Bipolar current collector, electrochemical device and electronic device

By designing bipolar current collectors and regulating the structural characteristics of the copper and aluminum layers, the problem of balancing energy density and cycle performance of lithium-ion batteries is solved, and an electrochemical device with high energy density and long cycle life is realized.

CN118738403APending Publication Date: 2024-10-01XIAMEN AMPACE TECH LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410881053.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

It is difficult to balance the energy density and cycle performance of lithium-ion batteries in demanding application scenarios, and the structural characteristics of the current collector affect its performance.

Method used

Design a bipolar current collector, including a copper layer, an aluminum layer and a polymer layer. By regulating the thickness, porosity and pore size of each layer, the contact resistance and quality difference between the copper layer and the aluminum layer are optimized to balance the positive and negative electrode materials. The difference in expansion rate improves the energy density and power density of electrochemical devices.

Benefits of technology

It achieves an improvement in the energy density and power density of lithium-ion batteries, while extending its cycle performance to meet the needs of high energy density and long cycle life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118738403A_ABST
    Figure CN118738403A_ABST
Patent Text Reader

Abstract

The invention provides a bipolar current collector, an electrochemical device and an electronic device. The bipolar current collector comprises a copper layer, an aluminum layer and a polymer layer, the polymer layer is located between the copper layer and the aluminum layer, the thickness of the copper layer is T1 [mu] m, the thickness of the aluminum layer is T2 [mu] m, the porosity of the copper layer is A1, the porosity of the aluminum layer is A2, and T2 (1-A2) is larger than T1 (1-A1). According to the application, T1, T2, A1 and A2 of the bipolar current collector are regulated and controlled to meet the relationship, and structure optimization is carried out aiming at different characteristics of the copper layer and the aluminum layer, so that the energy density, the power density and the cycle performance of the electrochemical device are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of electrochemical technology, and in particular to a bipolar current collector, an electrochemical device and an electronic device. Background Art

[0002] Electrochemical devices, such as lithium-ion batteries, are widely used in smartphones, wearable devices, consumer drones, and electric vehicles due to their high energy density, long cycle life, and no memory effect.

[0003] With the widespread application of lithium-ion batteries in the above fields, the market has higher and higher requirements for the energy density of lithium-ion batteries. The current collector is one of the indispensable components of lithium-ion batteries, and its structural characteristics will affect the energy density and cycle performance of lithium-ion batteries. Summary of the invention

[0004] The purpose of this application is to provide a bipolar current collector, an electrochemical device and an electronic device to simultaneously improve the energy density and cycle performance of the electrochemical device. The specific technical solution is as follows: The first aspect of the present application provides a bipolar current collector, including a copper layer, an aluminum layer and a polymer layer, wherein the polymer layer is located between the copper layer and the aluminum layer, the thickness of the copper layer is T1μm, the thickness of the aluminum layer is T2μm, the porosity of the copper layer is A1, the porosity of the aluminum layer is A2, and T2(1-A2)>T1(1-A1). The present application adjusts T1, T2, A1, and A2 of the bipolar current collector to satisfy the above relationship, optimizes the structure according to the different characteristics of the copper layer and the aluminum layer, and is conducive to balancing the contact impedance and mass difference between the copper layer and the aluminum layer. When applied to an electrochemical device, it is conducive to balancing the difference in expansion rate between the positive electrode active material and the negative electrode active material, thereby improving the energy density, power density, and cycle performance of the electrochemical device.

[0005] In some embodiments of the present application, the bipolar current collector satisfies any one of the following characteristics: (1) T1=T2, A1>A2; (2) T1<T2, A1=A2; (3) T1<T2, A1>A2. Applying the bipolar current collector that satisfies the above conditions to an electrochemical device is beneficial to improving the energy density, power density and cycle performance of the electrochemical device.

[0006] In some embodiments of the present application, 5%≤A1≤45%, 0%≤A2≤30%. By regulating the values ​​of A1 and A2 within the above range, it is beneficial to improve the energy density and cycle performance of the electrochemical device.

[0007] In some embodiments of the present application, 0.5≤T1≤10, 0.5≤T2≤10. By regulating the values ​​of T1 and T2 within the above range, it is beneficial to make the copper layer and the aluminum layer have higher mechanical strength, the bipolar current collector is not easy to break, and it is also beneficial to reduce the volume of the bipolar current collector, and make the copper layer and the aluminum layer have smaller contact impedance, which is beneficial to improve the energy density and power density of the electrochemical device when applied.

[0008] In some embodiments of the present application, 1≤T2 / T1≤4. By regulating the value of T2 / T1 within the above range, the thickness of the aluminum layer is greater than or equal to the thickness of the copper layer, which is beneficial to reducing the mass of the copper layer and the contact impedance of the aluminum layer, balancing the mass and contact impedance differences between the copper layer and the aluminum layer, and thus being beneficial to improving the energy density and power density of the electrochemical device when applied thereto.

[0009] In some embodiments of the present application, the average pore size of the copper layer is D1 μm, the average pore size of the aluminum layer is D2 μm, 20≤D1≤400, 20≤D2≤400. By regulating the average pore size D1 of the copper layer and the average pore size D2 of the aluminum layer within the above range, it is beneficial to reduce the mass of the copper layer and the aluminum layer, and at the same time, the bipolar current collector has good ion conductivity and high mechanical strength, so that it is beneficial to improve its energy density and cycle performance when applied to electrochemical devices.

[0010] In some embodiments of the present application, the surface of the copper layer away from the polymer layer is the first surface, and the surface of the aluminum layer away from the polymer layer is the second surface. The bipolar current collector includes a plurality of first holes and a plurality of second holes. The first holes extend from the first surface along the thickness direction of the bipolar current collector, and the second holes extend from the second surface along the thickness direction of the bipolar current collector. The depth of the first holes is H1 μm, the depth of the second holes is H2 μm, and the thickness of the polymer layer is T3 μm. The bipolar current collector satisfies any one of the following characteristics: (1) H1≤T1, H2≤T2; (2) T1

[0011] In some embodiments of the present application, the thickness of the polymer layer is T3 μm, 1≤T3≤20. By adjusting the value of T3 within the above range, it is helpful to reduce the volume and mass of the bipolar current collector, and at the same time, the bipolar current collector has a higher mechanical strength and is not prone to breakage, so that it is applied to electrochemical devices to improve their energy density. ​

[0012] In some embodiments of the present application, the material of the polymer layer includes at least one of polyethylene, polypropylene, polystyrene, polyvinyl chloride or polyethylene terephthalate. The polymer layer is made of the above materials, which is beneficial to improving the energy density and cycle performance of the electrochemical device.

[0013] The second aspect of the present application provides an electrochemical device, which includes a bipolar pole piece, and the bipolar pole piece includes the bipolar current collector provided in the first aspect of the present application. The electrochemical device provided by the present application has high energy density and power density and good cycle performance.

[0014] The third aspect of the present application provides an electronic device, which includes the electrochemical device provided in the second aspect of the present application. The electrochemical device provided in the present application has high energy density and power density and good cycle performance, so that the electronic device provided in the present application has a long service life and good performance.

[0015] Beneficial effects of the embodiments of the present application: The embodiments of the present application provide a bipolar current collector, an electrochemical device, and an electronic device. The bipolar current collector includes a copper layer, an aluminum layer, and a polymer layer, wherein the polymer layer is located between the copper layer and the aluminum layer, the thickness of the copper layer is T1μm, the thickness of the aluminum layer is T2μm, the porosity of the copper layer is A1, the porosity of the aluminum layer is A2, and T2(1-A2)>T1(1-A1). The present application adjusts T1, T2, A1, and A2 of the bipolar current collector to satisfy the above relationship, and optimizes the structure according to the different characteristics of the copper layer and the aluminum layer, which is beneficial to balancing the contact impedance and mass difference between the copper layer and the aluminum layer. The application in the electrochemical device is beneficial to balancing the difference in expansion rate between the positive electrode active material and the negative electrode active material, thereby improving the energy density, power density, and cycle performance of the electrochemical device.

