Electron donating type composite material bipolar plate as well as preparation method and application thereof
By intercalating graphite to form nickel-graphite interlayer compounds and surface modification treatment, the problem of high vertical resistance and performance attenuation of flexible graphite bipolar plates is solved, and a bipolar plate with high conductivity and mechanical strength is achieved, which is suitable for liquids. Applications of flow batteries and hydrogen fuel cells.
Patent Information
- Application Number
- CN202411178151.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure CN118738427A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of liquid flow energy storage batteries, and in particular relates to an electron-donating composite material bipolar plate and a preparation method and application thereof. Background Art
[0002] In recent years, vanadium redox flow batteries have entered the commercial application stage with their excellent safety and long-term energy storage advantages. Recently, in order to improve competitiveness, reducing the cost of battery stacks, improving battery performance, and reducing battery performance degradation have become important technical links in the development of vanadium redox flow batteries.
[0003] Bipolar plates are important components of vanadium flow batteries. They connect the positive and negative electrodes of different cells and produce electrochemical reactions to conduct current. The electrochemical reactions of the electrolyte at the positive and negative electrodes are as follows:
[0004] Among many bipolar plates, flexible graphite bipolar plates have become the mainstream product due to their good conductivity and excellent mechanical strength. Flexible graphite bipolar plates are mainly made of expanded graphite and PVDF, epoxy resin and other adhesive materials, and are made through a hot pressing process. In actual application, it is found that the vertical resistance of flexible graphite bipolar plates is high, which can easily cause battery performance degradation, and due to poor toughness, it is easy to crack during the packaging process.
[0005] Therefore, developing high-performance flexible graphite bipolar plates, improving vertical conductivity, reducing battery attenuation, and being suitable for large-scale production and application are of great significance to the technological progress and market promotion of liquid flow batteries.
[0006] Chinese Patent: A vanadium liquid flow battery bipolar plate and its preparation process, publication number: CN109768296B, publication date: May 17, 2019. The patent introduces the use of silane coupling agent to modify the surface of carbon cloth and flexible graphite, and the use of epoxy resin and graphite to form a conductive adhesive with bonding effect, and the use of internal mixer and open mixer to prepare conductive adhesive and vacuum molding process to prepare composite bipolar plates. This invention reduces the use of organic solvents, and the prepared vanadium battery composite bipolar plate material has the advantages of high conductivity, good corrosion resistance, excellent mechanical properties and good product stability, which solves the shortcomings and deficiencies of pure graphite plates and conductive plastics as bipolar plate materials in vanadium batteries. However, the value of its vertical resistance has not been reported, and the improvement of battery attenuation performance has not been reflected.
[0007] Adding metal materials to flexible graphite can improve electrical conductivity and reduce the internal resistance of the bipolar plate. Chinese patent: A highly conductive flexible graphite bipolar plate and its preparation method, publication number CN110993982A, publication date April 10, 2020. The patent uses two layers of flexible graphite plates and porous metal layers, metal fiber mesh, foam metal or non-metal to form a sandwich structure, and impregnates it with benzoxazine resin, and finally undergoes a grinding and polishing process to make a bipolar plate for fuel cells. However, due to the poor corrosion resistance of the metal, it is not suitable for vanadium flow batteries. The results of this patent show that the metal wire mesh in flexible graphite can reduce the internal resistance of the bipolar plate and improve the electrical conductivity.
[0008] In the process of preparing graphite composite bipolar plates, due to the extremely high specific surface energy and large van der Waals attraction of graphite and highly conductive carbon black surfaces, conductive carbon black is easy to agglomerate into large particles, which makes it more difficult to disperse in the resin liquid. In addition, the wettability and compatibility of conductive carbon black with the matrix are poor, making it difficult to establish a good interface with the matrix. In addition, as the temperature changes and the battery ages, the binder becomes "fatigued", the physical adhesion decreases, the conductive particles gradually separate from the binder, the conductive material gradually fails, the battery internal resistance increases, the polarization increases, and the battery performance shows a significant attenuation. Therefore, it is necessary to modify the surface of graphite and conductive carbon black to improve the wetting performance so that the mixture can be evenly mixed and a good conductive structure, interface structure and mechanical structure can be formed.
[0009] In order to enhance the uniformity of the mixture of expanded graphite and resin, the Chinese patent: Expanded graphite / phenolic resin composite material bipolar plate and its preparation method, publication number CN101593837A, publication date December 2, 2009, when mixing the expanded graphite / phenolic resin composite material, the expanded graphite is first added to the 100°C thermoplastic phenolic resin aqueous solution for stirring, cooling, filtering, and then the filtered product is dried at 50-100°C for 24 hours to finally obtain the composite material. Although this process solves the problem of graphite and resin delamination, the process is long, involves many equipments, and the process is complicated.
[0010] Silane coupling agents can modify the graphite surface, reduce surface energy, and improve compatibility with resins. Chinese Patent: Polymer Composite Bipolar Plate, Preparation Method and Vanadium Liquid Current, Publication No. CN110474067A, Publication Date November 19, 2019, This patent uses plasticizers and silicone coupling agents to mix carbon black and graphite to prepare carbon-plastic composite bipolar plates. However, the mechanical properties of the bipolar plate are poor (tensile strength 16MPa), and due to the introduction of silane, the impurities therein are prone to battery attenuation.
[0011] In order to improve the chemical stability and mechanical strength of the adhesive, China patented an impregnating resin and its preparation method and application, publication number CN115894822A, publication date April 4, 2023. The patent invented an epoxy acrylic resin with good heat resistance, strong corrosion resistance, good penetration, strong adhesion and other characteristics. The prepared bipolar plate can ensure the safety and stability of the battery stack in long-term operation. However, its internal resistance is high, the conductivity is not optimized, and the bipolar plate is easily compressed and delaminated, which seriously affects the performance of the bipolar plate.
