implementation, the technical solution of the present invention will be clearly and completely described below in conjunction with embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments.
[0048] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0049] Unless otherwise indicated, all numerical values expressing quantities of ingredients, reaction conditions, and so forth used in the specification and claims are to be understood as modified by the term “about.” Accordingly, unless indicated to the contrary, the numerical parameters set forth herein are approximations that can vary depending upon the desired properties desired to be obtained.
[0050] As used herein, "and / or" refers to one or all of the elements mentioned. -1
[0051] As used herein, “including” and “comprising” encompasses the case where only the stated elements are present as well as the case where there are other elements other than the stated elements.
[0052] All percentages in the present invention are by weight, unless otherwise specified.
[0053] Unless otherwise indicated, "a", "an", "an" and "the" used in this specification are intended to include "at least one" or "one or more". For example, "a component" means one or more components, so more than one component may be considered and may be employed or used in the implementation of the embodiment.
[0054] Example 1
[0055] 1. Preparation of phosphate-based cathode materials
[0056] S1, Fe 0.97 PO 4 , Li 2 CO 3 , mixed with glucose and polyethylene glycol in a mass ratio of 7:2, and added with TiO 2 and MgCO 3 , after adding deionized water, a premixed slurry with a solid content of 40 wt% is obtained;
[0057] S2, sand grinding the premixed slurry, using sand grinding beads (zirconia) with a particle size of 0.2-0.5 mm for 12 hours to obtain a ground slurry; spray drying the above-mentioned ground slurry at 200°C to obtain a solid product, sintering the above-mentioned solid product at 750°C for 10 hours, controlling the heating rate to be 5°C / min during the sintering process, and pumping ethanol into the sintering environment at a pumping rate of 10mL / min during the sintering process, and air-flow pulverizing the obtained product to obtain a phosphate-based positive electrode material; the chemical formula of the phosphate-based positive electrode material finally prepared is Li 1.03 Fe 0.97 PO 4 / C.
[0058] The SEM image of the phosphate-based cathode material prepared in this example is as follows Figure 3 (a) shown.
[0059] 2. Preparation of positive electrode
[0060] The positive electrode slurry is prepared as follows: the above-mentioned phosphate-based positive electrode material, the conductive agent acetylene black, and the binder PVDF are added to a vacuum mixer at a mass ratio of 97.9:0.9:1.2 for mixing, and then the solvent NMP is added to the mixed slurry, and the mixed slurry is stirred to a uniform state under the action of the vacuum mixer, thereby obtaining the positive electrode slurry of this embodiment. The above-mentioned positive electrode slurry is evenly coated on both surfaces of the positive electrode current collector aluminum foil, and after drying at room temperature, it is transferred to an oven for further drying, and after drying in the oven, a semi-finished positive electrode sheet is obtained, and then the semi-finished positive electrode sheet is cold pressed and cut to obtain the positive electrode sheet to be assembled.
[0061] 3.Button battery assembly
[0062] A commercially available polyethylene film is used as the separator of the lithium battery, a commercially available electrolyte suitable for a 4.2V (charging upper limit) voltage system battery is used as the electrolyte, and a commercially available lithium sheet is used as the negative electrode. The positive electrode sheet, the negative electrode and the separator are assembled, injected, and packaged to obtain a button battery.
[0063] The charge and discharge curve test diagram of the button battery prepared in this embodiment is as follows: Figure 4 (a) shown.
[0064] Example 2
[0065] 1. Preparation of phosphate-based cathode materials
[0066] S1, Mn 0.6 Fe 0.37 PO 4 , Li 2 CO 3 , mixed with glucose and polyethylene glycol in a mass ratio of 7:2, and added with V 2 O 5 , after adding deionized water, a premixed slurry with a solid content of 40 wt% is obtained;
[0067] S2, sand grinding the premixed slurry, using sand grinding beads (zirconia) with a particle size of 0.2-0.5 mm for 20 hours to obtain a ground slurry; spray drying the above-mentioned ground slurry at 300°C to obtain a solid product, sintering the above-mentioned solid product at 650°C for 20 hours, controlling the heating rate to be 2°C / min during the sintering process, and pumping methanol into the sintering environment at a pumping rate of 100mL / min during the sintering process, and mechanically crushing the obtained product to obtain a phosphate-based positive electrode material; the chemical formula of the phosphate-based positive electrode material finally prepared is Li 1.03 Mn 0.60 Fe 0.37 PO 4 / C.