[0016] Of course, implementing any product or method of the present application does not necessarily require achieving all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other embodiments can also be obtained based on these drawings.

[0018] Figure 1 A schematic diagram of the cross-sectional structure of a bipolar current collector along its thickness direction according to an embodiment of the present application; Figure 2 A schematic diagram of the cross-sectional structure of a bipolar current collector along its thickness direction according to another embodiment of the present application; Figure 3 This is a schematic diagram of the cross-sectional structure of a bipolar current collector along its thickness direction according to another embodiment of the present application; Figure 4 This is a schematic diagram of the cross-sectional structure of a bipolar current collector according to another embodiment of the present application along its thickness direction; Figure 5 This is a schematic diagram of the cross-sectional structure of the bipolar current collector along its thickness direction according to the fifth embodiment of the present application; Figure 6 This is a schematic diagram of the cross-sectional structure of the bipolar current collector along its thickness direction according to the sixth implementation scheme of the present application.

[0019] Reference numerals: bipolar current collector 10, copper layer 11, aluminum layer 12, polymer layer 13, first surface 11a, second surface 12a, first hole 11b, second hole 12b. DETAILED DESCRIPTION

[0020] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. All other embodiments obtained by those skilled in the art based on the present application belong to the scope of protection of the present application.

[0021] It should be noted that in the following content, lithium-ion batteries are used as an example of electrochemical devices to explain the present application, but the electrochemical devices of the present application are not limited to lithium-ion batteries. The specific technical solution is as follows: The first aspect of the present application provides a bipolar current collector, including a copper layer, an aluminum layer and a polymer layer, wherein the polymer layer is located between the copper layer and the aluminum layer, the thickness of the copper layer is T1 μm, the thickness of the aluminum layer is T2 μm, the porosity of the copper layer is A1, the porosity of the aluminum layer is A2, and T2 (1-A2) > T1 (1-A1).

[0022] For ease of understanding, in this application, the length direction of the bipolar current collector itself is defined as Y, and the thickness direction is defined as Z. After the bipolar current collector is unfolded, it usually has a long side and a short side. The length direction is the extension direction of the long side after the bipolar current collector is unfolded. It should be understood that the above definition of direction is for the purpose of convenient description of this application. Figure 1 As shown, the bipolar current collector 10 includes a copper layer 11, an aluminum layer 12, and a polymer layer 13 located between the copper layer 11 and the aluminum layer 12. T1 is the thickness of the copper layer 11, T2 is the thickness of the aluminum layer 12, and T3 is the thickness of the polymer layer 13.

[0023] Compared with using positive current collectors and negative current collectors separately in electrochemical devices, the use of the bipolar current collector of the present application is conducive to reducing the mass of the current collector in the electrochemical device, reducing the loss of energy density of the electrochemical device due to the increase in mass, thereby improving the energy density of the electrochemical device. At the same time, the use of the bipolar pole piece prepared by the bipolar current collector of the present application in the electrochemical device is conducive to saving the amount of isolation membrane, reducing the volume of the electrochemical device, and reducing the loss of energy density of the electrochemical device due to the increase in volume, thereby improving the energy density of the electrochemical device. The bipolar current collector of the present application is provided with pores, which is conducive to reducing the mass of the bipolar current collector, thereby further improving the energy density of the electrochemical device. At the same time, the pores are also conducive to embedding the positive active material and the negative active material, absorbing the expansion of the positive active material and the negative active material, thereby improving the cycle performance of the electrochemical device.

[0024] The bipolar current collector of the present application includes a copper layer and an aluminum layer. From the perspective of contact impedance, the resistivity of the copper layer is 1.68×10 -8 Ω / m, the resistivity of the aluminum layer is 2.65×10 -8 Ω / m, the resistivity of the copper layer is 0.6 times that of the aluminum layer. The thickness relationship and porosity relationship between the copper layer and the aluminum layer will affect the contact impedance of the bipolar current collector. The smaller the thickness, the greater the contact impedance; the greater the porosity, the greater the contact impedance. T1<T2 and / or A1>A2 are conducive to balancing the difference in contact impedance between the copper layer and the aluminum layer, reducing the internal resistance of the electrochemical device, and thus increasing the power density of the electrochemical device. If the thickness of the aluminum layer is smaller and / or the porosity is larger, that is, T1>T2 and / or A1<A2, or the copper layer and the aluminum layer have the same thickness and porosity, that is, T1=T2 and A1=A2, the contact impedance of the aluminum layer will be higher, thereby affecting the power density of the electrochemical device. From a mass perspective, the density of the copper layer is 8.96g / cm 3 The density of the aluminum layer is 2.7g / cm 3, the thickness relationship and porosity relationship between the copper layer and the aluminum layer will affect the mass of the bipolar current collector. The greater the thickness, the greater the mass; the smaller the porosity, the greater the mass. T1<T2 and / or A1>A2 are conducive to balancing the mass difference between the copper layer and the aluminum layer, thereby improving the energy density of the electrochemical device. If the thickness of the aluminum layer is smaller and / or the porosity is larger, that is, T1>T2 and / or A1<A2, or the copper layer and the aluminum layer have the same thickness and porosity, that is, T1=T2 and A1=A2, the mass of the copper layer will be larger, thereby affecting the energy density of the electrochemical device. From the perspective of expansion rate, the negative electrode material layer is usually arranged on the surface of the copper layer, and the positive electrode material layer is usually arranged on the surface of the aluminum layer. The expansion rate of the negative electrode active material in the negative electrode material layer is often greater than the expansion rate of the positive electrode active material in the positive electrode material layer. When A1>A2, it is beneficial to embed more negative electrode active materials into the pores of the copper layer, provide a larger expansion space for the negative electrode active materials, improve the problem of large expansion rate of negative electrode active materials, balance the stress distribution of the bipolar pole piece to reduce the deformation of the bipolar pole piece, and thus improve the cycle performance of the electrochemical device. If the porosity of the aluminum layer is larger, that is, A1<A2, or the copper layer and the aluminum layer use the same porosity, that is, A1=A2, the larger expansion of the negative electrode active material will make the stress of the copper layer larger, and the uneven stress distribution of the bipolar pole piece will cause the deformation of the bipolar pole piece to be serious, thereby affecting the cycle performance of the electrochemical device. Therefore, the present application adjusts the T1, T2, A1, and A2 of the bipolar current collector to meet the above relationship, optimizes the structure according to the different characteristics of the copper layer and the aluminum layer, and is beneficial to balancing the contact impedance and mass difference between the copper layer and the aluminum layer. It is applied to electrochemical devices to balance the expansion rate difference between the positive electrode active material and the negative electrode active material, thereby improving the energy density, power density, and cycle performance of the electrochemical device.

[0025] In the present application, appropriate T1, T2, A1 and A2 can be set according to the product characteristics of the electrochemical device. For example, for an electrochemical device requiring high energy density, the bipolar current collector can select smaller T1 and T2 and larger A1 and A2 to reduce its mass; for an electrochemical device requiring high power density, the bipolar current collector can select larger T1 and T2 and smaller A1 and A2 to reduce its contact impedance; for an electrochemical device requiring good cycle performance, the bipolar current collector can select a larger A1 to improve the problem of large expansion rate of negative electrode active materials.