[0012] According to research reports, since the conductive material used in bipolar plates is expanded graphite, impurities such as silicon dioxide and aluminum oxide are prone to electrochemical reactions during the charge and discharge process, causing battery performance to decay. It can be inferred that by doping metal particles in graphite to form electron donor graphite intercalation compounds, the vertical resistance of the bipolar plate can be reduced, its conductivity can be improved, and the battery attenuation performance can be reduced. The application of this graphite intercalation compound in liquid flow batteries has not been reported, so an attempt is made to use graphite intercalation compounds in liquid flow battery composite bipolar plates, and it is hoped that this can be expanded to the field of hydrogen fuel cells.
[0013] The research on the conductive theory and mechanical strength of bipolar plates has become a hot topic in the current energy storage field. It has a guiding role in actual production, but there are still many problems that need to be solved. Summary of the invention
[0014] In view of the problems in the prior art, the present invention provides an electron-donating composite material bipolar plate and its preparation method and application. In order to improve the conductivity of the conductive material and reduce the internal resistance of the bipolar plate of the flow battery, the present invention uses colloidal nickel prepared by redox reaction to intercalate in graphite to form an electron-donating nickel-graphite intercalation compound (Ni-GICs) material; in order to enhance the adhesion between the conductive material and the resin and reduce dust in the environment, soluble acrylic resin is used to modify graphite and carbon black to prevent graphite and carbon black from agglomerating. The conductive premix prepared can be further fused with acrylic epoxy resin, and a composite material bipolar plate with good mechanical strength is made through a molding process.
[0015] The technical solution of the present invention is: An electron-donating composite material bipolar plate, wherein the bipolar plate components include, by mass percentage: carbon powder: 17-25%, graphite: 49-63%, nickel-graphite intercalation compound: 1%-5%, conductive material surface modifier: 1.0-5.0%, thermosetting resin: 14%-20%; The intercalant used in the graphite intercalation compound GICs includes one or a mixture of Mn, Ni, Fe, Co, Cu, and Mo, or one of the commercially available colloidal nickel-coated graphite powders.
[0016] Furthermore, in the above-mentioned electron-donating composite bipolar plate, the carbon powder is one of conductive carbon black, graphitized acetylene black, and vapor-deposited carbon black; more preferably acetylene black, with an iodine absorption value of >80g / kg and a powder resistivity of <0.25Ω.cm; the graphite is one or a mixture of flake graphite, expanded graphite, high-purity graphite, isostatic graphite or colloidal graphite, preferably high-purity graphite with a particle size of >80 mesh.
[0017] Furthermore, in the above-mentioned electron-donating composite material bipolar plate, the conductive material surface modifier is a water-soluble shell-core toughened acrylate polymer. Conductive materials such as graphite and carbon black are difficult to mix with resins due to their very small bulk density and similar surface charges of particles, and are prone to generate dust and pollute the environment. Therefore, it is necessary to reduce the density of the conductive material, perform surface modification, and enhance the mixing and dispersion with the resin. Shell-core toughened acrylate polymers are polymerized from several pure acrylate copolymers or pure propionate emulsions, and have toughening, waterproofing, and anti-seepage functions. It is widely used in powder surface coating and toughening of polymer materials. The use of this polymer in graphite and carbon black mixtures greatly improves the bulk density of the powder, is beneficial to the mixing of conductive fillers and resins, and plays a role in volume expansion, toughening, and anti-seepage.
[0018] Furthermore, in the above-mentioned electron-donating composite material bipolar plate, the thermosetting resin is one of phenolic resin and epoxy resin; the preferred epoxy resin is epoxy acrylate, mainly including at least one of bisphenol A epoxy acrylate and phenolic epoxy acrylate. More preferably, the epoxy acrylate is bisphenol A epoxy acrylate. Since epoxy acrylate has a cross-linked grid structure, it has good mechanical strength and electrochemical stability, and has excellent impermeability and corrosion resistance, and is suitable for the manufacture of liquid flow battery bipolar plates.
[0019] Furthermore, in the electron-donating composite material bipolar plate, the nickel-graphite intercalation compound is an intercalation material of colloidal nickel intercalated graphite formed by a reduction reaction of nickel chloride and hydrazine hydrate in graphite and ethylene glycol slurry. The intercalated graphite is expanded graphite. Expanded graphite has an intercalation structure (SP 2 Hybridization), due to the weak van der Waals force of the interlayer structure and the large interlayer spacing, various substances (atoms, ions and ion clusters) can be inserted into the interlayer gap to form graphite intercalation compounds (GICs). Since the lattice constants of graphite and nickel are close, nickel can form a simple (1×1) adsorption phase between graphite layers. Nickel-graphite intercalation compounds (Ni-GICs) not only maintain the excellent physical and chemical properties of graphite, but also show unique physical and chemical properties such as high conductivity, isotope separation effect, catalytic effect and sealing effect. They are concentrated in battery materials, hydrogen storage materials, sealing materials and high conductivity materials, and have broad prospects.