[0068] The remaining steps and parameter settings are consistent with those in Example 1.
[0069] Example 3
[0070] 1. Preparation of phosphate-based cathode materials
[0071] S1, FePO 4 、MnCO 3 (Fe / Mn molar ratio 3.7:6), H 4 H 2 PO 4 Mix with glucose and polyethylene glycol in a mass ratio of 7:2, and add MgCO 3 , after adding deionized water, a premixed slurry with a solid content of 40 wt% is obtained;
[0072] S2, sand grinding the premixed slurry, using sand grinding beads (zirconia) with a particle size of 0.2-0.5 mm for 8 hours to obtain a ground slurry; spray drying the above-mentioned ground slurry at 150°C to obtain a solid product, sintering the above-mentioned solid product at 850°C for 5 hours, controlling the heating rate to be 15°C / min during the sintering process, and pumping acetone into the sintering environment at a pumping rate of 80mL / min during the sintering process, and air-flow pulverizing the obtained product to obtain a phosphate-based positive electrode material; the chemical formula of the phosphate-based positive electrode material finally prepared is Li 1.03 Mn 0.60 Fe 0.37 PO 4 / C.
[0073] The remaining steps and parameter settings are consistent with those in Example 1.
[0074] Example 4
[0075] 1. Preparation of phosphate-based cathode materials
[0076] S1, FePO 4 , Mn 3 CO 4 (Fe / Mn molar ratio 3.7:6), H 4 H 2 PO 4 Mixed with glucose and polyethylene glycol in a mass ratio of 7:2, and added with Cr 2 O 3 and ZrO 2 , after adding deionized water, a premixed slurry with a solid content of 40 wt% is obtained;
[0077] S2, sand grinding the premixed slurry, using sand grinding beads (zirconia) with a particle size of 0.2-0.5 mm for 12 hours to obtain a ground slurry; spray drying the above-mentioned ground slurry at 200°C to obtain a solid product, sintering the above-mentioned solid product at 750°C for 12 hours, controlling the heating rate to be 10°C / min during the sintering process, and pumping ethanol into the sintering environment at a pumping rate of 50mL / min during the sintering process, and air-flow pulverizing the obtained product to obtain a phosphate-based positive electrode material; the chemical formula of the phosphate-based positive electrode material finally prepared is Li 1.03 Mn 0.60 Fe 0.37 PO 4 / C.
[0078] The remaining steps and parameter settings are consistent with those in Example 1. The XRD pattern of the phosphate-based positive electrode material prepared in this example is shown in FIG. Figure 2 The SEM image of the phosphate-based positive electrode material prepared in this embodiment is shown in Figure 3 (b) As shown in the charge and discharge curve test diagram of the button battery prepared in this embodiment Figure 4 (b) as shown.
[0079] Example 5
[0080] The difference between this embodiment and embodiment 4 is that the phosphate-based positive electrode material is prepared;
[0081] 1. Preparation of phosphate-based cathode materials
[0082] S1, Fe 2 O 3 、MnCO 3 (Fe / Mn molar ratio 3.7:6), H 4 H 2 PO 4 Mixing with glucose and polyethylene glycol in a mass ratio of 7:2, adding CoO and MgO, and adding deionized water to obtain a premixed slurry with a solid content of 40 wt%;
[0083] S2, sand grinding the premixed slurry, using sand grinding beads (zirconia) with a particle size of 0.2-0.5 mm for 12 hours to obtain a ground slurry; spray drying the ground slurry at 200°C to obtain a solid product, sintering the solid product at 700°C for 12 hours, controlling the heating rate to 10°C / min during the sintering process, and pumping ethanol into the sintering environment at a pumping rate of 30 mL / min during the sintering process, and air-grinding the obtained product to obtain a phosphate-based positive electrode material; the chemical formula of the phosphate-based positive electrode material finally prepared is Li 1.03 Mn 0.60 Fe 0.37 PO 4 / C.