[0026] In some embodiments of the present application, the bipolar current collector satisfies: T1=T2, A1>A2. When the thickness of the copper layer and the aluminum layer is the same, the porosity A1 of the copper layer is greater than the porosity A2 of the aluminum layer. Since the resistivity of the aluminum layer is higher, the smaller porosity of the aluminum layer is conducive to reducing the contact impedance of the aluminum layer, making the difference in contact impedance between the aluminum layer and the copper layer smaller, and reducing the internal resistance of the electrochemical device, so that it is applied to the electrochemical device to improve its power density. At the same time, since the density of the copper layer is higher, the larger porosity of the copper layer is conducive to reducing the mass of the copper layer, so that the mass difference between the aluminum layer and the copper layer is reduced, so that it is applied to the electrochemical device to improve its energy density. The expansion rate of the negative electrode active material is often greater than the expansion rate of the positive electrode active material. The larger porosity of the copper layer is also conducive to embedding more negative electrode active materials into the pores of the copper layer, improving the problem of the large expansion rate of the negative electrode active material, so that it is applied to the electrochemical device to improve its cycle performance. Therefore, the bipolar current collector that meets the above conditions is applied to the electrochemical device, which is conducive to improving the energy density, power density and cycle performance of the electrochemical device.

[0027] In some embodiments of the present application, the bipolar current collector satisfies: T1<T2, A1=A2. When the porosity of the copper layer and the aluminum layer is the same, the thickness of the copper layer is less than the thickness of the aluminum layer. Since the resistivity of the aluminum layer is higher, the greater thickness of the aluminum layer is conducive to reducing the contact impedance of the aluminum layer, making the difference in contact impedance between the aluminum layer and the copper layer smaller, and reducing the internal resistance of the electrochemical device, so that it is applied to the electrochemical device to improve its power density. At the same time, since the density of the copper layer is higher, the smaller thickness of the copper layer is conducive to reducing the mass of the copper layer, reducing the difference in mass between the aluminum layer and the copper layer, so that it is applied to the electrochemical device to improve its energy density. Therefore, applying the bipolar current collector that meets the above conditions to the electrochemical device is conducive to improving the energy density and power density of the electrochemical device.

[0028] In some embodiments of the present application, the bipolar current collector satisfies: T1<T2, A1>A2. The thickness of the copper layer is less than the thickness of the aluminum layer, and the porosity of the copper layer is greater than the porosity of the aluminum layer. Since the resistivity of the aluminum layer is higher, the greater thickness and smaller porosity of the aluminum layer are conducive to further reducing the contact impedance of the aluminum layer, making the impedance difference between the aluminum layer and the copper layer smaller, and reducing the internal resistance of the electrochemical device, so that the application of the electrochemical device is conducive to further improving its power density. At the same time, since the density of the copper layer is greater, the smaller thickness and greater porosity of the copper layer are conducive to further reducing the mass of the copper layer, so that the mass difference between the aluminum layer and the copper layer is reduced, so that the application of the electrochemical device is conducive to further improving its energy density. The expansion rate of the negative electrode active material is often greater than the expansion rate of the positive electrode active material. The greater porosity of the copper layer is also conducive to embedding more negative electrode active materials into the pores of the copper layer, improving the problem of the large expansion rate of the negative electrode active material, so that the application of the electrochemical device is conducive to improving its cycle performance. Therefore, the bipolar current collector that meets the above conditions is applied to the electrochemical device, which is conducive to further improving the energy density, power density and cycle performance of the electrochemical device.

[0029] In some embodiments of the present application, 5%≤A1≤45%, 0%≤A2≤30%. For example, A1 can be 5%, 10%, 14%, 20%, 26%, 30%, 35%, 40%, 45% or a range consisting of any two of the above values, and A2 can be 0%, 5%, 10%, 16%, 20%, 24%, 30% or a range consisting of any two of the above values. By regulating the values ​​of A1 and A2 within the above range, the bipolar current collector has a high mechanical strength, is not prone to breakage, and is also conducive to reducing the mass of the copper layer and the aluminum layer, so that it is applied to an electrochemical device to improve its energy density. In addition, the pores of the copper layer are conducive to embedding the negative electrode active material and absorbing the expansion of the negative electrode active material, and the pores of the aluminum layer are conducive to embedding the positive electrode active material and absorbing the expansion of the positive electrode active material, so that it is applied to an electrochemical device to improve its cycle performance. Therefore, the bipolar current collector that meets the above conditions is applied to an electrochemical device, which is conducive to improving the energy density and cycle performance of the electrochemical device.

[0030] In some embodiments, such as Figure 2 As shown, the aluminum layer 12 does not include pores, and A2=0%. Since the aluminum layer has a low density and does not include pores, it is beneficial to improve the mechanical strength of the bipolar current collector on the basis of having little effect on the energy density of the electrochemical device, and to make the aluminum layer have a smaller contact impedance, thereby reducing the internal resistance of the electrochemical device, so that it is beneficial to improve the power density and cycle performance of the electrochemical device when applied to the electrochemical device.

[0031] In some embodiments of the present application, 0.5≤T1≤10, 0.5≤T2≤10. For example, T1 can be 0.5, 2, 3.2, 4, 5, 6, 7.1, 8, 9.3, 10 or a range consisting of any two of the above values, and T2 can be 0.5, 2, 3.4, 4, 5, 6, 7.2, 8, 9.1, 10 or a range consisting of any two of the above values. By regulating the values ​​of T1 and T2 within the above range, the copper layer and the aluminum layer have higher mechanical strength, and the bipolar current collector is not prone to breakage. At the same time, it is beneficial to reduce the volume of the bipolar current collector, and make the copper layer and the aluminum layer have a smaller contact impedance, and the electrochemical device has a smaller internal resistance, so that it is applied to the electrochemical device to improve its energy density and power density.

[0032] In some embodiments of the present application, 1≤T2 / T1≤4. For example, T2 / T1 can be 1, 1.2, 1.8, 2.0, 2.3, 2.6, 2.8, 3.0, 3.3, 3.5, 4 or a range consisting of any two of the above values. By regulating the value of T2 / T1 within the above range, the thickness of the aluminum layer is greater than or equal to the thickness of the copper layer. Since the resistivity of the aluminum layer is higher, the greater thickness of the aluminum layer is conducive to reducing the contact impedance of the aluminum layer, making the difference in contact impedance between the aluminum layer and the copper layer smaller, and reducing the internal resistance of the electrochemical device, so that it is applied to the electrochemical device to improve its power density. At the same time, since the density of the copper layer is greater, the smaller thickness of the copper layer is conducive to reducing the mass of the copper layer, so that the mass difference between the aluminum layer and the copper layer is reduced, so that it is applied to the electrochemical device to improve its energy density. Therefore, the bipolar current collector that meets the above conditions is applied to the electrochemical device, which is conducive to improving the energy density and power density of the electrochemical device.

[0033] In some embodiments of the present application, the average pore size of the copper layer is D1 μm, the average pore size of the aluminum layer is D2 μm, 20≤D1≤400, 20≤D2≤400. For example, D1 can be 20, 60, 100, 170, 200, 240, 300, 350, 400 or a range consisting of any two of the above values, and D2 can be 20, 50, 100, 160, 200, 250, 300, 340, 400 or a range consisting of any two of the above values. By regulating the average pore size D1 of the copper layer and the average pore size D2 of the aluminum layer within the above range, it is beneficial to reduce the mass of the copper layer and the aluminum layer, and it is also beneficial to the transmission of lithium ions, so that the bipolar current collector has good ion conductivity and high mechanical strength, so that it is applied to electrochemical devices to improve their energy density and cycle performance.