[0020] The above-mentioned method for preparing an electron-donating composite material bipolar plate has the following process steps: Step S1, preparation of nickel-graphite intercalation compound Ni-GICs: in a water bath at 80°C-90°C, add 155mg-775mg of hydrazine hydrate to a beaker containing 50mL-250mL of ethylene glycol and dissolve it, and set it aside after the hydrazine hydrate is dissolved; add 60mg-300mg of nickel chloride hexahydrate to 50mL-250mL of ethylene glycol solution, then add 10g-50g of expanded graphite, stir and microwave oscillate for 15min to obtain a nickel chloride-graphite suspension; slowly add the nickel chloride-graphite suspension dropwise to the hydrazine hydrate solution for 20-30min, and then react for 20-30min to obtain a graphite intercalation compound formed by colloidal nickel intercalation graphite, filter it, wash it with ethylene glycol or ethanol, and dry it at 75°C-85°C for 4h to obtain a nickel-graphite intercalation compound Ni-GICs; Step S2: Preparation of composite conductive preform: Take 1% to 5% by mass of conductive material surface modifier, add 49% to 63% by mass of graphite and 17% to 25% by mass of carbon powder, stir in a mixer for 30 to 40 minutes, and dry at 75° C. to prepare a composite conductive preform; Step S3, preparation of composite bipolar plate: put 1% to 5% by mass of nickel-graphite intercalation compound, composite conductive prefabricated material, and pre-modulated 14% to 20% by mass of thermosetting resin (epoxy acrylate AB material, A:B=10:1, diluent is 10% to 15% of the resin) into a mixer, mix for 30 minutes, and then form in a kneader to obtain a bipolar plate premix. Finally, take 130±2g of the bipolar plate premix and put it into a mold, hot press under vacuum conditions to make a composite bipolar plate for electronic all-vanadium liquid flow battery.
[0021] Furthermore, in the above-mentioned method for preparing an electron-donating composite material bipolar plate, the conditions for the hot pressing molding in step S3 are: vacuum degree of -0.08 MPa, temperature of 75°C~85°C, and pressure of 20-30 MPa.
[0022] Furthermore, the technical indicators of the above-mentioned electron-donating composite bipolar plate are: tensile strength>35Mpa, bending strength>54MPa, bulk conductivity>150S / cm, vertical resistance<10 mΩ.c㎡, and under the condition of operating at 200 mA / c㎡ in an all-vanadium liquid flow battery, its energy efficiency EE>81%, Coulomb efficiency CE>98.5%, voltage efficiency VE is 82.2% and capacity retention rate is>65% under 100 cycle conditions.
[0023] The electron-donating composite bipolar plate can be used in all-vanadium liquid flow battery packs and can also be extended to hydrogen fuel cells.
[0024] Advantages and beneficial effects of the present invention: 1. Improve the conductivity of composite bipolar plates, reduce vertical resistance, and delay battery performance degradation. In order to improve the conductivity of bipolar plates and reduce the internal resistance of bipolar plates, the present invention prepares nickel-graphite intercalation compounds (Ni-GICs) formed by colloidal nickel intercalated graphite. As an electron-donating conductive material, Ni-GICs synergizes with graphite and carbon black to construct a good conductive path, reduce the internal resistance of the bipolar plate, and solve the problem of battery performance degradation of the bipolar plate. It can be used for long-term operation, laying a strong technical support for improving the performance of bipolar plates, and can be expanded to the field of hydrogen fuel cells, which has far-reaching theoretical guiding significance; 2. Improve the mechanical properties of the composite bipolar plate, increase the toughness of the bipolar plate, and facilitate the completion of the packaging process of the bipolar plate. The present invention uses core-shell acrylic polymer to modify the surface of graphite and carbon black, improves the compatibility of conductive particles with resin, effectively constructs the grid structure of the bipolar plate, enhances the mechanical properties and toughness, reduces the risk of cracking during the packaging process, and prolongs the service life of the bipolar plate; 3. Enhance the dispersibility of conductive materials and reduce environmental pollution. The present invention adopts core-shell toughened acrylic polymer to prepare conductive preforms, which reduces the agglomeration of carbon black, enhances the dispersion between conductive material particles and the compatibility with resin, reduces the dust pollution generated by mixing, and improves the production environment; 4. The preparation method and process of the composite material bipolar plate are simple, the production cost is low, and it is suitable for large-scale production. The raw materials used in the present invention are all commercially available products with a wide range of sources, suitable for large-scale production, and can be promoted and applied. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 Schematic diagram of the hierarchical structure of nickel-graphite intercalation compound, in which the solid line represents the graphite layer; the dotted line represents the intercalation layer nickel; Figure 2 At 150 mA / cm 2 Energy efficiency EE and coulomb efficiency CE curves of the single cell of Example 3 after 146 cycles of constant current charge and discharge at current density; Figure 3 At 150 mA / cm 2 The capacity retention rate curve of the single cell of Example 3 is shown after 146 cycles of constant current charge and discharge at the current density. DETAILED DESCRIPTION
[0026] In order to illustrate the purpose, technical solutions and product performance of the present invention, the specific implementation methods of the present invention are further described in detail in conjunction with examples. The following examples are used to illustrate the present invention but cannot be used to limit the scope of the present invention.
[0027] Unless otherwise specified, the raw materials used in the examples described below are commercially available.
[0028] In the following embodiments, the raw materials are selected as follows: The graphite is high-purity graphite LP-80, with a loose density of 0.5g / cm 3 , particle size 80 mesh (sieve residue 85%), carbon content 99.957%, purchased from Qingdao Dongkai Graphite Co., Ltd.; The carbon powder is conductive carbon black HCD-7, which has a graphitization effect and a specific surface area of 100~260 (m 2 / g), iodine absorption value 550~700g / kg, resistivity 0.08~0.13Ω / m, purchased from Tianjin Huacai Chemical; The thermosetting resin is epoxy acrylate, and the epoxy acrylate is AC816 type acrylic structural adhesive, which is composed of synthetic epoxy acrylate (component A) and modified curing agent (component B), and the mixing ratio is 10:1, purchased from Shenzhen Aosbon Co., Ltd.; the diluent is acryl glycidyl ether, purchased from Myrel; The expanded graphite is 9950350 expanded graphite (EG), purchased from Qingdao Dongkai Graphite Co., Ltd. The conductive material surface modifier is a water-soluble shell-core toughened acrylate polymer, and the shell-core toughened acrylate polymer is a pure acrylic emulsion BA-201 acrylate polymerization emulsion with a solid content of 50% and a viscosity of 100-500 mPa.s, purchased from Shandong Yousuo.