[0084] The remaining steps and parameter settings are consistent with those in Example 4.
[0085] Example 6
[0086] The difference between this embodiment and embodiment 4 is that the phosphate-based positive electrode material is prepared;
[0087] 1. Preparation of phosphate-based cathode materials
[0088] S1, Fe 2 O 3 , Mn 3 O 4 (Fe / Mn molar ratio 3.7:6), H 4 H 2 PO 4Mixed with glucose and polyethylene glycol in a mass ratio of 7:2, and added with NiO and ZrO 2 , after adding deionized water, a premixed slurry with a solid content of 40 wt% is obtained;
[0089] S2, sand grinding the premixed slurry, using sand grinding beads (zirconia) with a particle size of 0.2-0.5 mm for 12 hours to obtain a ground slurry; spray drying the above-mentioned ground slurry at 200°C to obtain a solid product, sintering the above-mentioned solid product at 700°C for 12 hours, controlling the heating rate to be 5°C / min during the sintering process, and pumping ethanol into the sintering environment at a pumping rate of 60mL / min during the sintering process, and mechanically crushing the obtained product to obtain a phosphate-based positive electrode material; the chemical formula of the phosphate-based positive electrode material finally prepared is Li 1.03 Mn 0.60 Fe 0.37 PO 4 / C.
[0090] The remaining steps and parameter settings are consistent with those in Example 4.
[0091] Example 7
[0092] The difference between this embodiment and embodiment 4 is that the phosphate-based positive electrode material is prepared;
[0093] 1. Preparation of phosphate-based cathode materials
[0094] S1, FeC 2 O 4 、MnCO 3 (Fe / Mn molar ratio 3.7:6), H 4 H 2 PO 4 Mixed with glucose and polyethylene glycol in a mass ratio of 7:2, and added with TiO 2 and MgO, and adding deionized water to obtain a premixed slurry with a solid content of 40 wt%;
[0095] S2, sand grinding the premixed slurry, using sand grinding beads (zirconia) with a particle size of 0.2-0.5 mm for 12 hours to obtain a ground slurry; spray drying the above-mentioned ground slurry at 200°C to obtain a solid product, sintering the above-mentioned solid product at 750°C for 12 hours, controlling the heating rate to be 10°C / min during the sintering process, and pumping ethanol into the sintering environment at a pumping rate of 80mL / min during the sintering process, and air-flow pulverizing the obtained product to obtain a phosphate-based positive electrode material; the chemical formula of the phosphate-based positive electrode material finally prepared is Li 1.03 Mn 0.60 Fe 0.37 PO4 / C.
[0096] The remaining steps and parameter settings are consistent with those in Example 4.
[0097] Example 8
[0098] The difference between this embodiment and embodiment 4 is that the phosphate-based positive electrode material is prepared;
[0099] 1. Preparation of phosphate-based cathode materials
[0100] S1, FeC 2 O 4 , Mn 3 O 4 (Fe / Mn molar ratio 3.7:6), H 4 H 2 PO 4 Mixed with glucose and polyethylene glycol in a mass ratio of 7:2, and added with TiO 2 and ZrO 2 , after adding deionized water, a premixed slurry with a solid content of 40 wt% is obtained;
[0101] S2, sand grinding the premixed slurry, using sand grinding beads (zirconia) with a particle size of 0.2-0.5 mm for 12 hours to obtain a ground slurry; spray drying the above-mentioned ground slurry at 200°C to obtain a solid product, sintering the above-mentioned solid product at 700°C for 12 hours, controlling the heating rate to be 5°C / min during the sintering process, and pumping ethanol into the sintering environment at a pumping rate of 30mL / min during the sintering process, and mechanically crushing the obtained product to obtain a phosphate-based positive electrode material; the chemical formula of the phosphate-based positive electrode material finally prepared is Li 1.03 Mn 0.60 Fe 0.37 PO 4 / C.