[0034] The present application has no particular restrictions on the shape of the holes in the copper layer and the aluminum layer, as long as the purpose of the present application can be achieved. For example, the shape of the holes in the copper layer and the aluminum layer may include but is not limited to at least one of a circle, a square, a triangle or a slot. In the present application, the average pore size refers to the diameter of the circumscribed circle of the hole shape, and the diameter of the circumscribed circle of the hole can be measured by using the Keyence IM8000 to draw the outline of the hole.

[0035] exist Figures 1 to 6 In the embodiment, the surface of the copper layer 11 away from the polymer layer 13 is the first surface 11a, the surface of the aluminum layer 12 away from the polymer layer 13 is the second surface 12a, the bipolar current collector 10 includes a plurality of first holes 11b and a plurality of second holes 12b, the first holes 11b extend from the first surface 11a along the thickness direction of the bipolar current collector 10, the second holes 12b extend from the second surface 12a along the thickness direction of the bipolar current collector 10, the depth of the first holes 11b is H1 μm, the depth of the second holes 12b is H2 μm, and the thickness of the polymer layer 13 is T3 μm.

[0036] In some embodiments of the present application, the bipolar current collector satisfies: H1≤T1, H2≤T2. Specifically, in some embodiments, such as Figure 1 As shown, H1<T1, H2<T2; In other embodiments, as Figure 3 As shown, H1=T1, H2=T2. When the bipolar current collector meets the above conditions, there is no special restriction on the positional relationship between the first hole and the second hole, as long as the purpose of this application can be achieved. By regulating H1, H2, T1, and T2 to meet the above relationship, the bipolar current collector has a higher mechanical strength, and is also beneficial to reduce the mass of the copper layer and the aluminum layer, as well as embedding the positive electrode active material and the negative electrode active material, absorbing the expansion of the positive electrode active material and the negative electrode active material, thereby helping to improve the energy density and cycle performance of the electrochemical device.

[0037] In some embodiments of the present application, the bipolar current collector satisfies: T1 Figure 4 As shown, along the thickness direction of the bipolar current collector 10, the projection of the first hole 11b and the projection of the second hole 12b can be separated;​ Figure 5 As shown, along the thickness direction of the bipolar current collector 10, the projection of the first hole 11b and the projection of the second hole 12b can intersect. By adjusting H1, H2, T1, T2, and T3 to meet the above relationship, the sum of the depths of the first hole and the second hole is less than the thickness of the bipolar current collector, and no through holes will appear inside the bipolar current collector, which is beneficial to reduce the internal short circuit between the positive and negative electrodes during the use of the electrochemical device, and is also beneficial to reduce the mass of the bipolar current collector on the basis of having a high mechanical strength, so that it is beneficial to improve its energy density when applied to the electrochemical device. At the same time, it is also beneficial to embed the positive active material and the negative active material, absorb the expansion of the positive active material and the negative active material, and thus be beneficial to improve its cycle performance when applied to the electrochemical device. Therefore, the bipolar current collector that meets the above conditions is applied to the electrochemical device, which is beneficial to improve the energy density and cycle performance of the electrochemical device.

[0038] In some embodiments of the present application, Figure 6 As shown, the bipolar current collector satisfies: T1

[0039] In some embodiments, 0.1≤H1≤15, 0.1≤H2≤15. For example, H1 can be 0.1, 1, 2.5, 4, 5, 7.5, 9, 10, 12, 15, or a range consisting of any two of the above values, and H2 can be 0.1, 1, 2.5, 4, 5, 7.5, 9, 10, 12, 15, or a range consisting of any two of the above values. The bipolar current collector meets the above conditions, which is beneficial to improving the energy density and cycle performance of the electrochemical device.

[0040] ​In some embodiments of the present application, the thickness of the polymer layer is T3 μm, 1≤T3≤20. For example, T3 can be 1, 3, 5, 8, 10, 12, 15, 18, 20, or a range consisting of any two of the above values. By regulating the value of T3 within the above range, it is beneficial to reduce the volume and mass of the bipolar current collector, and at the same time, the bipolar current collector has a higher mechanical strength and is not prone to breakage, so that it is applied to electrochemical devices to improve their energy density.

[0041] In some embodiments of the present application, the material of the polymer layer includes at least one of polyethylene (PE), polypropylene (PP), polystyrene (PS), polyvinyl chloride (PVC) or polyethylene terephthalate (PET). The above-mentioned types of polymer materials have the characteristics of low density, light weight, high temperature resistance, and not easily corroded by electrolyte. The polymer layer is selected from the above materials, and the bipolar current collector has a lighter weight, good stability during the use of the electrochemical device, and is also conducive to absorbing the expansion of the positive electrode active material and the negative electrode active material. Therefore, the bipolar current collector that meets the above conditions is applied to the electrochemical device, which is conducive to improving the energy density and cycle performance of the electrochemical device.

[0042] The present application has no particular restrictions on the preparation method of the bipolar current collector, as long as the purpose of the present application can be achieved. For example, the preparation method of the bipolar current collector may include but is not limited to the following steps: (1) forming a copper layer on one surface of the polymer layer; (2) forming an aluminum layer on the other surface of the polymer layer; (3) drilling holes in the copper layer and the aluminum layer respectively to obtain a bipolar current collector.

[0043] The present application has no particular restrictions on the method of forming the copper layer in the above step (1) and the aluminum layer in the step (2), as long as the purpose of the present application can be achieved. For example, the method of forming the copper layer and / or the aluminum layer can be chemical deposition, magnetron sputtering or vacuum evaporation. The present application has no particular restrictions on the process parameters of chemical deposition, magnetron sputtering or vacuum evaporation, and those skilled in the art can choose according to actual needs, as long as the purpose of the present application can be achieved. The present application has no particular restrictions on the method of punching holes in the copper layer and the aluminum layer in the above step (3), as long as the purpose of the present application can be achieved. For example, the method of punching holes in the copper layer and the aluminum layer can be chemical etching, laser drilling or mechanical drilling independently. The above chemical etching method can include but is not limited to: after the bipolar current collector is degreased, hydrochloric acid is used as an etching solution, and the hydrochloric acid concentration, etching time and etching temperature are adjusted to etch pores on the surface of the copper layer and the aluminum layer respectively. The above laser drilling method can include but is not limited to: processing the bipolar current collector using femtosecond laser technology to obtain a porous bipolar current collector. The above-mentioned mechanical punching method may include but is not limited to: punching or punching the bipolar current collector using a mold or a punch to obtain a porous bipolar current collector. The present application has no particular restrictions on the distribution of pores in the copper layer and the aluminum layer, as long as the purpose of the present application can be achieved. For example, the distribution of pores in the copper layer and the aluminum layer can be evenly distributed or unevenly distributed.

[0044] The present application does not particularly limit the method for regulating the porosity A1 of the copper layer and the porosity A2 of the aluminum layer, as long as the purpose of the present application can be achieved. For example, it can be obtained by regulating the number of holes per unit area of ​​the copper layer and the aluminum layer. When other conditions remain unchanged, the number of holes per unit area of ​​the copper layer increases, A1 increases, the number of holes per unit area of ​​the copper layer decreases, and A1 decreases; the number of holes per unit area of ​​the aluminum layer increases, A2 increases; the number of holes per unit area of ​​the aluminum layer decreases, and A2 decreases. For example, it can be obtained by regulating the average pore size D1 of the copper layer and the average pore size D2 of the aluminum layer. When other conditions remain unchanged, D1 increases, A1 increases, D2 increases, and A2 increases; D1 decreases, A1 decreases, D2 decreases, and A2 decreases. For example, it can be obtained by regulating the depth H1 of the first hole and the depth H2 of the second hole. When other conditions remain unchanged, H1 increases, A1 increases, H2 increases, and A2 increases; H1 decreases, A1 decreases, H2 decreases, and A2 decreases.