[0029] The ethylene glycol, ethanol, nickel chloride hexahydrate and hydrazine hydrate (80%) are all commercially available chemically pure products.
[0030] The bipolar plate material compositions of the following examples and comparisons are shown in Table 1: Table 1 Composition list of embodiments and comparative examples
[0031] Example 1 The bipolar plate manufacturing process of this embodiment is as follows: Step S1: Preparation of nickel-graphite intercalation compounds (Ni-GICs): In a 500mL beaker, add 50mL of ethylene glycol, then add 155mg of hydrazine hydrate (2.5g / L, 50mmol), mix well in a water bath at 80℃, and set aside; add 50mL of ethylene glycol in another beaker, then add 60mg of nickel chloride hexahydrate (1.2g / L, 5mmol) to dissolve, add 10g of expanded graphite, stir for 15min, and oscillate in a microwave for 15min to obtain a nickel chloride-graphite suspension. Slowly add the nickel chloride-graphite suspension dropwise to the hydrazine hydrate solution, add for 20min, and then react for 20min to obtain an intercalation compound formed by colloidal nickel intercalation graphite. After standing and settling, filter, wash with 10mL of ethanol 3 times, and dry at 75℃ to obtain about 10g of nickel-graphite intercalation compound Ni-GICs, set aside.
[0032] Step S2: Preparation of composite conductive preform: Take 50g (mass percentage 5%) of pure acrylic emulsion BA-201 and dissolve it in 1000ml water, stir it into a solution, add 490g high-purity graphite (mass percentage 49%) and 250g carbon powder (mass percentage 25%) into a mixer, stir for 30min, dry at 75℃ for 4h, and obtain 790g of composite conductive prefabricated material; Step S3: Preparation of composite bipolar plate preform: Weigh 10g of Ni-GICs (1% by mass), 750g of composite conductive prefabricated material, and 200g of prepared epoxy acrylate (20% by mass, 152g of component A, 18g of component B, 30g of diluent, mix evenly) and add them into a mixer and mix for 30 minutes; then transfer them to a kneader for molding, and finally make a bipolar plate prefabricated material.
[0033] Step S4: Preparation of bipolar plates: A certain amount of bipolar plate preform was taken, added into a mold, and pressed in a vacuum leveling machine with a pressing time of 5 minutes, a vacuum degree of -0.08 MPa, a temperature of 75°C, and a pressure of 20 MPa to produce a 0.85 mm thick composite bipolar plate.
[0034] Step S5: Bipolar plate performance test: The mechanical properties test execution standard of bipolar plates is NB / T42007-2013 "Test method for bipolar plates for all-vanadium liquid flow batteries".
[0035] Cut 110×70mm composite bipolar plates and conduct battery performance tests at 200 mA / c㎡.
[0036] Example 2
[0037] Step S1: Preparation of graphite intercalation compounds (Ni-GICs): In a 500mL beaker, add 100mL of ethylene glycol, then add 310mg of hydrazine hydrate (2.5g / L, 50mmol), mix well in a 90℃ water bath, and set aside; add 100mL of ethylene glycol in another beaker, then add 120mg of nickel chloride hexahydrate (1.2g / L, 5mmol) to dissolve, add 20g of expanded graphite, stir for 15min, and microwave for 15min to obtain a nickel chloride-graphite suspension. Slowly add the nickel chloride-graphite suspension dropwise to the hydrazine hydrate solution, add for 30min, and then react for 30min to obtain an intercalation compound formed by colloidal nickel intercalation graphite. After standing and settling, filter, wash with 20mL of ethanol 3 times, and dry at 75℃ to obtain about 20g of nickel-graphite intercalation compound Ni-GICs for later use.
[0038] Step S2: Preparation of composite conductive preform: Take 40g (4% by mass) of pure acrylic emulsion BA-201 and dissolve it in 1000ml of water, stir it into a solution, add 530g of high-purity graphite (53% by mass) and 230g of carbon powder (23% by mass) into a mixer, stir for 40min, and dry it at 75℃ for 4h to obtain 800g of composite conductive prefabricated material; Step S3: Preparation of composite bipolar plate preform: Weigh 20g of Ni-GICs (2% by mass), 790g of conductive prefabricated material, and 180g of prepared epoxy acrylate (18% by mass, 137g of component A, 16g of component B, 27g of diluent, mix evenly) and add them into a mixer and mix for 30 minutes; then transfer them to a kneader for molding, and finally make a bipolar plate prefabricated material.
[0039] Step S4: Preparation of bipolar plates: A certain amount of bipolar plate preform was taken, added into a mold, and pressed in a vacuum leveling machine with a pressing time of 7 minutes, a vacuum degree of -0.08 MPa, a temperature of 75°C, and a pressure of 20 MPa to produce a 0.85 mm thick composite material bipolar plate.
[0040] Step S5: Bipolar plate performance test: The mechanical properties test execution standard of bipolar plates is NB / T42007-2013 "Test method for bipolar plates for all-vanadium liquid flow batteries".