[0102] The remaining steps and parameter settings are consistent with those in Example 4.
[0103] Example 9
[0104] The difference between this embodiment and embodiment 4 is that the carbon content in the phosphate-based positive electrode material is 0.2 wt %, and the remaining steps and parameter settings are consistent with those in embodiment 4.
[0105] Example 10
[0106] The difference between this embodiment and embodiment 4 is that the doping amount of the first metal element in the phosphate-based positive electrode material is 10000 ppm, and the remaining steps and parameter settings are consistent with those of embodiment 4.
[0107] Embodiment 11
[0108] The difference between this embodiment and embodiment 4 is that the doping amount of the first metal element in the phosphate-based positive electrode material is 7000 ppm, and the remaining steps and parameter settings are consistent with those of embodiment 4.
[0109] Comparative Example 1
[0110] The difference between this comparative example and Example 4 is that in this comparative example, the phosphate-based positive electrode material is not doped at the M position and the Li position, and the remaining steps and parameter settings are consistent with those of Example 4.
[0111] Comparative Example 2
[0112] The difference between this comparative example and Example 4 is that the disorder degree of the carbon material used in this comparative example is 1.5;
[0113] 1. Preparation of phosphate-based cathode materials
[0114] S1, FeC 2 O 4 , Mn 3 O 4 (Fe / Mn molar ratio 3.7:6), H 4 H 2 PO 4 Mix with glucose and add TiO 2 and ZrO 2 , after adding deionized water, a premixed slurry with a solid content of 40 wt% is obtained;
[0115] S2, sand grinding the premixed slurry, using sand grinding beads (zirconia) with a particle size of 0.2-0.5 mm for 12 hours to obtain a ground slurry; spray drying the ground slurry at 200°C to obtain a solid product, sintering the solid product at 700°C for 12 hours, controlling the heating rate to 20°C / min during the sintering process, and mechanically crushing the obtained product to obtain a phosphate-based positive electrode material; the chemical formula of the phosphate-based positive electrode material finally prepared is Li 1.03 Mn 0.60 Fe 0.37 PO 4 / C.
[0116] The remaining steps and parameter settings are consistent with those in Example 4.
[0117] Test Method
[0118] I. D / I G test
[0119] The phosphate-based materials prepared in the above examples and comparative examples were subjected to Raman spectroscopy testing. The specific testing steps were as follows: by measuring the G band (about 1580cm -1 ) of the peak intensity (I G ) and D belt (approximately 1350cm -1 ) of the peak intensity (I D ) to calculate the I of carbon materials D / I G The measuring equipment / conditions are as follows:
[0120] (1) Raman spectrometer: inVia, Renishaw (UK);
[0121] (2) Argon ion laser wavelength: 532nm;
[0122] (3) Exposure time: 10 seconds, number of integration times: 10 times.
[0123] 2. Carbon content test
[0124] The carbon content of the phosphate-based materials prepared in the above examples and comparative examples was tested, specifically, by using a high-frequency infrared carbon-sulfur analyzer HW2000.
[0125] 3. Metal element doping content test
[0126] The carbon content of the phosphate-based materials prepared in the above embodiments and comparative examples was tested. The specific testing method was based on GB / T 30902-2014 "Determination of impurity elements in inorganic chemical products - Inductively coupled plasma optical emission spectrometry". During the testing process, ICP-OES equipment was used to test the content of the first metal element doped at the M position and the content of the second metal element doped at the Li position.
[0127] 4. Ion dissolution rate test
[0128] The phosphate-based cathode materials prepared in the above embodiments and comparative examples were tested for Mn / Fe ion dissolution rate. The specific testing method was as follows: ① Weigh 5 g of phosphate-based cathode material powder, pour it into a beaker, and add 50 ml of ultrapure water; ② Seal the mouth of the beaker with plastic wrap and let it stand at room temperature for 70 hours; ③ The supernatant of the material obtained after standing was uniformly introduced into a three-layer medium-speed filter paper, and the filtrate was collected; ④ The collected filtrate was filtered with a three-layer filter membrane (pore size of 0.22 um), and 1 ml of the filtrate was taken to a 50 / 100 ml volumetric flask for constant volume, and then the Mn / Fe content was tested using ICP; ⑤ The Mn / Fe content in the solution was converted to the dissolution rate of 5 g of phosphate-based cathode material powder.