[0045] The present application does not particularly limit the method for regulating the thickness T1 of the copper layer and the thickness T2 of the aluminum layer, as long as the purpose of the present application can be achieved. For example, it can be obtained by regulating the deposition time during the preparation of the copper layer and the aluminum layer. When other conditions remain unchanged, the deposition time increases during the preparation of the copper layer, T1 increases, and the deposition time increases during the preparation of the aluminum layer, T2 increases; the deposition time decreases during the preparation of the copper layer, T1 decreases, and the deposition time decreases during the preparation of the aluminum layer, T2 decreases.

[0046] The second aspect of the present application provides an electrochemical device, which includes a bipolar pole piece, and the bipolar pole piece includes the bipolar current collector provided in the first aspect of the present application. The electrochemical device provided by the present application has high energy density and power density and good cycle performance. The surface of the aluminum layer of the bipolar current collector is provided with a positive electrode material layer, and the surface of the copper layer of the bipolar current collector is provided with a negative electrode material layer. It should be noted that the "surface" here can be the entire area of ​​the bipolar current collector or a partial area of ​​the bipolar current collector. There is no special limitation in the present application, as long as the purpose of the present application can be achieved.

[0047] The present application has no particular limitation on the coating surface density of the positive electrode material layer, as long as the purpose of the present application can be achieved. For example, the coating surface density of the positive electrode material layer can be 8 mg / cm 2 Up to 20mg / cm 2 The present application has no particular limitation on the coating surface density of the negative electrode material layer, as long as the purpose of the present application can be achieved. For example, the coating surface density of the negative electrode material layer can be 4 mg / cm 2 Up to 15mg / cm 2 The present application has no particular restrictions on the compaction density of the positive electrode material layer and the negative electrode material layer, as long as the purpose of the present application can be achieved. For example, the compaction density of the positive electrode material layer can be 1g / cm 3 Up to 5g / cm 3 The compaction density of the negative electrode material layer can be 0.5g / cm 3 Up to 2g / cm 3 .

[0048] The positive electrode material layer of the present application includes a positive electrode active material, and the positive electrode active material includes a substance that can reversibly embed and extract active ions such as lithium ions. The positive electrode material layer can be one or more layers, and each layer in the multi-layer positive electrode material layer can contain the same or different positive electrode active materials. The present application has no special restrictions on the positive electrode active material, as long as the purpose of the present application can be achieved. For example, the positive electrode active material may include but is not limited to lithium nickel cobalt manganese oxide (such as NCM811, NCM622, NCM523, NCM111), lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium-rich manganese-based materials, lithium cobalt oxide (LiCoO2), lithium manganese oxide, lithium iron manganese phosphate or lithium titanate. The chemical formula of the above-mentioned lithium-rich manganese-based material is γLi2MnO3·(1-γ)LiGO2, 0<γ<1, and G is a transition metal nickel, cobalt, manganese or iron. In the present application, the surface of the positive electrode active material may be attached with a substance having a different composition from the positive electrode active material. For example, the substance attached to the surface may include, but is not limited to, at least one of aluminum oxide, silicon dioxide, titanium dioxide, zirconium oxide, magnesium oxide, calcium oxide, boron oxide, antimony oxide, bismuth oxide, lithium sulfate, sodium sulfate, potassium sulfate, magnesium sulfate, calcium sulfate, aluminum sulfate, lithium carbonate, calcium carbonate, magnesium carbonate, or carbon. By attaching the above substances to the surface of the positive electrode active material, it is beneficial to inhibit the oxidation reaction of the electrolyte on the surface of the positive electrode active material, thereby increasing the service life of the electrochemical device.

[0049] The positive electrode material layer may also include a positive electrode conductor and a positive electrode binder. The present application has no particular restrictions on the types of the positive electrode conductor and the positive electrode binder, as long as the purpose of the present application can be achieved. For example, the positive electrode binder may include but is not limited to polyvinyl alcohol, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylic (ester) styrene-butadiene rubber, epoxy resin or nylon; the positive electrode conductor may include but is not limited to at least one of carbon-based materials, metal-based materials or conductive polymers. Exemplarily, the carbon-based material may include at least one of natural graphite, artificial graphite, conductive carbon black (Super P) or carbon fiber, the metal-based material may include but is not limited to at least one of metal powder, metal fiber, copper, nickel, aluminum or silver; the conductive polymer may include but is not limited to polyphenylene derivatives. The present application has no particular restriction on the mass ratio of the positive electrode active material, the positive electrode conductive agent, and the positive electrode binder in the positive electrode material layer, which can be selected according to actual needs as long as the purpose of the present application can be achieved.

[0050] The negative electrode material layer of the present application includes a negative electrode active material. The negative electrode material layer can be one or more layers, and each layer of the multiple negative electrode material layers can contain the same or different negative electrode active materials. The negative electrode active material is any substance that can reversibly embed and extract active ions such as lithium ions. The negative electrode active material can include but is not limited to graphite, mesophase microcarbon beads (MCMB), hard carbon, soft carbon, silicon, silicon-carbon composites, SiO x (0<x≤2), Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, spinel structure lithium titanate TiO2-Li4Ti5O 12 , Li-Al alloy and at least one of metallic lithium.

[0051] The negative electrode material layer in the present application may also include a negative electrode binder and a negative electrode conductor, or the negative electrode material layer may also include a negative electrode binder, a negative electrode conductor or a thickener. The present application has no particular restrictions on the types of negative electrode binders and negative electrode conductors, as long as the purpose of the present application can be achieved. For example, the negative electrode binder may include but is not limited to at least one of the above-mentioned positive electrode binders, and the negative electrode conductor may include but is not limited to at least one of the above-mentioned positive electrode conductors. The present application has no particular restrictions on the types of thickeners, as long as the purpose of the present application can be achieved. For example, the thickener may include but is not limited to at least one of sodium carboxymethyl cellulose or carboxymethyl cellulose. The present application has no particular restrictions on the mass ratio of the negative electrode active material, the negative electrode conductor, the thickener and the negative electrode binder in the negative electrode material layer, as long as the purpose of the present application can be achieved.

[0052] The electrochemical device of the present application also includes an electrolyte, and the electrolyte includes a lithium salt and a non-aqueous solvent. The lithium salt may include various lithium salts commonly used in the art, such as at least one of LiPF6, LiBF4, LiAsF6, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, Li2SiF6, lithium bis(oxalate)borate (LiBOB) or lithium difluoroborate. The present application has no particular restrictions on the concentration of lithium salts in the electrolyte, as long as the purpose of the present application can be achieved. The present application has no particular restrictions on non-aqueous solvents, as long as the purpose of the present application can be achieved, for example, it may include but is not limited to at least one of carbonate compounds, carboxylate compounds, ether compounds or other organic solvents. The above-mentioned carbonate compounds may include but are not limited to at least one of chain carbonate compounds, cyclic carbonate compounds or fluorinated carbonate compounds. The above-mentioned linear carbonate compound may include but is not limited to at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methylpropyl carbonate (MPC), ethylpropyl carbonate (EPC) or ethylmethyl carbonate (EMC). The above-mentioned cyclic carbonate may include but is not limited to at least one of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC) or vinylethylene carbonate (VEC). The above-mentioned fluorinated carbonate compound may include but is not limited to at least one of fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate or trifluoromethylethylene carbonate. The above-mentioned carboxylate compound may include but is not limited to at least one of methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decanolactone, valerolactone or caprolactone. The above-mentioned ether compound may include but is not limited to at least one of dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, 1-ethoxy-1-methoxyethane, 2-methyltetrahydrofuran or tetrahydrofuran. The above-mentioned other organic solvents may include but are not limited to at least one of dimethyl sulfoxide, 1,2-dioxolane, cyclopentane, methyl cyclopentane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate or trioctyl phosphate.