[0041] Cut 110×70mm composite bipolar plates and conduct battery performance tests at 200 mA / c㎡.
[0042] Example 3
[0043] The bipolar plate manufacturing process of this embodiment is as follows: Step S1: Preparation of graphite intercalation compounds (Ni-GICs): In a 500mL beaker, add 150mL of ethylene glycol, then add 465mg of hydrazine hydrate (2.5g / L, 50mmol), mix well in a water bath at 80℃, and set aside; add 150mL of ethylene glycol in another beaker, then add 180mg of nickel chloride hexahydrate (1.2g / L, 5mmol) to dissolve, add 30g of expanded graphite, stir for 15min, and microwave for 15min to obtain nickel chloride-graphite suspension. Slowly add the nickel chloride-graphite suspension dropwise to the hydrazine hydrate solution, add for 30min, and then react for 30min to obtain an intercalation compound formed by colloidal nickel intercalation graphite. After standing and settling, filter, wash with 30mL of ethanol 3 times, and dry at 75℃ to obtain about 30g of nickel-graphite intercalation compound Ni-GICs, set aside.
[0044] Step S2: Preparation of composite conductive preform: Take 30g (3% by mass) of pure acrylic emulsion BA-201 and dissolve it in 1000ml of water, stir it into a solution, add 560g of high-purity graphite (56% by mass) and 220g of carbon powder (22% by mass) into a mixer, stir for 30min, dry it at 75℃ for 4h, and obtain 810g of composite conductive prefabricated material; Step S3: Preparation of composite bipolar plate preform: Weigh 30g of Ni-GICs (3% by mass), 810g of conductive prefabricated material, and 160g of prepared epoxy acrylate (16% by mass, 122g of component A, 14g of component B, 24g of diluent, mix evenly) and add them into a mixer and mix for 30 minutes; then transfer them to a kneader for molding, and finally make a bipolar plate prefabricated material.
[0045] Step S4: Preparation of bipolar plates: A certain amount of bipolar plate preform was taken, added into a mold, and pressed into shape in a vacuum leveling machine for 8 minutes, with a vacuum degree of -0.08 MPa, a temperature of 85°C, and a pressure of 30 MPa to produce a bipolar plate with a thickness of 0.85 mm.
[0046] Step S5: Bipolar plate performance test: The mechanical properties test execution standard of bipolar plates is NB / T42007-2013 "Test method for bipolar plates for all-vanadium liquid flow batteries".
[0047] Cut 110×70mm composite bipolar plates and conduct battery performance tests at 200 mA / c㎡.
[0048] Example 4
[0049] The bipolar plate manufacturing process of this embodiment is as follows: Step S1: Preparation of graphite intercalation compounds (Ni-GICs): In a 1000mL beaker, add 200mL of ethylene glycol, then add 620mg of hydrazine hydrate (2.5g / L, 50mmol), mix well in a water bath at 80℃, and set aside; add 200mL of ethylene glycol in another beaker, then add 240mg of nickel chloride hexahydrate (1.2g / L, 5mmol) to dissolve, add 40g of expanded graphite, stir for 15min, and oscillate in a microwave for 15min to obtain a nickel chloride-graphite suspension. Slowly add the nickel chloride-graphite suspension dropwise to the hydrazine hydrate solution, add it dropwise for 30min, and then react for 30min to obtain an intercalation compound formed by colloidal nickel intercalation graphite. After standing and settling, filter it with suction, wash it with 40mL of ethanol 3 times, and dry it at 75℃ to obtain about 40g of nickel-graphite intercalation compound Ni-GICs, which is set aside.
[0050] Step S2: Preparation of composite conductive preform: Take 20g (mass percentage is 2%) of pure acrylic emulsion BA-201 and dissolve it in 1000ml water, stir it into a solution, add 590g high-purity graphite (mass percentage is 59%) and 200g carbon powder (mass percentage is 20%) into a mixer, stir for 30min, dry it at 80℃ for 4h, and obtain 810g of composite conductive prefabricated material; Step S3: Preparation of composite bipolar plate preform: Weigh 40g of Ni-GICs (4% by mass), 810g of conductive prefabricated material, and 150g of prepared epoxy acrylate (15% by mass, 113g of component A, 14g of component B, 23g of diluent, mix evenly) and add them into a mixer and mix for 30 minutes; then transfer them to a kneader for molding, and finally make a bipolar plate prefabricated material.
[0051] Step S4: Preparation of bipolar plates: A certain amount of bipolar plate preform was taken, added into a mold, and pressed in a vacuum leveling machine with a molding time of 9 minutes, a vacuum degree of -0.08 MPa, a temperature of 85°C, and a pressure of 30 MPa to produce a 0.85 mm thick composite bipolar plate.
[0052] Step S5: Bipolar plate performance test: The mechanical properties test execution standard of bipolar plates is NB / T42007-2013 "Test method for bipolar plates for all-vanadium liquid flow batteries".
[0053] Cut 110×70mm composite bipolar plates and conduct battery performance tests at 200 mA / c㎡.
[0054] Example 5
[0055] The bipolar plate manufacturing process of this embodiment is as follows: Step S1: Preparation of graphite intercalation compounds (Ni-GICs): In a 1000mL beaker, add 250mL of ethylene glycol, then add 775mg of hydrazine hydrate (2.5g / L, 50mmol), mix well in a 90℃ water bath, and set aside; add 250mL of ethylene glycol in another beaker, then add 300mg of nickel chloride hexahydrate (1.2g / L, 5mmol) to dissolve, add 50g of expanded graphite, stir for 15min, and oscillate in a microwave for 15min to obtain a nickel chloride-graphite suspension. Slowly add the nickel chloride-graphite suspension dropwise to the hydrazine hydrate solution, add for 20min, and then react for 30min to obtain an intercalation compound formed by colloidal nickel intercalation graphite. After standing and settling, filter, wash with 50mL of ethanol 3 times, and dry at 75℃ to obtain about 50g of nickel-graphite intercalation compound Ni-GICs for later use.