[0129] 5. Powder compaction density test
[0130] The phosphate-based cathode materials prepared in the above-mentioned embodiments and comparative examples were subjected to a compaction density test. The specific testing equipment used was a powder compaction density meter UTM7305 manufactured by Shenzhen Sansi Zongheng, and the testing condition was a pressure of 30 kN.
[0131] 6. Rct test
[0132] The button cells prepared in the above-mentioned embodiments and comparative examples were subjected to EIS test by means of an electrochemical workstation, and the measured EIS data were fitted to obtain Rct; the specific testing equipment was VMP3 French Bio-Logic multi-channel electrochemical workstation.
[0133] Table 1
[0134]
[0135] In combination with Examples 1-4, Comparative Examples 1-2 and Table 1, it can be seen that by doping the first metal element at the M position and / or doping the second metal element at the Li position and controlling the order of the carbon material in the carbon coating layer, the Fe / Mn dissolution rate of the phosphate-based positive electrode material can be significantly reduced, which is beneficial to improving the cycle performance of the positive electrode material; and, at this time, the charge transfer impedance of the phosphate-based positive electrode material is small, so that the positive electrode material has excellent rate performance.
[0136] In combination with Examples 1-8 and Table 1, it can be seen that the phosphate-based positive electrode material with a non-strict stoichiometric ratio is prepared by the method in the present application. The phosphate-based positive electrode material has a low charge transfer impedance and a low Fe / Mn dissolution rate, and has excellent rate performance and low-temperature cycle performance; and also has a wide range of powder compaction density, which can be suitable for the application requirements of different lithium batteries.
[0137] In combination with Examples 4, 9, and Table 1, it can be seen that when the carbon content in the phosphate-based positive electrode material is low, the Fe / Mn dissolution rate and charge transfer impedance of the positive electrode material both increase to a certain extent. This is because the carbon coating layer cannot construct an effective coated conductive network structure on the surface of the phosphate-based positive electrode active material. The carbon material in the carbon coating layer of the phosphate-based positive electrode material in Example 4 of the present application has a low degree of disorder and a high degree of graphitization, and can form an efficient conductive network structure, which significantly reduces the charge transfer impedance of the phosphate-based positive electrode material.
[0138] In combination with Examples 4, 10-11, and Table 1, it can be seen that when the doping content of the first metal element is too high or the doping content of the second metal element is too high, impurity phases will be generated in the phosphate-based positive electrode material, reducing the stability of the crystal structure, and the Fe / Mn dissolution rate and charge transfer impedance of the phosphate-based positive electrode material will increase to a certain extent; while in Example 4, since the doping of the first metal element and the second metal element is controlled within a reasonable range, not only can the generation of impurity phases be reduced, but also the defects in the carbon coating layer can be inhibited from promoting the side reactions of the phosphate-based positive electrode material in the electrolyte, which also helps to reduce the degree of degradation of the carbon coating layer due to side reactions, thereby further stabilizing the structural stability of the phosphate-based positive electrode material, reducing its Fe / Mn dissolution rate, and helping to improve the cycle performance of the lithium battery.
[0139] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the protection scope of the present invention. Although the present invention is described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the technical solutions of the present invention can be modified or equivalently replaced, but these modifications or replacements are all within the protection scope of the present invention.
Claims
1. A phosphate-based positive electrode material, characterized in that: The phosphate-based positive electrode material comprises a base particle and a carbon coating layer coated on the surface of the base particle; the chemical formula of the base particle is Li x M y PO4, 0.96≤x≤1.08, 0.96≤y≤1, M includes at least one of Fe and Mn; Wherein, the M position is doped with a first metal element, the first metal element includes at least one of Ti, V, Cr, Co, Ni, Nb, Mo, and W; and / or, the Li position is doped with a second metal element, the second metal element includes at least one of Mg and Zr; The carbon coating layer includes a carbon material, and the disorder degree of the carbon material is D / I G ≤1.