[0053] In the present application, the electrochemical device also includes a separator, which is used to separate the bipolar pole pieces, prevent the internal short circuit of the electrochemical device, allow the electrolyte ions to pass freely, and do not affect the electrochemical charge and discharge process. The present application has no special restrictions on the separator, as long as the purpose of the present application can be achieved. For example, the material of the separator may include but is not limited to polyethylene (PE), polypropylene (PP)-based polyolefins (PO), polyesters (such as polyethylene terephthalate (PET) film), cellulose, polyimide (PI), polyamide (PA), spandex or aramid; the type of the separator may include at least one of a woven membrane, a non-woven membrane, a microporous membrane, a composite membrane, a rolled membrane or a spun membrane. For example, the separator may include a substrate layer and a surface treatment layer. The substrate layer may be a non-woven fabric, a membrane or a composite membrane with a porous structure, and the material of the substrate layer may include at least one of polyethylene, polypropylene, polyethylene terephthalate or polyimide. Optionally, a polypropylene porous membrane, a polyethylene porous membrane, a polypropylene non-woven fabric, a polyethylene non-woven fabric or a polypropylene-polyethylene-polypropylene porous composite membrane may be used. Optionally, a surface treatment layer is provided on at least one surface of the substrate layer, and the surface treatment layer may be a polymer layer or an inorganic layer, or a layer formed by a mixed polymer and an inorganic substance. For example, the inorganic layer includes inorganic particles and a binder, and the present application has no particular restrictions on the inorganic particles, for example, it may include at least one of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide or barium sulfate. The present application has no particular restrictions on the binder in the inorganic layer, for example, it may be at least one of the above-mentioned positive electrode binders. The polymer layer contains a polymer, and the present application has no particular restrictions on the polymer, for example, the polymer includes at least one of polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyacrylate, polyvinyl pyrrolidone, polyvinyl ether or polyvinylidene fluoride or poly (vinylidene fluoride-hexafluoropropylene). In the present application, there is no particular limitation on the thickness of the isolation film, as long as the purpose of the present application can be achieved. For example, the thickness of the isolation film may be 5 μm to 30 μm.

[0054] The electrochemical device of the present application also includes a packaging bag for containing a bipolar pole piece, a separator and an electrolyte, as well as other components known in the art in the electrochemical device, and the present application has no particular restrictions on the above-mentioned other components. The present application has no particular restrictions on the packaging bag, and it can be a packaging bag known in the art, as long as it can achieve the purpose of the present application. For example, an aluminum-plastic film packaging bag can be used.

[0055] The electrochemical device of the present application is not particularly limited, and may include any device that undergoes an electrochemical reaction. In some embodiments, the electrochemical device may include, but is not limited to, a lithium ion battery, a sodium ion battery, a lithium polymer electrochemical device, or a lithium ion polymer electrochemical device.

[0056] The present application does not particularly limit the preparation method of the electrochemical device, as long as the purpose of the present application can be achieved. For example, the preparation method of the electrochemical device includes but is not limited to the following steps: stacking the separator and the bipolar pole piece, winding to obtain an electrode assembly of a winding structure, placing the electrode assembly in a packaging bag, injecting an electrolyte into the packaging bag and sealing it to obtain an electrochemical device; or stacking the separator and the bipolar pole piece, and then fixing the four corners of the entire stacked structure to obtain an electrode assembly of a stacked structure, placing the electrode assembly in a packaging bag, injecting an electrolyte into the packaging bag and sealing it to obtain an electrochemical device.

[0057] The third aspect of the present application provides an electronic device, which includes the electrochemical device provided in the second aspect of the present application. The electrochemical device provided in the present application has high energy density and power density and good cycle performance, so that the electronic device provided in the present application has a long service life and good performance.

[0058] The electronic device of the present application is not particularly limited, and it can be used for any electronic device known in the prior art. For example, the electronic device can include but is not limited to a laptop computer, a pen-input computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, a liquid crystal television, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery, and a lithium-ion capacitor.

[0059] Example Hereinafter, the embodiments of the present application will be described in more detail with reference to Examples and Comparative Examples. Various tests and evaluations were performed according to the following methods. In addition, unless otherwise specified, "parts" and "%" are by mass.

[0060] Test methods and equipment: Sampling method of bipolar current collector After the lithium-ion batteries of each embodiment and comparative example are discharged to 2.5V at 0.1C, they are disassembled to obtain bipolar pole pieces, and then the positive electrode material layer and the negative electrode material layer are scraped off to obtain a bipolar current collector. After the bipolar current collector is cleaned with dimethyl carbonate (DMC), it is dried at 60°C to obtain a bipolar current collector sample. The bipolar current collector sample is cut in a direction parallel to the plane defined by the thickness direction and the width direction, and in a direction parallel to the plane defined by the thickness direction and the length direction to obtain a rectangular sample with a length of 20 mm and a width of 10 mm. The following tests of porosity, average pore size, thickness, and the depth of the first hole and the second hole can be obtained by using the above sampling method to obtain a rectangular sample.

[0061] Porosity test Industrial CT (Zeiss Xradia 620 Versa) was used to perform tomography on the rectangular sample to obtain a three-dimensional image of the rectangular sample. The outer contour volume X1 of the copper layer, the volume Y1 of the pores in the copper layer, and the outer contour volume X2 of the aluminum layer and the volume Y2 of the pores in the aluminum layer in the rectangular sample were obtained by image analysis. The porosity A1 of the copper layer was calculated by the following formula: A1 (%) = Y1 / X1 × 100%. The porosity A2 of the aluminum layer was calculated by the following formula: A2 (%) = Y2 / X2 × 100%.

[0062] Average pore size test An industrial CT (Zeiss Xradia 620 Versa) was used to perform tomography on the rectangular sample to obtain a three-dimensional image of the rectangular sample. Ten holes were randomly selected in the copper layer, and the circumscribed circle diameter of the hole shape was obtained by image analysis. The average value of the above 10 circumscribed circle diameters was calculated as the average pore size D1 of the copper layer. Ten holes were randomly selected in the aluminum layer, and the circumscribed circle diameter of the hole shape was obtained by image analysis. The average value of the above 10 circumscribed circle diameters was calculated as the average pore size D2 of the aluminum layer.

[0063] Thickness test An industrial CT (Zeiss Xradia 620 Versa) was used to perform a tomographic scan on the rectangular sample to obtain a three-dimensional image of the rectangular sample. Ten unpunched areas were selected, and the thickness of the copper layer, aluminum layer, and polymer layer in the above 10 unpunched areas was obtained by image analysis, and the average values ​​were calculated as the thickness T1 of the copper layer, the thickness T2 of the aluminum layer, and the thickness T3 of the polymer layer.

[0064] Depth test of the first and second holes An industrial CT (Zeiss Xradia 620 Versa) was used to perform a tomographic scan on the rectangular sample to obtain a three-dimensional image of the rectangular sample. Ten first holes were selected, and the depth of the first holes was obtained by image analysis. The average value was calculated as the depth H1 of the first hole. Ten second holes were selected, and the depth of the second holes was obtained by image analysis. The average value was calculated as the depth H2 of the second hole.

[0065] Energy density test At 25°C, the lithium-ion battery was charged at a constant current of 0.2C to a voltage of 4.30V, then charged at a constant voltage of 4.30V to a current of 0.05C, and left to stand for 15 minutes; then discharged at a constant current of 0.2C to a voltage of 2.5V. The discharge energy at this time was tested and recorded by a battery tester (Neware CTE-4016-5V-200A), which was recorded as the energy E of the lithium-ion battery; and the mass of the lithium-ion battery was measured and recorded as m. The energy density was calculated by the following formula: Energy density (Wh / kg) = E / m.