[0056] Step S2: Preparation of composite conductive preform: Take 10g (mass percentage is 1%) of pure acrylic emulsion BA-201 and dissolve it in 800ml of water, stir it into a solution, add 630g of high-purity graphite (mass percentage is 63%) and 170g of carbon powder (mass percentage is 17%) into a mixer, stir for 30min, dry it at 85℃ for 4h, and obtain 810g of composite conductive prefabricated material; Step S3: Preparation of bipolar plate preform: Weigh 50g of Ni-GICs (5% by mass), 810g of conductive prefabricated material, and 140g of prepared epoxy acrylate (14% by mass, 106g of component A, 13g of component B, 21g of diluent, mix evenly) and add them into a mixer and mix for 30 minutes; then transfer them to a kneader for molding, and finally make a bipolar plate prefabricated material.
[0057] Step S4: Preparation of bipolar plates: A certain amount of bipolar plate preform was taken, added into a mold, and pressed into shape in a vacuum leveling machine for 10 minutes, with a vacuum degree of -0.08 MPa, a temperature of 85°C, and a pressure of 30 MPa to produce a 0.85 mm thick composite bipolar plate.
[0058] Step S5: Bipolar plate performance test: The mechanical properties test execution standard of bipolar plates is NB / T42007-2013 "Test method for bipolar plates for all-vanadium liquid flow batteries".
[0059] Cut 110×70mm composite bipolar plates and conduct battery performance tests at 200 mA / c㎡.
[0060] In order to further describe the effects of the graphite intercalation compounds (Ni-GICs) and the conductive material surface modifier in the examples, a comparative example description is given.
[0061] Comparative Example 1 This comparative example refers to Example 1, without adding interlayer compounds, and the bipolar plate manufacturing process is as follows: Step S1: Preparation of composite conductive preform: Take 50g (mass percentage is 5%) of pure acrylic emulsion BA-201 and dissolve it in 1000ml of water, stir it into a solution, add 500g of high-purity graphite (mass percentage is 50%) and 250g of carbon powder (mass percentage is 25%) into a mixer, stir for 30min, dry it at 75℃ for 4h, and obtain 800g of composite conductive prefabricated material; Step S2: Preparation of bipolar plate preform: Weigh 800g of conductive prefabricated material and 200g of prepared acrylic epoxy resin (mass percentage 20%, 152g of component A, 18g of component B, 30g of diluent, mix evenly) and add them into a mixer and mix for 30 minutes; then transfer them to a kneader for molding, and finally make a bipolar plate prefabricated material.
[0062] Step S3: Preparation of bipolar plates: A certain amount of bipolar plate preform was taken, added into a mold, and pressed in a vacuum leveling machine with a pressing time of 5 minutes, a vacuum degree of -0.08 MPa, a temperature of 75°C, and a pressure of 20 MPa to produce a bipolar plate with a thickness of 0.85 mm.
[0063] Step S4: Bipolar plate performance test: The mechanical properties test execution standard of bipolar plates is NB / T42007-2013 "Test method for bipolar plates for all-vanadium liquid flow batteries".
[0064] Cut bipolar plates of 110×70 mm and conduct battery performance tests at 200 mA / c㎡.
[0065] Comparative Example 2 Comparative Example 2 is compared with Example 2, without graphite intercalation compound, and the bipolar plate manufacturing process is as follows: Step S1: Preparation of composite conductive preform: Take 30g (3% by mass) of pure acrylic emulsion BA-201 and dissolve it in 1000ml of water, stir it into a solution, add 590g of high-purity graphite (59% by mass) and 220g of carbon powder (22% by mass) into a mixer, stir for 30min, dry it at 80℃ for 4h, and obtain 840g of composite conductive prefabricated material; Step S2: Preparation of bipolar plate preform: Weigh 840g of conductive prefabricated material and 160g of prepared acrylic epoxy resin (mass percentage 16%, 122g of component A, 14g of component B, 24g of diluent, mix evenly) and add them into a mixer and mix for 30 minutes; then transfer them to a kneader for molding, and finally make a bipolar plate prefabricated material.
[0066] Step S3: Preparation of bipolar plates: A certain amount of bipolar plate preform was taken, added into a mold, and pressed into shape in a vacuum leveling machine for 10 minutes, with a vacuum degree of -0.08 MPa, a temperature of 85°C, and a pressure of 30 MPa to produce a bipolar plate with a thickness of 0.85 mm.
[0067] Step S4: Bipolar plate performance test: The mechanical properties test execution standard of bipolar plates is NB / T42007-2013 "Test method for bipolar plates for all-vanadium liquid flow batteries".
[0068] Cut bipolar plates of 110×70 mm and conduct battery performance tests at 200 mA / c㎡.
[0069] Comparative Example 3 Comparative Example 3 is compared with Example 3, except that no graphite intercalation compound and conductive material surface modifier are added, and the bipolar plate manufacturing process is as follows: Step S1: Preparation of composite conductive preform: In 1000 ml of water, 590 g of high-purity graphite (mass percentage 59%) and 220 g of carbon powder (mass percentage 22%) were added to a mixer, stirred for 30-40 min, and dried at 75 ° C for 4 h to obtain 810 g of composite conductive preform; Step S2: Preparation of bipolar plate preform: Weigh 810g of conductive prefabricated material and 190g of prepared acrylic epoxy resin (mass percentage 19%, 145g of component A, 17g of component B, 28g of diluent, mix evenly) and add them into a mixer and mix for 30 minutes; then transfer them to a kneader for molding, and finally make a bipolar plate prefabricated material.