2.
2. The phosphate-based positive electrode material according to claim 1, characterized in that: The carbon content in the phosphate-based positive electrode material is 1 wt%-2 wt%.
3. The phosphate-based positive electrode material according to claim 1, characterized in that: The doping amount of the first metal element is ≤5000ppm.
4. The phosphate-based positive electrode material according to claim 1, characterized in that: The doping amount of the second metal is ≤3000ppm.
5. The phosphate-based positive electrode material according to claim 1, characterized in that: The particle size D50 of the phosphate-based positive electrode material is 50-2000 nm.
6. The phosphate-based positive electrode material according to any one of claims 1 to 5, characterized in that: The compaction density of the phosphate-based positive electrode material is 2-2.7 g / cm 3 .
7. The method for preparing a phosphate-based positive electrode material according to any one of claims 1 to 6, characterized in that: The steps include: S1, mixing an iron source, a manganese source, a lithium source and a carbon source, adding water and grinding to obtain a premixed slurry; S2, spray-drying, sintering and then crushing the premixed slurry to obtain the phosphate-based positive electrode material.
8. The method for preparing a phosphate-based positive electrode material according to claim 7, characterized in that: The iron source includes at least one of FePO4, Fe2O3, and FeC2O4; The manganese source includes at least one of MnPO4, MnCO3, and Mn3O4; The lithium source includes at least one of Li2CO3, LiOH.H2O, LiCl, Li2SO4, Li2HPO4, LiH2PO4, Li3PO4, and LiNO3; The doping source comprises an M-site doping source and a Li-site doping source, wherein the M-site doping source comprises at least one of Ti salts and oxides thereof, V salts and oxides thereof, Cr salts and oxides thereof, Co salts and oxides thereof, Ni salts and oxides thereof, Nb salts and oxides thereof, Mo salts and oxides thereof, and W salts and oxides thereof, and the Li-site doping source comprises at least one of Mg salts and oxides thereof, and Zr salts and oxides thereof; The carbon source includes a polymer carbon source and a small molecule carbon source; wherein the polymer carbon source includes at least one of polyethylene glycol, polyvinyl pyrrolidone, graphene, and carbon nanotubes; and the small molecule carbon source includes at least one of glucose, sucrose, and conductive carbon black.
9. The method for preparing a phosphate-based positive electrode material according to claim 7, characterized in that: In S1, the solid content of the premixed slurry is 20wt%-60wt%; In S2, the grinding slurry is ground by sand milling for 8-20 hours; the spray drying temperature is ≤300°C; the sintering temperature is 650-850°C, the sintering time is 5-20 hours, and the heating rate during the sintering process is 2-15°C / min.
10. A lithium ion battery, characterized in that: It comprises a positive electrode sheet, wherein the positive electrode sheet comprises an active material layer, and the active material layer comprises the phosphate-based positive electrode material according to any one of claims 1 to 6.
Citation Information
Patent Citations
Lithium iron phosphate composite positive electrode material and preparation method and application thereof
CN110085839A
Titanium and zirconium co-doped carbon-coated lithium iron phosphate material as well as preparation method and application thereof
CN114314548A
Positive electrode material and preparation method thereof, positive electrode plate and secondary battery
CN115714171A
Lithium manganese iron phosphate material and preparation method thereof, positive pole piece and lithium ion battery
CN117525331A
Composite phosphate positive electrode material and preparation method and application thereof
CN117638026A
Cited By
Phosphate positive electrode material and preparation method and application thereof
CN120453328A
Phosphate positive electrode material and preparation method thereof, positive plate and battery
CN121307021A
Phosphate-based positive electrode material, and preparation method therefor and use thereof
WO2026000898A1
Phosphate positive electrode material and preparation method therefor, positive electrode sheet, and secondary battery
WO2026123398A1
Positive electrode material, secondary battery and electronic apparatus
WO2026188405A1