[0066] Internal resistance test The lithium-ion batteries of each embodiment and comparative example were placed in a 25°C constant temperature box and left to stand for 30 minutes. The lithium-ion batteries were then charged at a constant current of 0.2C to a voltage of 4.30V, and then charged at a constant voltage of 4.30V to a current of 0.05C. After standing for 15 minutes, they were discharged at 0.2C to 2.5V, and then an internal resistance tester was used to apply an AC signal of 1kHz to the lithium-ion battery. The internal resistance of the lithium-ion battery is calculated by the following formula: internal resistance R=ΔU / I, where ΔU is the voltage change at both ends of the lithium-ion battery when an AC signal is applied, and I is the AC current passing through the lithium-ion battery at the same time. The power density of the lithium-ion battery is evaluated by its internal resistance. The larger the internal resistance of the lithium-ion battery, the smaller the power density, and the smaller the internal resistance, the greater the power density.

[0067] Cycle performance test (1) Cycle capacity retention rate test At 25°C, the lithium-ion battery was charged at a constant current of 1.0C to a voltage of 4.30V, then charged at a constant voltage of 4.30V to a current of 0.05C, and allowed to stand for 15 minutes; then discharged at a constant current of 4.0C to a voltage of 2.5V, and allowed to stand for 15 minutes. The above is a charge and discharge cycle. The discharge capacity was tested by a battery tester (Neware CTE-4016-5V-200A) and recorded as the initial capacity Q0. According to the above charge and discharge method, 500 cycles were cycled, and the discharge capacity of the 500th cycle was recorded as the capacity Q1 after 500 cycles. The cycle capacity retention rate was calculated by the following formula: Cycle capacity retention rate (%) = Q1 / Q0×100%.

[0068] (2) Cyclic expansion rate test The lithium-ion battery was placed in a 25°C environment and charged at a constant current of 1.0C to a voltage of 3.60V, that is, the initial thickness of the lithium-ion battery was tested in a half-charged state, which was recorded as T0; the lithium-ion battery was charged at a constant current of 1.0C to a voltage of 4.30V, and then charged at a constant voltage of 4.30V to a current of 0.05C, and then left to stand for 15 minutes; then discharged at a constant current of 4.0C to a voltage of 2.5V, and left to stand for 15 minutes. The above is a charge and discharge cycle. After 500 cycles according to the above charge and discharge method, the lithium-ion battery was charged at a constant current of 1.0C to a voltage of 4.30V, and then charged at a constant voltage of 4.30V to a current of 0.05C to reach a full charge state, and the thickness of the lithium-ion battery was tested, which was recorded as T1. The cycle expansion rate was calculated by the following formula: Cycle expansion rate (%) = (T1-T0) / T0×100%.

[0069] Example 1-1 <Preparation of Bipolar Current Collector> In the polymer layer PET (weight average molecular weight Mw = 2×10 4 A copper layer with a thickness of 2 μm T1 is formed on one surface of the PET sheet by vacuum evaporation, and an aluminum layer with a thickness of 2 μm T2 is formed on the other surface of the polymer layer PET sheet by vacuum evaporation. The copper layer and the aluminum layer are respectively punched by laser drilling, wherein the porosity A1 of the copper layer and the porosity A2 of the aluminum layer are shown in Table 1, and the average pore size D1 of the copper layer, the average pore size D2 of the aluminum layer, the depth H1 of the first hole, and the depth H2 of the second hole are shown in Table 2.

[0070] <Preparation of bipolar pole piece> The positive electrode active material is lithium nickel cobalt manganese oxide NCM811, the positive electrode conductive agent is conductive carbon black (Super P), and the positive electrode binder is polyvinylidene fluoride (PVDF, Mw = 7×10 6 ) were mixed in a weight ratio of 95:3:2, N-methylpyrrolidone (NMP) was added as a solvent, a positive electrode slurry with a solid content of 65wt% was prepared, and the slurry was stirred evenly.

[0071] The negative electrode active material artificial graphite, the negative electrode active material silicon, the negative electrode conductive agent conductive carbon black (Super P), the negative electrode binder styrene butadiene rubber (SBR, Mw = 5×10 6 ) are mixed in a weight ratio of 74:20:1:5, deionized water is added as a solvent, and a negative electrode slurry with a solid content of 70wt% is prepared, and the mixture is stirred evenly.

[0072] The positive electrode slurry is evenly coated on the aluminum layer of the bipolar current collector and dried at 85°C to form a positive electrode material layer. After drying, the coating surface density of the positive electrode material layer is 13 mg / cm 2The negative electrode slurry is evenly coated on the copper layer of the bipolar current collector and dried at 110°C to form a negative electrode material layer. After drying, the coating surface density of the negative electrode material layer is 8 mg / cm 2 After cold pressing, slitting and welding of the pole ears, a bipolar pole piece with a specification of 50mm×80mm is obtained, in which the compaction density of the positive electrode material layer is 3.5g / cm 3 The compaction density of the negative electrode material layer is 1.6 g / cm 3 Then, auxiliary processes such as pole ear welding and adhesive tape are carried out to complete the preparation process of bipolar pole pieces.

[0073] <Preparation of Electrolyte> In a dry argon atmosphere, non-aqueous solvents ethylene carbonate (EC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC) are first mixed in a mass ratio of EC:EMC:DEC=30:50:20, and then lithium salt lithium hexafluorophosphate (LiPF6) is added to the non-aqueous solvent to dissolve and mix evenly to obtain an electrolyte with a lithium salt concentration of 1.15 mol / L.

[0074] <Preparation of Separator Film> A polyethylene (PE) porous polymer film with a thickness of 8 μm (provided by Celgard) was used as the isolation membrane.

[0075] <Preparation of lithium-ion batteries> The prepared isolation membrane and bipolar pole piece are alternately stacked, with 21 isolation membrane layers and 22 bipolar pole pieces. The four corners of the entire stacked structure are then fixed to obtain an electrode assembly of the stacked structure. The electrode assembly is placed in an aluminum-plastic film packaging bag, and after drying, the electrolyte is injected. After vacuum packaging, standing, formation (0.02C constant current charging to 3.3V, then 0.1C constant current charging to 4.0V), shaping and other processes, a lithium-ion battery is obtained.

[0076] Example 1-2 to Example 1-14 Except for adjusting the relevant preparation parameters in <Preparation of Bipolar Current Collector> according to Table 1, the rest is the same as Example 1-1. Among them, the thickness T1 of the copper layer is regulated by adjusting the deposition time during the preparation of the copper layer, and the thickness T2 of the aluminum layer is regulated by adjusting the deposition time during the preparation of the aluminum layer. The porosity A1 of the copper layer is regulated by adjusting the punching density of the copper layer, and the porosity A2 of the aluminum layer is regulated by adjusting the punching density of the aluminum layer.

[0077] Example 2-1 to Example 2-14 Except for adjusting the relevant preparation parameters in <Preparation of Bipolar Current Collector> according to Table 2, the rest is the same as Example 1-1. In Example 2-10, along the thickness direction of the bipolar current collector, the projection of the first hole and the projection of the second hole are separated.

[0078] Comparative Example 1 Except that the copper layer and the aluminum layer are not perforated in <Preparation of Bipolar Current Collector>, the rest is the same as Example 1-1.

[0079] Comparative Example 2 to Comparative Example 5 Except for adjusting the relevant preparation parameters in <Preparation of Bipolar Current Collector> according to Table 1, the rest is the same as Example 1-1. Among them, the thickness T1 of the copper layer is regulated by adjusting the deposition time during the preparation of the copper layer, and the thickness T2 of the aluminum layer is regulated by adjusting the deposition time during the preparation of the aluminum layer. The porosity A1 of the copper layer is regulated by adjusting the punching density of the copper layer, and the porosity A2 of the aluminum layer is regulated by adjusting the punching density of the aluminum layer.