[0070] Step S3: Preparation of bipolar plates: A certain amount of bipolar plate preform was taken, added into a mold, and pressed into shape in a vacuum leveling machine for 10 minutes, with a vacuum degree of -0.08 MPa, a temperature of 85°C, and a pressure of 30 MPa to produce a bipolar plate with a thickness of 0.85 mm.
[0071] Step S4: Bipolar plate performance test: The mechanical properties test execution standard of bipolar plates is NB / T42007-2013 "Test method for bipolar plates for all-vanadium liquid flow batteries".
[0072] Cut bipolar plates of 110×70 mm and conduct battery performance tests at 200 mA / c㎡.
[0073] The bipolar plate performance test was conducted on the embodiments of the present invention and the comparative examples, and the implementation standard was NB / T42007-2013, the test method for bipolar plates for all-vanadium redox flow batteries. The test results are shown in Table 2: Table 2 Test results of examples and comparative examples
[0074] Note: The reference bipolar plate is a flexible graphite bipolar plate of a domestic brand.
[0075] At 200mA / cm 2 At the current density, constant current charge and discharge were performed for 10 cycles, and the energy efficiency (EE), coulomb efficiency (CE) and voltage efficiency (VE) test results of the battery of Example 3 and the reference sample are shown in Table 3: Table 3 Example 3 and reference sample at 200mA / cm 2 Table of battery performance data after 10 cycles of discharge at current density
[0076] The data analysis based on Table 2 is as follows: 1. The density of the bipolar plate is related to the amount of resin and conductive filler used, and also to the compaction degree (molding pressure) of the resin and the conductive filler. The density of the bipolar plate will be related to the electrochemical corrosion of the bipolar plate and the attenuation of the battery performance. Therefore, the density of the bipolar plate should be uniform and the compaction degree should be good to prevent the battery performance from attenuating. In the embodiment, as the amount of graphite increases and the amount of resin decreases, the density of the bipolar plate in the embodiment increases. In Comparative Example 3, since the conductive filler is not surface modified, the degree of adhesion between its particles and the resin is relatively low, and the bulk density is relatively low.
[0077] 2. Nickel-graphite intercalation compounds (Ni-GICs) can enhance the conductivity of bipolar plates, especially the lower vertical resistance, which is beneficial to improving battery performance. This is because the electron donor (Ni) particles are inserted into the graphite interlayer to form intercalation compounds such as Figure 1 As shown, the conductivity between graphite particles is improved. The particle size of the nickel (Ni) particles inserted between graphite layers directly affects the conductivity of the interlayer compound. Nickel chloride ions can be inserted between graphite layers (graphite interlayer spacing 0.335nm), and under the reduction of hydrazine hydrate, generate nanoparticles with good dispersion and conductive properties. Reaction conditions such as temperature, time, and concentration affect the particle size of nickel ions. If the concentration is high and the reaction is fast, nickel mirrors or large particles will be generated, which will seriously affect the conductivity of the graphite interlayer compound. In comparing the embodiment with the comparative example and the reference sample, the vertical resistance of the bipolar plate is significantly smaller than that of the comparative example and the reference sample, and the bulk conductivity of the embodiment is significantly greater than the conductivity of the comparative example.
[0078] 3. The conductivity and mechanical strength of the bipolar plate are a pair of contradictions. The type and amount of conductive material determine the conductivity of the bipolar plate, while the type and amount of resin determine the mechanical properties of the bipolar plate. In the embodiment, the added 0-dimensional conductive carbon black and 2-dimensional high-purity graphite have improved adhesion under the action of the core-shell toughening agent, which solves the stratification phenomenon of the reference sample flexible graphite plate, and increases the compatibility with epoxy acrylic resin, further improving the mechanical strength of the bipolar plate. For example, in comparative example 3, no compatibility agent is added, and its mechanical properties are relatively low. In the embodiment, after optimizing the conductive properties and mechanical strength (tensile strength, bending strength), the comprehensive performance of implementation 3 is better.
[0079] 4. The optimized Example 3 has a comprehensive balance between conductivity and mechanical strength, and its battery performance is good. Compared with the reference sample, the toughness of Example 3 is better, while the toughness of the reference sample bipolar plate is poor and relatively brittle; the results in Table 3 show that during the battery test, the long-cycle coulomb efficiency and energy efficiency of the reference sample bipolar plate are lower than those of Example 3, as shown in Table 3 and Figure 2 As shown, the capacity retention rate decays faster, as shown in Figure 3 After disassembling the battery pack, the edges of the reference bipolar plates are prone to brittle fractures or cracks, and are also prone to delamination when squeezed.
[0080] In summary, the nickel-graphite intercalation compound (Ni-GICs) prepared by the present invention has good electrical conductivity, can reduce the vertical resistance of the bipolar plate, improve battery performance, and reduce the risk of battery performance degradation. The use of shell-core toughened acrylic emulsion as a surface modifier for conductive materials improves the adhesion between carbon black and graphite, is conducive to further compatibility with epoxy acrylic resin, increases mechanical strength, and prevents the occurrence of stratification or fracture of the bipolar plate. By optimizing the indicators of electrical conductivity and mechanical properties, the bipolar plate of Example 3 has good battery performance, which is significantly better than the flexible graphite bipolar plate on the market, is suitable for long-term operation under high current density conditions, and has good product market competitiveness.
[0081] The electron-donating composite material bipolar plate of the present invention explores the technical ideas and methods for improving the current technical problems of liquid flow battery bipolar plates from the aspects of conductive mechanism, mechanical properties and production process. Further detailed research is needed to provide reliable technical support for the promotion of liquid flow battery energy storage, fuel cells and other technologies.
[0082] According to the disclosure and description of the above specification, those skilled in the art to which the present invention belongs may also make changes and modifications to the above embodiments. Therefore, the present invention is not limited to the specific embodiments disclosed and described above, and some modifications and changes to the invention should also fall within the scope of protection of the claims of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.
Claims
1. An electron-donating composite material bipolar plate, characterized in that: The bipolar plate components include, by mass percentage: carbon powder: 17% to 25%, graphite: 49% to 63%, graphite intercalation compounds GICs: 1.0% to 5.0%, conductive material surface modifier: 1.0% to 5.0%, thermosetting resin: 14% to 20%; The intercalant used in the graphite intercalation compound GICs includes one or a mixture of Mn, Ni, Fe, Co, Cu, and Mo, or one of the commercially available colloidal nickel-coated graphite powders.
2. The electron-donating composite bipolar plate according to claim 1, characterized in that: The carbon powder is one of conductive carbon black, graphitized acetylene black and vapor-deposited carbon black; the graphite is one of flake graphite, expanded graphite, high-purity graphite, isostatic graphite or colloidal graphite or a mixture of several of them.
3. The electron-donating composite bipolar plate according to claim 1, characterized in that: The conductive material surface modifier is one or a mixture of several of water-soluble shell-core toughened acrylic ester polymer, acrylic emulsion and styrene acrylic emulsion.
4. The electron-donating composite bipolar plate according to claim 1, characterized in that: The thermosetting resin is one of epoxy resin and phenolic resin.
5. The electron-donating composite bipolar plate according to claim 1, characterized in that: The graphite intercalation compound is a nickel-graphite intercalation compound, which is a nickel-graphite intercalation compound Ni-GICs prepared by a reduction reaction of nickel chloride and hydrazine hydrate in expanded graphite and ethylene glycol slurry.
6. The method for preparing an electron-donating composite material bipolar plate according to claim 5, characterized in that: The process steps are as follows: Step S1, preparation of nickel-graphite intercalation compound Ni-GICs: in a water bath at 80°C-90°C, add 155mg-775mg of hydrazine hydrate to a beaker containing 50mL-250mL of ethylene glycol and dissolve it, and set it aside after the hydrazine hydrate is dissolved; add 60mg-300mg of nickel chloride hexahydrate to 50mL-250mL of ethylene glycol solution, then add 10g-50g of expanded graphite, stir and microwave oscillate for 15min to obtain a nickel chloride-graphite suspension; slowly add the nickel chloride-graphite suspension dropwise to the hydrazine hydrate solution for 20-30min, and then react for 20-30min to obtain a graphite intercalation compound formed by colloidal nickel intercalation graphite, filter it, wash it with ethylene glycol or ethanol, and dry it at 75°C-85°C for 4h to obtain a nickel-graphite intercalation compound Ni-GICs; Step S2: Preparation of composite conductive preform: Take 1% to 5% by mass of conductive material surface modifier, add 49% to 63% by mass of graphite and 17% to 25% by mass of carbon powder, stir in a mixer for 30 to 40 minutes, and dry at 75° C. to prepare a composite conductive preform; Step S3, preparation of composite bipolar plates: put 1% to 5% by mass of nickel-graphite intercalation compound, composite conductive preform, and pre-modulated thermosetting resin with a mass percentage of 14% to 20% into a mixer, mix for 30 minutes, and then form in a kneader to obtain a bipolar plate premix; finally, take 130±2g of the bipolar plate premix and put it into a mold, hot-press under vacuum conditions to make a composite bipolar plate for an electronic all-vanadium liquid flow battery.
7. The method for preparing an electron-donating composite material bipolar plate according to claim 6, characterized in that: The conditions for hot pressing molding in step S3 are: vacuum degree of -0.08 MPa, temperature of 75°C to 85°C, and pressure of 20-30 MPa.
8. The method for preparing an electron-donating composite material bipolar plate according to claim 6, characterized in that: The technical indicators of the bipolar plate prepared by this method are: tensile strength>35Mpa, bending strength>54MPa, bulk conductivity>150S / cm, vertical resistance<10.0mΩ.cm 2 , in the all-vanadium redox flow battery with a current density of 200 mA / cm 2 When operated under the conditions of , its energy efficiency EE>81%, Coulomb efficiency CE>98.5%, voltage efficiency VE is 82.2% and the capacity retention rate is>65% after 100 cycles.
9. Use of the electron-donating composite bipolar plate according to any one of claims 1 to 5 in an all-vanadium liquid flow battery.
Citation Information
Patent Citations
Method for preparing fuel cell bipolar plate by using transition metal-graphite interlayer complex as filler
CN102074714A
Preparation method of graphene / metal nanoparticle composite material with sandwich structure
CN103157809A
Preparation method for graphene powder loading nickel particles
CN108655412A
Preparation method of graphite bipolar plate of fuel cell
CN110590230A
Conductive polymer bipolar plate for flow battery and preparation method of conductive polymer bipolar plate
CN114256476A
Cited By
Composite graphite-based material for bipolar plate and preparation method of composite graphite-based material
CN120453406A
Preparation method of a toughened bipolar plate and application thereof in a vanadium redox flow battery
CN122868569B