[0080] The preparation parameters and performance parameters of each embodiment and comparative example are shown in Tables 1 and 2.

[0081] Table 1

[0082] From Examples 1-1 to 1-14 and Comparative Examples 1 to 5, it can be seen that the lithium-ion battery in the embodiments of the present application satisfies the following conditions by regulating T1, T2, A1, and A2 of the bipolar current collector: T2 (1-A2) > T1 (1-A1), and the lithium-ion battery has a higher energy density and cycle capacity retention rate, as well as a lower internal resistance and cycle expansion rate, indicating that the lithium-ion battery has a higher energy density and power density and good cycle performance. However, in the lithium-ion batteries of Comparative Examples 1 to 5, the bipolar current collectors T1, T2, A1, and A2 do not satisfy the above relationship, and the lithium-ion batteries of Comparative Examples 1 to 5 cannot simultaneously have a higher energy density and cycle capacity retention rate, as well as a lower internal resistance and cycle expansion rate, indicating that the lithium-ion battery cannot simultaneously have a higher energy density and power density and good cycle performance.

[0083] The values ​​of T1 and T2 usually affect the energy density, power density and cycle performance of lithium-ion batteries. It can be seen from Examples 1-1 to 1-10 that when the values ​​of T1 and T2 are within the range of this application, the lithium-ion battery has a higher energy density and cycle capacity retention rate, as well as a lower internal resistance and cycle expansion rate, indicating that the lithium-ion battery has a higher energy density and power density and good cycle performance.

[0084] The value of T2 / T1 usually affects the energy density, power density and cycle performance of lithium-ion batteries. It can be seen from Examples 1-1, 1-3, 1-8 to 1-10 that when the value of T2 / T1 is within the range of the present application, the lithium-ion battery has a higher energy density and cycle capacity retention rate, as well as a lower internal resistance and cycle expansion rate, indicating that the lithium-ion battery has a higher energy density and power density and good cycle performance.

[0085] The values ​​of A1 and A2 usually affect the energy density, power density and cycle performance of lithium-ion batteries. It can be seen from Examples 1-1, 1-2, 1-11 to 1-14 that when the values ​​of A1 and A2 are within the range of this application, the lithium-ion battery has a higher energy density and cycle capacity retention rate, as well as a lower internal resistance and cycle expansion rate, indicating that the lithium-ion battery has a higher energy density and power density and good cycle performance.

[0086] Table 2

[0087] Note: In Table 2, T1=2μm, T2=2μm for Examples 2-1 to 2-14, and Mw=3×10 4 , the Mw of PS in Example 2-14 is 6×10 4 .

[0088] The values ​​of D1 and D2 usually affect the energy density, power density and cycle performance of lithium-ion batteries. It can be seen from Examples 1-1, 2-1 to 2-5 that when the values ​​of D1 and D2 are within the range of this application, the lithium-ion battery has a higher energy density and cycle capacity retention rate, as well as a lower internal resistance and cycle expansion rate, indicating that the lithium-ion battery has a higher energy density and power density and good cycle performance.

[0089] The size relationship between H1 and T1 and T3, the size relationship between H2 and T2 and T3, and the size relationship between H1+H2 and T1+T2+T3 usually affect the energy density, power density and cycle performance of lithium-ion batteries. It can be seen from Examples 1-1, 2-6 to 2-10 that when the size relationship between H1 and T1 and T3, the size relationship between H2 and T2 and T3, and the size relationship between H1+H2 and T1+T2+T3 are within the scope of this application, the lithium-ion battery has a higher energy density and cycle capacity retention rate, as well as a lower internal resistance and cycle expansion rate, indicating that the lithium-ion battery has a higher energy density and power density and good cycle performance.

[0090] The value of T3 usually affects the energy density, power density and cycle performance of lithium-ion batteries. It can be seen from Examples 1-1, 2-11 and 2-12 that when the value of T3 is within the range of the present application, the lithium-ion battery has a higher energy density and cycle capacity retention rate, as well as a lower internal resistance and cycle expansion rate, indicating that the lithium-ion battery has a higher energy density and power density and good cycle performance.

[0091] The material of the polymer layer usually affects the energy density, power density and cycle performance of the lithium-ion battery. It can be seen from Examples 1-1, 2-13 and 2-14 that when the polymer layer material within the scope of the present application is selected, the lithium-ion battery has a higher energy density and cycle capacity retention rate, as well as a lower internal resistance and cycle expansion rate, indicating that the lithium-ion battery has a higher energy density and power density and good cycle performance.

[0092] It should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method or article that includes a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method or article.

[0093] Each embodiment in this specification is described in a related manner, and the same or similar parts between the embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.

[0094] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.

Claims

1. A bipolar current collector, comprising a copper layer, an aluminum layer and a polymer layer, wherein the polymer layer is located between the copper layer and the aluminum layer, the thickness of the copper layer is T1 μm, the thickness of the aluminum layer is T2 μm, the porosity of the copper layer is A1, the porosity of the aluminum layer is A2, and T2 (1-A2) > T1 (1-A1).

2. The bipolar current collector according to claim 1, wherein: The bipolar current collector satisfies any one of the following characteristics: (1) T1=T2, A1>A2; (2) T1<T2, A1=A2; (3) T1<T2, A1>A2.

3. The bipolar current collector according to claim 1 or 2, wherein: 5%≤A1≤45%, 0%≤A2≤30%.

4. The bipolar current collector according to any one of claims 1 to 3, wherein: 0.5≤T1≤10, 0.5≤T2≤10.

5. The bipolar current collector according to claim 4, wherein: 1≤T2 / T1≤4.

6. The bipolar current collector according to any one of claims 1 to 5, wherein: The average pore size of the copper layer is D1 μm, the average pore size of the aluminum layer is D2 μm, 20≤D1≤400, 20≤D2≤400.

7. The bipolar current collector according to any one of claims 1 to 6, wherein: The surface of the copper layer away from the polymer layer is the first surface, the surface of the aluminum layer away from the polymer layer is the second surface, the bipolar current collector includes a plurality of first holes and a plurality of second holes, the first holes extend from the first surface along the thickness direction of the bipolar current collector, the second holes extend from the second surface along the thickness direction of the bipolar current collector, the depth of the first holes is H1 μm, the depth of the second holes is H2 μm, the thickness of the polymer layer is T3 μm, and the bipolar current collector satisfies any one of the following characteristics: (1) H1≤T1, H2≤T2; (2) T1<H1<T1+T3 and / or T2<H2<T2+T3, and H1+H2<T1+T2+T3; (3) T1<H1<T1+T3, T2<H2<T2+T3, H1+H2≥T1+T2+T3, and along the thickness direction of the bipolar current collector, the projection of the first hole is separated from the projection of the second hole.

8. The bipolar current collector according to any one of claims 1 to 7, wherein: The thickness of the polymer layer is T3 μm, 1≤T3≤20.

9. The bipolar current collector according to any one of claims 1 to 8, wherein: The material of the polymer layer includes at least one of polyethylene, polypropylene, polystyrene, polyvinyl chloride or polyethylene terephthalate.

10. An electrochemical device, wherein: The electrochemical device comprises a bipolar pole piece, and the bipolar pole piece comprises the bipolar current collector according to any one of claims 1 to 9.

11. An electronic device, wherein: The electronic device comprises the electrochemical device according to claim 10.

Citation Information

Cited By

  • Bipolar current collector, electrochemical device, and electronic device

    WO2026007803A1

  • Current collector, electrode, and secondary battery

    WO2026134657A1